Pattern forming method

By removing edge beads of photoresist in the semiconductor industry, the indentation and pattern defect problems caused by photoresist accumulation at the edges of silicon substrates are solved, and efficient edge cleaning and pattern formation are achieved. Improves the performance of semiconductor devices.

CN119002174APending Publication Date: 2024-11-22SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410572064.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-05-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the semiconductor industry, the accumulation of photoresist on the edges and rear surface of silicon substrates results in indentation and pattern defects, and the prior art is difficult to effectively remove without leaving residues.

Method used

Using a diluent composition, a photoresist layer is formed on a silicon substrate by spin coating and drying treatment, and edge beads are removed using specific surface tension and viscosity characteristics, followed by exposure and development to form a pattern.

Benefits of technology

Effectively remove edge beads of photoresist, reduce metal contamination, avoid photoresist residues, meet the needs of small features and patterning, and improve the integration and reliability of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119002174A_ABST
    Figure CN119002174A_ABST
Patent Text Reader

Abstract

A method of forming a pattern is provided, the method including: applying a metal-containing resist composition on a substrate to form a resist layer; coating a composition for removing edge beads along the edge of the substrate; performing drying and heat treatment; and performing exposure and development to form a resist pattern, in which a maximum bump height of the resist layer is less than or equal to about 300 nm in a region of about 1 mm to about 30 mm from an edge of the substrate toward a center of the substrate after coating the composition for removing the edge beads.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0063963 filed in the Korean Intellectual Property Office on May 17, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] Embodiments of the present disclosure relate to a method of forming a pattern, the method comprising applying a composition for removing edge beads to reduce metal contamination occurring along an edge of a wafer. Background Art

[0004] In recent years, the semiconductor industry has witnessed a substantial continuous reduction in critical dimensions, and such reductions in dimensions will benefit from new types or classes of high-performance photoresist materials and patterning methods that meet the demands for processing and patterning with increasingly smaller features.

[0005] With the recent rapid development of the semiconductor industry, semiconductor devices will benefit from relatively fast operating speeds and large storage capacities, and in accordance with such requirements, process technologies for improving the integration, reliability, and response speed of semiconductor devices are being developed. For example, it would be advantageous to accurately control / implant impurities in working regions of a silicon substrate and interconnect these regions to form devices and ultra-high density integrated circuits, which can be achieved through a photolithographic process. For example, it would be advantageous to integrate a photolithographic process including coating a photoresist on a substrate, selectively exposing the photoresist to ultraviolet (UV) (including extreme ultraviolet (EUV)), an electron beam (E-Beam), X-rays, etc., and then developing the photoresist.

[0006] For example, in the process of forming a photoresist layer, the photoresist is mainly coated on the substrate while the silicon substrate is rotated, wherein the photoresist is coated on the edge and rear surface of the substrate, which may cause indentations or pattern defects in subsequent semiconductor processes (such as etching processes and ion implantation processes). Therefore, a process of stripping and removing the photoresist coated on the edge and rear surface of the silicon substrate using a thinner composition, such as an edge bead removal (EBR) process, can be implemented. The EBR process utilizes a composition that exhibits excellent solubility to the photoresist and effectively removes the beads and photoresist remaining in the substrate without generating photoresist residues. Summary of the invention

[0007] In recent years, the semiconductor industry has witnessed a substantial continuous reduction in critical dimensions, and such reductions in dimensions will benefit from new types or classes of high-performance photoresist materials and patterning methods that meet the demands for processing and patterning with increasingly smaller features.

[0008] With the recent rapid development of the semiconductor industry, semiconductor devices will benefit from relatively fast operating speeds and large storage capacities, and in accordance with such requirements, process technologies for improving the integration, reliability, and response speed of semiconductor devices are being developed. For example, it would be advantageous to accurately control / implant impurities in working regions of a silicon substrate and interconnect these regions to form devices and ultra-high density integrated circuits, which can be achieved through a photolithographic process. For example, it would be advantageous to integrate a photolithographic process including coating a photoresist on a substrate, selectively exposing the photoresist to ultraviolet (UV) (including extreme ultraviolet (EUV)), an electron beam (E-Beam), X-rays, etc., and then developing the photoresist.

[0009] For example, in the process of forming a photoresist layer, the photoresist is mainly coated on the substrate while the silicon substrate is rotated, wherein the photoresist is coated on the edge and rear surface of the substrate, which may cause indentations or pattern defects in subsequent semiconductor processes (such as etching processes and ion implantation processes). Therefore, a process of stripping and removing the photoresist coated on the edge and rear surface of the silicon substrate using a thinner composition, such as an edge bead removal (EBR) process, can be implemented. The EBR process utilizes a composition that exhibits excellent solubility to the photoresist and effectively removes the beads and photoresist remaining in the substrate without generating photoresist residues. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] The drawings, together with the specification, illustrate various embodiments of the presently disclosed subject matter, and, together with the description, serve to explain principles of the embodiments of the presently disclosed subject matter.

[0011] Figure 1 is a schematic diagram showing an embodiment of a photoresist coating apparatus.

[0012] Figure 2 It is a schematic diagram of the bulge.

[0013] Figure 3 is an electron microscope image of a photoresist film according to an example measured using a profilometer equipment after spraying a composition for removing edge beads on the photoresist film on a substrate.

[0014] Figure 4 is an electron microscopic image of a photoresist film according to a comparative example obtained using a profilometer equipment after spraying a composition for removing edge beads on the photoresist film on a substrate.

[0015] [Explanation of Symbols]

[0016] 1: Substrate support part

[0017] 2: Nozzle

[0018] 10: Metal-containing resist composition

[0019] 12: Edge Beads

[0020] a: Photoresist film

[0021] b: bulge

[0022] c: substrate

[0023] W: substrate DETAILED DESCRIPTION

[0024] Hereinafter, embodiments of the present disclosure are described in more detail with reference to the accompanying drawings. In the following description of the present disclosure, well-known functions or constructions may not be described in order to more clearly describe the subject matter of the present disclosure.

[0025] In order to clearly illustrate the subject matter of the present disclosure, some descriptions and relationships may be omitted, and in the entire disclosure, the same or similar configuration elements are represented by the same reference numerals. In addition, since the size and thickness of each configuration shown in the drawings can be arbitrarily shown for better understanding and ease of description, the present disclosure is not necessarily limited thereto.

[0026] In the drawings, the thickness of each layer, film, panel, region, etc. may be exaggerated for clarity. In the drawings, the thickness of a portion of each layer or region may be exaggerated for clarity. It should be understood that if an element (such as a layer, film, region, or substrate) is referred to as being "on" another element, the element may be directly on the other element or intervening elements may also be present.

[0027] In the present disclosure, "substituted" means that a hydrogen atom is replaced by a deuterium, a halogen group, a hydroxyl group, an amino group, a substituted or unsubstituted C1 to C30 amino group, a nitro group, a substituted or unsubstituted C1 to C40 silyl group, a C1 to C30 alkyl group, a C1 to C10 haloalkyl group, a C1 to C10 alkylsilyl group, a C3 to C30 cycloalkyl group, a C6 to C30 aryl group, a C1 to C20 alkoxy group, or a cyano group. "Unsubstituted" means that a hydrogen atom remains a hydrogen atom without being replaced by another substituent.

[0028] In the present disclosure, unless otherwise defined, the term "alkyl" means a straight or branched aliphatic hydrocarbon group. The alkyl group may be a "saturated alkyl group" not including any double bond or triple bond.

[0029] The alkyl group may be a C1 to C20 alkyl group. In some embodiments, the alkyl group may be a C1 to C10 alkyl group or a C1 to C6 alkyl group. For example, a C1 to C5 alkyl group means that the alkyl chain contains 1 to 5 carbon atoms and may be selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl.

[0030] Examples of the alkyl group include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl and the like.

[0031] In the present disclosure, if a definition is not otherwise provided, the term "cycloalkyl group" refers to a monovalent cyclic aliphatic hydrocarbon group.

[0032] The cycloalkyl group may be cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, or the like.

[0033] In the present disclosure, if a definition is not otherwise provided, the term "alkenyl" is a straight or branched aliphatic hydrocarbon group, and refers to an aliphatic unsaturated alkenyl group containing one or more double bonds.

[0034] In the present disclosure, if a definition is not otherwise provided, the term "alkynyl" is a straight or branched aliphatic hydrocarbon group, and refers to an unsaturated alkynyl group including one or more triple bonds.

[0035] In the present disclosure, "aryl" means a substituent in which all elements of a cyclic substituent have p-orbitals, and these p-orbitals form conjugation and may include monocyclic, polycyclic or fused ring (e.g., rings that share adjacent pairs of carbon atoms) functional groups.

[0036] In some embodiments, the substituted or unsubstituted C6 to C30 aryl group may be a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted tetraphenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted p-terphenyl group, a substituted or unsubstituted m-terphenyl group, a substituted or unsubstituted o-terphenyl group, a substituted or unsubstituted chrysene group, a substituted or unsubstituted triphenylene group, a substituted or unsubstituted triphenylene group, a substituted or unsubstituted perylene group, a substituted or unsubstituted fluorenyl group, a substituted or unsubstituted indenyl group, or a combination thereof, but is not limited thereto.

[0037] Figure 1 is a schematic diagram showing an embodiment of a photoresist coating apparatus.

[0038] Reference Figure 1 , a substrate supporting portion 1 on which a substrate W is placed is provided, and the substrate supporting portion 1 includes a spin chuck or a spin coater.

[0039] The substrate support part 1 rotates in a first direction at a set or predetermined rotation speed to provide a centrifugal force to the substrate W. A nozzle 2 may be positioned on the substrate support part 1 in the atmospheric region, but the nozzle 2 is positioned away from the upper portion of the substrate W (for example, the nozzle 2 may be spaced apart from the substrate W), so that the nozzle may move toward the upper portion of the substrate W and spray the metal-containing resist composition 10 during spraying. Therefore, the metal-containing resist composition 10 is coated on the surface of the substrate W by the centrifugal force. Herein, the metal-containing resist composition 10 supplied to the center of the substrate W is coated while being diffused to the edge of the substrate W by the centrifugal force, wherein a portion of the metal-containing resist composition 10 moves to the side surface of the substrate W and the lower surface of the edge of the substrate.

[0040] In some embodiments, in the coating process, the metal-containing resist composition 10 is mainly coated by a spin coating method, wherein a set or predetermined amount of the metal-containing resist composition 10 having a certain viscosity (e.g., a set viscosity) is supplied to the central portion of the substrate W and gradually diffuses toward the edge of the substrate W by centrifugal force.

[0041] Therefore, the photoresist film is uniformly formed by the rotation speed of the substrate supporting portion.

[0042] In some embodiments, such rotation evaporates the solvent from the solution and thus gradually increases the viscosity, resulting in a relatively large amount of photoresist accumulating on the edge of the substrate due to the effect of surface tension, and in severe cases even accumulating on the lower surface of the edge of the substrate, which is called an edge bead 12. As described herein, reference to an "edge bead" may refer to a single edge bead around the perimeter of the substrate.

[0043] Hereinafter, methods of forming patterns according to some exemplary embodiments are described.

[0044] In this manual, if Figure 2 As shown, a hump b means an increase in film thickness (Δthickness) at the boundary with the portion where the edge bead is removed.

[0045] A method for forming a pattern according to another embodiment includes: coating a metal-containing photoresist composition on a substrate to form a photoresist layer; coating a composition for removing edge beads along an edge of the substrate (the "edge" mentioned herein may refer to a single edge around the periphery of the substrate); performing drying and heat treatment; and performing exposure and development to form a photoresist pattern.

[0046] Wherein after applying the composition for removing edge beads, a maximum protrusion height of the resist layer in a region of about 1 mm to about 30 mm from an edge of the substrate toward a center of the substrate may be less than or equal to about 300 nm.

[0047] The maximum ridge height may be from about 10 nm to about 300 nm.

[0048] In some embodiments, the step of applying a metal-containing photoresist composition to form a photoresist layer comprises: applying the metal-containing photoresist composition on a substrate by spin coating, slit coating, inkjet printing, etc., and drying the metal-containing photoresist composition to form a photoresist film. The metal compound contained in the metal-containing photoresist may be, for example, a tin compound, and the tin compound may be, for example, at least one selected from a tin compound containing an organic oxygen group and a tin compound containing an organic carbonyl oxygen group.

[0049] For example, the metal compound included in the metal-containing photoresist may be represented by Chemical Formula 1.

[0050] [Chemical formula 1]

[0051]

[0052] In Chemical Formula 1,

[0053] R 1 is selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C7 or C30 arylalkyl, and L a -OR a (Where L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl),

[0054] R 2 to R 4 each independently represents a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C7 or C30 arylalkyl group, -OR b or -OC(=O)R c ,

[0055] R 2 to R 4 At least one of -OR b or -OC(=O)R c ,

[0056] R b is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and

[0057] R c is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

[0058] In addition, the metal-containing photoresist composition according to one embodiment may include at least one selected from the group consisting of a surfactant, a dispersant, a hygroscopic agent, and a coupling agent.

[0059] Surfactant can be used to improve the coating uniformity and wettability of photoresist composition. In some exemplary embodiments, surfactant can be composed of sulfate ester salt, sulfonate, phosphate, soap, amine salt, quaternary ammonium salt, polyethylene glycol, alkylphenol ethylene oxide adduct, polyol, nitrogen-containing vinyl polymer or its combination, but is not limited to this. For example, surfactant can include alkylbenzene sulfonate, alkylpyridinium salt, polyethylene glycol and / or quaternary ammonium salt. If photoresist composition includes surfactant, then based on the gross weight of photoresist composition, surfactant can be included in an amount of about 0.001 weight % to about 3 weight %.

[0060] The dispersant can be used to uniformly (e.g., substantially uniformly) disperse the components constituting the photoresist composition in the photoresist composition. In some exemplary embodiments, the dispersant can be composed of epoxy resin, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, glucose, sodium lauryl sulfate, sodium citrate, oleic acid, linoleic acid, or a combination thereof, but is not limited thereto. If the photoresist composition includes the dispersant, the dispersant can be included in an amount of about 0.001 wt % to about 5 wt % based on the total weight of the photoresist composition.

[0061] The hygroscopic agent can be used to prevent or reduce the adverse effects caused by moisture in the photoresist composition. For example, the hygroscopic agent can be used to prevent or reduce the oxidation of the metal contained in the photoresist composition due to moisture. In some exemplary embodiments, the hygroscopic agent can be composed of polyoxyethylenenonylphenolether, polyethylene glycol, polypropylene glycol, polyacrylamide or a combination thereof, but is not limited thereto. If the photoresist composition includes the hygroscopic agent, then the hygroscopic agent can be included in an amount of about 0.001 weight % to about 10 weight % based on the total weight of the photoresist composition.

[0062] If the photoresist composition is coated on the lower film, a coupling agent can be used to improve the adhesion to the lower film. In some exemplary embodiments, the coupling agent can include a silane coupling agent. The silane coupling agent can be composed of vinyl trimethoxy silane, vinyl triethoxy silane, vinyl trichlorosilane, vinyl tris (β-methoxyethoxy) silane, 3-methacryloxy propyl trimethoxy silane, 3-acryloxy propyl trimethoxy silane, p-phenylyl trimethoxy silane, 3-methacryloxy propyl methyl dimethoxy silane, 3-methacryloxy propyl methyl diethoxy silane and / or trimethoxy [3- (phenylamino) propyl] silane, but is not limited thereto. If the photoresist composition includes a coupling agent, the coupling agent can be included in an amount of about 0.001 wt % to about 5 wt % based on the total weight of the photoresist composition.

[0063] Subsequently, application of a composition for removing edge beads may be carried out.

[0064] After the edge beads are removed by applying the composition for removing edge beads, a bulge in which an increase in film thickness (Δthickness) occurs may be generated at the boundary with the removed portion.

[0065] Since the lifting may cause cracks and / or peeling of the film during baking, contaminate the mask, and cause non-uniformity in subsequent processes, there is a need for a composition for removing edge beads that can obtain a photoresist film with a better edge cut portion after coating the composition for removing edge beads.

[0066] In the coating of the composition for removing edge beads according to the embodiments of the present disclosure, the difference between the main properties such as the surface energy of the photoresist and the viscosity of the composition for removing edge beads, as well as the process conditions when removing the edge beads can be adjusted to find a protrusion height that is less likely to cause problems in subsequent processes, thereby implementing a suitable or optimal method for achieving the corresponding protrusion height.

[0067] The difference between the surface energy of the photoresist layer and the surface tension of the composition for removing the edge beads may be about 2 mN / m to about 15 mN / m.

[0068] If the difference between the surface energy of the photoresist layer and the surface tension of the composition for removing edge beads exceeds the above range (for example, becomes larger), the composition for removing edge beads may hardly dissolve the photoresist due to reduced wettability and may be expected to exhibit deteriorated cleaning ability, and since there may be mutual pushing pressure due to low affinity at the interface, the ridges may further increase, and the dissolved photoresist may not be removed but remain in the form of aggregates near the interface.

[0069] In some embodiments, if the difference between the surface energy of the photoresist layer and the surface tension of the composition for removing edge beads does not reach the aforementioned range (e.g., becomes smaller), the wettability may be higher, but the composition for removing edge beads may penetrate into the photoresist too quickly, resulting in damage to the photoresist and swelling.

[0070] In some embodiments, the method of forming a pattern according to the present disclosure can ensure that there is a suitable or appropriate difference between the surface energy of the photoresist layer and the surface tension of the composition used to remove edge beads, thereby reducing metal-based contamination and minimizing or reducing the impact on the photoresist film, and thereby meeting the requirements or desired features for processing and patterning smaller features.

[0071] The surface tension of the composition for removing edge beads can be about 25.0 mN / m to about 40.0 mN / m. For example, the surface tension can be about 27.0 mN / m to about 40.0 mN / m, or for example, about 27.0 mN / m to about 36.0 mN / m.

[0072] The composition for removing edge beads may have a viscosity of about 1 cPs to about 10 cPs.

[0073] The composition for removing edge beads according to an embodiment of the present disclosure may include an additive and a solvent, and the additive and the solvent may be selected within a range satisfying the above conditions as materials suitable for the composition for removing edge beads in the art.

[0074] For example, the additive may be at least one selected from an acid compound (eg, carboxylic acid, phosphoric acid, phosphorous acid, and sulfuric acid), an alcohol compound, and a ketone compound.

[0075] For example, the solvent may be propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), propylene glycol butyl ether (PGBE), ethylene glycol methyl ether, diethyl glycol ethyl methyl ether, dipropyl glycol dimethyl ether, ethanol, 2-butoxyethanol, n-propanol, isopropanol, n-butanol, isobutanol, hexanol, ethylene glycol, propylene glycol, heptanone, propylene carbonate, butylene carbonate, diethyl ether, dibutyl ether, ethyl acetate, n-butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, butyl acetate, propylene carbonate, propylene carbonate, propylene glycol acetate, propylene glycol acetate, propylene glycol acetate, propylene glycol acetate, propylene glycol acetate, propylene glycol acetate, propylene glycol acetate, propylene glycol acetate, propylene glycol methyl ether (PGME), propylene glycol methyl ether (PGMEA), propylene glycol methyl ether, propylene glycol methyl ether, acetate, nBA), methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, diisoamyl ether, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, dimethyl sulfoxide, dimethylformamide, acetonitrile, diacetone alcohol, 3,3-dimethyl-2-butanone, N-methyl-2-pyrrolidone, dimethylacetamide, cyclohexanone methyl-2-hydroxy-2-methylpropane acid (HBM), gamma-butyrolactone (GBL), 1-butanol (n-butanol), ethyl lactate (ethyllactate, EL), diene butyl ether (dienebutylether, DBE), diisopropyl ether (diisopropylether, DIAE), acetylacetone, butyl lactate (n-butyl lactate), 4-methyl-2-pentenol (or methyl isobutyl carbinol (methyl isobutyl carbinol, MIBC)), 1-methoxy-2-propanol, 1-ethoxy-2-propanol, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-hydroxyethyl propionate, 2-hydroxy-2-methylethyl propionate, ethoxyethyl acetate, hydroxyethyl acetate, 2-hydroxy-3-methylbutyric acid methyl ester, 3-methoxymethyl propionate, 3-methoxyethyl propionate, 3-ethoxyethyl propionate, 3-ethoxymethyl propionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, methyl 2-hydroxyisobutyrate, methoxybenzene, n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxy propionate, ethoxyethoxy propionate or a mixture thereof, but are not limited thereto.

[0076] In some example embodiments, the composition for removing edge beads from a metal-containing photoresist may include about 0.01 wt % to about 50 wt % of the aforementioned additives and about 50 wt % to about 99.99 wt % of a solvent.

[0077] The composition for removing edge beads may further include other additives as described below. In an embodiment including other additives, a solvent may be included in an amount other than the included components.

[0078] The composition may further include at least one other additive selected from a surfactant, a dispersant, a hygroscopic agent, and a coupling agent.

[0079] The composition for removing edge beads may be applied while the substrate is rotated at a speed of, for example, about 1,000 rpm to about 4,000 rpm.

[0080] In some embodiments of the present disclosure, the application of the composition for removing edge beads may be repeatedly performed several times to reduce metal-based contamination on the edge and rear surface of the substrate and also reduce the photoresist to a suitable or desired level.

[0081] The patterning method including edge bead removal according to the present disclosure may be particularly effective for removing metal-containing photoresists and, for example, removing undesirable metal residues (eg, tin-based metal residues).

[0082] Subsequently, a first heat treatment process of heating the substrate on which the photoresist layer is formed is performed. The first heat treatment process may be performed at a temperature of about 80° C. to about 160° C., and in such a process, the solvent is evaporated and the photoresist layer may be more firmly bonded to the substrate to form a photoresist film.

[0083] Then, an exposure process of selectively exposing the photoresist film may be performed.

[0084] Examples of light used in the exposure process may include not only light with a short wavelength such as i-line (wavelength: 365nm), KrF excimer laser (wavelength: 248nm), ArF excimer laser (wavelength: 193nm), but also light with a high energy wavelength such as EUV (extreme ultraviolet; wavelength: 13.5nm) or electron beam (electron beam, E-Beam).

[0085] In some embodiments, the light used for exposure according to some exemplary embodiments may be light with a short wavelength in the range of about 5 nm to about 150 nm, or may be light with a high energy wavelength such as EUV (extreme ultraviolet, wavelength: about 13.5 nm), E-Beam (electron beam), etc.

[0086] When forming the photoresist pattern, a negative type pattern may be formed.

[0087] The exposed region of the photoresist film has a solubility different from that of the unexposed region of the photoresist film because a polymer is formed by a cross-linking reaction (eg, condensation between organometallic compounds).

[0088] Then, the substrate may be subjected to a second heat treatment process. The second heat treatment process may be performed at a temperature of about 90° C. to about 200° C. By performing the second heat treatment process, the exposed region of the photoresist film becomes difficult to dissolve in a developer.

[0089] Then, development using a developer composition may be carried out.

[0090] In some embodiments, a developer composition is used to dissolve and remove the photoresist film corresponding to the unexposed area to complete a photoresist pattern corresponding to the negative image.

[0091] The developer composition used in the method of forming a pattern may be, for example, an organic solvent, such as: ketones, such as methyl ethyl ketone, acetone, cyclohexanone, 2-heptanone, etc.; alcohols, such as 4-methyl-2-propanol, 1-butanol, isopropanol, 1-propanol, methanol, propylene glycol methyl ether (PGME), methyl isobutylcarbinol (MIBC), etc.; esters, such as propylene glycol methyl ether acetate, ethyl acetate, ethyl lactate, n-butyl acetate, methyl-2-hydroxyisobutyrate, butyrolactone, etc.; aromatic compounds, such as benzene, xylene, toluene, etc.; or combinations thereof.

[0092] As described above, the photoresist pattern formed by exposure to the following light may have a width in the range of about 5 nm to about 100 nm: light with high energy, such as EUV (extreme ultraviolet light; wavelength: about 13.5 nm), E-Beam (electron beam), etc.; and light with a certain wavelength, such as i-line (wavelength: about 365 nm), KrF excimer laser (wavelength: about 248 nm), ArF excimer laser (wavelength: about 193 nm), etc. For example, the photoresist pattern may have a width in the range of about 5 nm to about 90 nm, about 5 nm to about 80 nm, about 5 nm to about 70 nm, about 5 nm to about 60 nm, about 5 nm to about 50 nm, about 5 nm to about 40 nm, about 5 nm to about 30 nm, or about 5 nm to about 20 nm.

[0093] In some embodiments, the photoresist pattern may have a half-pitch pitch of less than or equal to about 50 nm, e.g., less than or equal to about 40 nm, e.g., less than or equal to about 30 nm, e.g., less than or equal to about 20 nm, e.g., less than or equal to about 15 nm, and a line width roughness of less than or equal to about 10 nm, less than or equal to about 5 nm, less than or equal to about 3 nm, or less than or equal to about 2 nm.

[0094] Hereinafter, the embodiments of the present disclosure will be described in more detail by examples related to the above-mentioned method of forming a pattern. However, the technical features of the present disclosure are not limited by the following examples.

[0095] Preparation of photoresist composition containing organic metal

[0096] Preparation Example A

[0097] The organometallic compound having the structure of Chemical Formula C was dissolved in 4-methyl-2-pentanol at a concentration of 1.0 wt %, and then filtered through a 0.1 μm polytetrafluoroethylene (PTFE) syringe filter to obtain a photoresist composition.

[0098] [Chemical formula C]

[0099]

[0100] Preparation Example B

[0101] A composition was prepared in substantially the same manner as in Preparation Example A, except that the organometallic compound having the structure of Chemical Formula D was used.

[0102] [Chemical formula D]

[0103]

[0104] Preparation of a composition for removing edge beads

[0105] Preparation Example 1 to Preparation Example 22

[0106] The additives according to the composition shown in Table 1 were mixed together with the solvent and completely dissolved by shaking at room temperature (25° C.) Thereafter, a composition for removing final edge beads was obtained by passing through a filter made of PTFE having a pore size of 0.1 μm.

[0107] [Table 1]

[0108]

[0109] Preparation of developer

[0110] Preparation Example C

[0111] The developer was prepared by dissolving 1.0 wt % acetic acid in PGMEA.

[0112] Propylene glycol methyl ether acetate

[0113] Examples

[0114] 2.0 mL of the photoresist composition containing an organic metal compound according to Preparation Example A and Preparation Example B was placed on an 8-inch silicon wafer, and then allowed to stand for 20 seconds and spin-coated at a speed of 1500 rpm for 30 seconds (PR(A) or PR(B) formation step). Subsequently, as shown in Table 2, 10 mL of each of the compositions for removing edge beads according to the Preparation Examples was placed 1 mm above the periphery of the wafer, and then rotated at a processing speed shown in Table 2 for 30 seconds, and dried at 160°C for 60 seconds.

[0115] Assessment 1: Measurement of the surface energy of the photoresist layer

[0116] 2.0 mL of each of the photoresist compositions containing an organometallic compound according to the preparation example was placed in an 8-inch silicon wafer, allowed to stand for 20 seconds, spin-coated at 1500 rpm for 30 seconds, and heat-treated at 100° C. for 60 seconds, thereby forming a photoresist layer.

[0117] After cleaning the surface of the photoresist layer, DSA100 (Cruss Co., Ltd. GmbH) was installed on the surface to measure the contact angle of deionized water (DIW), the contact angle of diiodomethane and the surface energy calculated by the OWRK method. The same measurement was repeated 5 times to obtain the average value of the other 3 measurements except the upper and lower limits, and the results are shown in Table 2.

[0118] Evaluation 2: Measurement of surface tension of compositions for removing edge beads

[0119] The surface tension of each of the compositions for removing edge beads according to Preparation Examples 1 to 22 at 25° C. was measured 5 times using a K11-MK1 (Cruss Co., Ltd.) surface tensiometer, and then the average value of the other 3 measurements excluding the upper and lower limits was calculated, and the average value is then provided in Table 2.

[0120] Evaluation 3: Measurement of viscosity of the composition for removing edge beads

[0121] The absolute viscosity of each of the compositions for removing edge beads according to Preparation Examples 1 to 22 was measured 5 times using LVDV-III-U CP (Brookfield Corp.) at 25°C and torque % 45, and then the average value of the other 3 measurements excluding the upper and lower limits was calculated, and the average value is then provided in Table 2.

[0122] Assessment 4: Assessment of bulge

[0123] Figure 2 It is a schematic diagram of the bulge.

[0124] Reference Figure 2 , bump b means the △ thickness (hump) produced by the convex end of the photoresist film a containing an organic metal compound after spraying the composition for removing edge beads from the metal-containing photoresist on the substrate c, and the △ thickness (hump) values ​​measured using the profiler P17OF facility of Tencor are shown in Table 2.

[0125] The measured elevation height was evaluated according to the following criteria and the results are also explained.

[0126] A: Height of protrusion ≤ 100nm

[0127] B: 100nm<ridge height≤300nm

[0128] C: 300nm<ridge height≤1000nm

[0129] D: 1000nm<ridge height

[0130] Evaluation 5: Evaluation of the defect rate of edge patterns

[0131] Each wafer of the example in which edge bead removal had been completed was exposed to a 1 cm×1 cm square pattern using an ArF scanner (XT1250D, ASML) at a dose of 40 mJ, cured at 170° C. for 60 seconds, spin-developed at 1500 rpm for 30 seconds using a developer composition (Preparation Example C), and then cured at 240° C. for 60 seconds.

[0132] If the curing is completed, the pattern wafer on which the line / space CD pattern is formed is transported to a critical dimension-scanning electron microscope (CD-SEM) measuring equipment to measure the critical dimension (CD) size. The CD size is determined by performing measurement at 12 points on the CD-SEM image and calculating the average value thereof, and the defect rate is calculated according to Equation 1 by setting 80 nm as the target CD and counting the points where there are points that exceed the error range (±10%) from the target CD or where bridges or scums appear, wherein a defect rate of 1.5% or less is evaluated as good, but a defect rate of more than 1.5% is evaluated as defective, and then the results are shown in Table 2.

[0133] [Equation 1]

[0134] Defect rate of edge pattern = (number of defective exposure areas / total number of exposure areas)*100

[0135] [Table 2]

[0136]

[0137] Referring to Table 2, the pattern wafers of Examples 1 to 18 exhibited low ridges, and thus low pattern defect rates, compared to Comparative Examples 1 to 11.

[0138] In the above, certain embodiments of the present disclosure have been described and illustrated. However, it should be obvious to those skilled in the art that the present disclosure is not limited to the described embodiments, but various modifications and changes can be made without departing from the spirit and scope of the present disclosure. Therefore, the modified or changed embodiments themselves cannot be understood separately from the technical ideas and aspects of the embodiments of the present disclosure, and the modified embodiments are within the scope of the claims of the present disclosure and their equivalent forms.

Claims

1. A method for forming a pattern, comprising: coating a metal-containing resist composition on a substrate to form a resist layer; applying a composition for removing edge beads along the edge of the substrate; Implement drying and heat treatment; as well as Exposure and development are performed to form a resist pattern, wherein after applying the composition for removing edge beads, a maximum protrusion height of the resist layer in a region of 1 mm to 30 mm from the edge of the substrate toward the center of the substrate is less than or equal to 300 nm.

2. The method according to claim 1, wherein: The maximum protrusion height is 10 nm to 300 nm.

3. The method according to claim 1, wherein: The difference between the surface energy of the resist layer and the surface tension of the composition for removing edge beads is 2 mN / m to 15 mN / m.

4. The method according to claim 1, wherein: The surface tension of the composition for removing edge beads is from 25.0 mN / m to 40.0 mN / m.

5. The method according to claim 1, wherein: The surface tension of the composition for removing edge beads is 27.0 mN / m to 36.0 mN / m.

6. The method according to claim 1, wherein: The composition for removing edge beads has a viscosity of 1 cPs to 10 cPs.

7. The method according to claim 1, wherein: The coating of the composition for removing edge beads is performed while the substrate is rotated at a speed of 1,000 rpm to 4,000 rpm.

8. The method according to claim 1, wherein: The metal compound contained in the metal-containing resist composition includes at least one selected from the group consisting of an organic oxygen group-containing tin compound and an organic carbonyl oxygen group-containing tin compound.

9. The method according to claim 1, wherein: The metal compound contained in the metal-containing resist composition is represented by Chemical Formula 1: [Chemical formula 1] Wherein, in Chemical Formula 1, R 1 is selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C7 or C30 arylalkyl, and L a -OR a , where L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl group, R 2 to R 4 each independently represents a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C7 or C30 arylalkyl group, -OR b or -OC(=O)R c , R 2 to R 4 At least one of -OR b or -OC(=O)R c , R b is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and R c is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.