Back contact solar cell and solar cell module

By setting up an isolation layer formed by light-curing ink on the front of the back contact solar cell, the problem of cost and efficiency of the isolation paper is solved, reducing cell scratches, improving storage and transportation efficiency, and extending the service life of the cell.

CN119008713APending Publication Date: 2024-11-22ZHEJIANG AIKO SOLAR ENERGY TECH CO LTD +4
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410175628.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-01-19
Filing Date
2024-02-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing back contact solar cells during storage and transportation increase costs and affect efficiency due to the presence of isolation paper, and are prone to scratches on the battery.

Method used

The isolation layer is arranged on the top layer of the front surface of the back contact solar cell, formed by curing light curing ink, using a planar structure or evenly distributed isolation lines or isolation points. The isolation layer is perpendicular to the thin grid line on the back, with a thickness of 3 to 100 microns, transparent The light rate is ≥80% under light above 300 nm and consists of polymers such as polyurethane or isobornyl methacrylate.

Benefits of technology

Replacement of isolation paper reduces the probability of scratching on the cell, reduces production costs, improves storage and transportation efficiency, and extends the service life of the cell with high light transmittance and stable polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008713A_ABST
    Figure CN119008713A_ABST
Patent Text Reader

Abstract

The invention provides a back contact solar cell and a solar cell module, specifically, the back contact solar cell comprises an isolation layer arranged on the top layer of the front surface of the solar cell, and the isolation layer is formed by curing light-cured ink. Therefore, based on the back contact solar cell provided by the invention, isolation paper between two adjacent cell pieces in the process of storing and transporting the back contact solar cell can be replaced, the front surface of the back contact solar cell is protected, and the probability that the front surface of the back contact solar cell is scratched is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the priority of the Chinese patent application entitled “Back-contact solar cell, solar cell module” and application number CN202420144088.3 filed on January 19, 2024, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The invention belongs to the technical field of solar cells, and in particular relates to a back contact solar cell. Background Art

[0003] Currently, the front side of the back-contact solar cell does not include the grid line, and the grid line is set on the back side of the back-contact solar cell. In the process of storing and transporting the back-contact solar cell, two adjacent cells usually need to be separated by isolation paper. However, due to the existence of isolation paper, on the one hand, the cost is increased; on the other hand, in the process of taking and placing the cell, the action of taking and placing the isolation paper needs to be increased accordingly, which affects the efficiency. Summary of the invention

[0004] The present application provides a back-contact solar cell and a solar cell module, which are used to solve the problems caused by isolation paper in the prior art.

[0005] In a first aspect, the present application provides a back-contact solar cell, wherein the back-contact solar cell comprises an isolation layer disposed on a top layer of a front side of the back-contact solar cell, wherein the isolation layer is formed by curing a photocurable ink.

[0006] Therefore, the back-contact solar cell provided in the present application can replace the isolation paper between two adjacent solar cells during the storage and transportation of the back-contact solar cell, protect the front side of the back-contact solar cell, and reduce the probability of the front side of the back-contact solar cell being scratched.

[0007] As an implementation manner of the first aspect, the isolation layer is a planar structure.

[0008] As an implementation manner of the first aspect, the isolation layer is composed of a plurality of evenly distributed isolation lines.

[0009] As an implementation manner of the first aspect, the plurality of isolation lines are perpendicular to the back side fine grid lines of the back contact solar cell.

[0010] As an implementation manner of the first aspect, the isolation layer is composed of a plurality of evenly distributed isolation points.

[0011] As an implementation manner of the first aspect, some of the multiple isolation points form a plurality of equilateral triangles, and each of the multiple equilateral triangles is composed of three adjacent isolation points.

[0012] As an implementation manner of the first aspect, the side length of the equilateral triangle is 0.5-4 mm.

[0013] As an implementation manner of the first aspect, the back side of the back-contact solar cell includes a welding point, and the isolation layer is not provided at a position corresponding to the welding point on the front side of the back-contact solar cell.

[0014] As an implementation of the first aspect, the thickness of the isolation layer is 3 to 100 micrometers.

[0015] As an implementation of the first aspect, the light transmittance of the isolation layer is ≥80% under light with a wavelength of 300 nm or more.

[0016] As an implementation manner of the first aspect, the isolation layer includes a polymer formed by polymerization of the photocurable ink.

[0017] As an implementation manner of the first aspect, the polymer is polyurethane.

[0018] As an implementation of the first aspect, the polymer is polyisobornyl methacrylate. Alternatively, the polymer may include vinyl polymer and ethyl methacrylate. Alternatively, the polymer may include ethyl methacrylate. Alternatively, the polymer may include isobornyl methacrylate. Alternatively, the polymer may include polyethyl acrylate and polystyrene. Alternatively, the polymer may include polyacrylamide. Alternatively, the polymer may include polyisopropyl methacrylate. Alternatively, the polymer may include polyisobornyl methacrylate and polymethacrylate. Alternatively, the polymer may include methylisoacrylamide and acrylate.

[0019] In the second aspect, the present application also provides a photocurable ink, which includes a monomer, a tertiary amine co-initiator, and a photoinitiator; wherein the mass percentage of the monomer is 50-95%, the mass percentage of the tertiary amine co-initiator is 1-10%; and the mass percentage of the photoinitiator is 1-40%.

[0020] As an implementation of the second aspect, the monomer is one or more of alkyl methacrylate, dimethyl acrylamide, 2-phenoxyethyl acrylate, isobornyl acrylate, 1,6-hexanediol dimethacrylate, tetraethylene glycol-diacrylate oligoethylene glycol, dipropylene glycol diacrylate, and tetrahydrofuran acrylate.

[0021] As an implementation of the second aspect, the tertiary amine co-initiator is one or more of active amine 002 and active amine 008.

[0022] As an implementation of the second aspect, the photoinitiator is one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methylphenylacetone, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and 1-hydroxycyclohexyl phenyl ketone.

[0023] As an implementation of the second aspect, the formula of the photocurable ink is:

[0024] Formula 1: alkyl methacrylate, tetrahydrofuran acrylate, 2-phenoxyethyl acrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, active amine 002; or,

[0025] Formula 2: alkyl methacrylate, dimethyl acrylamide, 1,6-hexanediol dimethacrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, active amine 008; or,

[0026] Formula 3: dimethyl acrylamide, isobornyl acrylate, tetrahydrofuran acrylate, 2-hydroxy-2-methylphenyl acetone, active amine 002; or,

[0027] Formula 4: dimethylacrylamide, isobornyl acrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, active amine 008; or,

[0028] Formula 5: 2-phenoxyethyl acrylate, dipropylene glycol diacrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 1-hydroxycyclohexyl phenyl ketone, active amine 008; or,

[0029] Formula 6: isobornyl acrylate, dipropylene glycol diacrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, active amine 002; or,

[0030] Formula 7: isobornyl acrylate, 1,6-hexanediol dimethacrylate, 2-hydroxy-2-methylphenylacetone, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, active amine 002; or,

[0031] Formula 8: dipropylene glycol diacrylate, tetraethylene glycol-diacrylate oligoethylene glycol, 2-hydroxy-2-methylphenylacetone, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, active amine 008; or,

[0032] Formula 9: dipropylene glycol diacrylate, alkyl methacrylate, 2-hydroxy-2-methylphenylacetone, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, active amine 002; or,

[0033] Formula 10: dipropylene glycol diacrylate, dimethyl acrylamide, 2-hydroxy-2-methylphenyl acetone, 1-hydroxycyclohexyl phenyl ketone, active amine 008; or,

[0034] Formula 11: dipropylene glycol diacrylate, tetrahydrofuran acrylate, 2-hydroxy-2-methylphenylacetone, 1-hydroxycyclohexyl phenyl ketone, active amine 008; or,

[0035] Formula 12: tetraethylene glycol-diacrylate oligoethylene glycol, tetrahydrofuran acrylate, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, active amine 002; or,

[0036] Formulation 13: tetraethylene glycol-diacrylate oligoethylene glycol, tetrahydrofuran acrylate, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, active amine 002; or,

[0037] Formulation 14: dipropylene glycol diacrylate, dimethyl acrylamide, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, and active amine 002.

[0038] As an implementation of the second aspect, the curing energy of the photocurable ink is 120 to 12000 mJ / m 2 The photocurable ink has a viscosity of 1 to 120 cps and a surface tension of 10 to 1000 mN / m at 25°C; the particles in the photocurable ink have a maximum particle size of <10 μm and a median particle size of <0.25 μm.

[0039] It can be understood that by setting the curing energy of the photocurable ink to 120-12000 mJ / m 2 The above-mentioned light curing can reduce the time required for curing and improve production efficiency. In addition, by setting the viscosity and particle size of the light curing ink within the above-mentioned range, the probability of ink clogging the inkjet head can be reduced.

[0040] In a third aspect, a solar cell assembly is provided, comprising the back-contact solar cell according to any one of the first aspects. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The structure of the back contact solar cell provided by the present application;

[0042] Figure 2 It is an isolation line of a back contact solar cell provided by the present application;

[0043] Figure 3 It is the isolation point of the back contact solar cell provided by the present application;

[0044] Figure 4 It is a pattern composed of isolation points of the back contact solar cell provided by the present application;

[0045] Figure 5 It is another pattern composed of isolation points of the back contact solar cell provided by the present application;

[0046] Figure 6 It is another pattern composed of isolation points of the back contact solar cell provided by the present application.

[0047] Figure 7 This is the result obtained after testing the near-infrared spectral transmittance of sample #A in this application.

[0048] Figure 8 This is the result obtained after testing the near-infrared spectral transmittance of sample #B in this application.

[0049] Fig. 9 This is the result obtained after testing the near-infrared spectral transmittance of sample #C in this application. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Examples of embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be construed as limiting the present invention. In addition, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0051] In the description of the present invention, it is necessary to understand that the terms "length", "width", "up", "down", "left", "right", "horizontal", "top", "bottom", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0052] Figure 1A back-contact solar cell provided by the present application is shown, and the back-contact solar cell includes a front side and a back side (100). It can be understood that the back side of the back-contact solar cell includes grid lines, and the front side of the back-contact solar cell does not include grid lines, that is, the front side of the back-contact solar cell has no grid lines.

[0053] In order to replace the isolation paper between adjacent back contact solar cells in the prior art, such as Figure 1 As shown, an isolation layer (200) is provided on the top layer of the front side of the back contact solar cell, and the isolation layer is formed by curing the photocurable ink. The isolation layer can be used to isolate two adjacent back contact solar cells, protect the front side of the back contact solar cell, and reduce the probability of scratching the front side of the back contact solar cell.

[0054] Optionally, as a possible situation, the isolation layer can be a planar structure. In other words, the isolation layer is a whole surface structure printed on the front of the back contact solar cell, so as to protect the front of the back contact solar cell. Exemplarily, the thickness of the isolation layer can be 3 to 100 μm, preferably, the thickness of the isolation layer can be 7 μm.

[0055] Optionally, as another case, in order to reduce the amount of light-curable ink used and further reduce the cost, as Figure 2 As shown, the isolation layer may also be composed of a plurality of isolation lines. Exemplarily, the plurality of isolation lines may be evenly distributed on the front side of the back contact solar cell.

[0056] Optionally, the plurality of isolation lines may be solid lines, or may be dashed lines, or may include both solid lines and dashed lines.

[0057] Optionally, the plurality of isolation lines intersect with the fine grid lines on the back side of the back contact solar cell (eg, are perpendicular to each other). It is understood that making the isolation grid lines perpendicular to the fine grid lines can better achieve isolation between the solar cells.

[0058] Exemplarily, the distance between two adjacent isolation lines may be 0.5-4 mm, preferably, 1.3 mm. Exemplarily, the height of the isolation line may be 3-100 μm, preferably, 7 μm.

[0059] It is understandable that if the isolation layer is set in the form of a whole surface or multiple isolation lines, during the photocuring process of the isolation layer, due to the large amount of photocurable ink accumulation, the required curing energy is also high, and the stress inside the back contact solar cell after curing is large, which increases the probability of cell damage. Therefore, optionally, in order to further reduce the amount of photocurable ink used and reduce the internal stress of the cell, such as Figure 3As shown, the isolation layer may also be composed of a plurality of isolation points. Exemplarily, the plurality of isolation points may be evenly distributed on the front side of the back contact solar cell.

[0060] As a preferred solution, some of the plurality of isolation points may form a plurality of equilateral triangles, each of the plurality of equilateral triangles (such as Figure 4 In other words, the plurality of isolation points include isolation points forming a plurality of regular hexagons, and isolation points located in the regular hexagon (such as Figure 5 The isolation point of the geometric center of the .

[0061] refer to Figure 6 For example, the distance between two adjacent isolation points (300) may be 0.5-4 mm, preferably, 1.3 mm. For example, the height of the isolation points may be 3-100 μm, preferably, 7 μm.

[0062] Optionally, since the back side of the back-contact solar cell includes a welding point, when the battery cells are serially soldered, solder paste is set on the welding point, and then soldering is performed using a solder ribbon. Before soldering, as a method, the position on the front side of the back-contact solar cell corresponding to the welding point can be heated by a heating device, so that heat is conducted from the front side of the back-contact solar cell to the back side of the back-contact solar cell, thereby melting the solder paste. Therefore, in order to improve the efficiency of heat conduction, when an isolation layer is set on the front side of the back-contact solar cell, the position on the front side of the back-contact solar cell corresponding to the welding point can be avoided. In other words, the isolation layer is not set at the position on the front side of the back-contact solar cell corresponding to the welding point.

[0063] refer to Figure 6 No isolation layer is provided at the position corresponding to the welding point on the front side of the back contact solar cell, and around the corresponding position (400), for example, no isolation layer is provided at a distance of 2 to 10 mm from the corresponding position.

[0064] It is understandable that the isolation layer can be formed by inkjet printing or other processes, such as screen printing.

[0065] As an optional embodiment of the photocurable ink, the photocurable ink comprises monomer, tertiary amine co-initiator and photoinitiator. Preferably, the photocurable ink comprises 20-95% monomer, 1-10% tertiary amine co-initiator and 1-40% photoinitiator.

[0066] The monomer is one or more of alkyl methacrylate, dimethyl acrylamide, 2-phenoxyethyl acrylate, isobornyl acrylate, 1,6-hexanediol dimethacrylate, tetraethylene glycol-diacrylate oligoethylene glycol, dipropylene glycol diacrylate, tetrahydrofuran acrylate, but is not limited thereto.

[0067] The tertiary amine co-initiator is one or more of active amine 002 and active amine 008, but is not limited thereto.

[0068] The photoinitiator is one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methylphenylacetone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and 1-hydroxycyclohexylphenyl ketone, but is not limited thereto.

[0069] In addition, the photocurable ink may also include prepolymers. Under the action of ultraviolet light, the photoinitiator in the photocurable ink system can undergo a photochemical reaction and generate active groups, thereby initiating crosslinking and polymerization of monomers and prepolymers in the photocurable ink, so that the photocurable ink changes from a liquid coating to a solid coating in a very short time.

[0070] Exemplarily, after the above-mentioned monomers, tertiary amine co-initiators and photoinitiators are photocured, the acrylic resin is polymerized into a solid state, which is environmentally friendly and energy-saving, and has the advantages of small shrinkage, fast curing and high strength, meeting the needs of solar cells. The isolation layer includes a polymer formed by the polymerization of the photocurable ink. For example, the polymer is polyurethane. The polymer can also be polyisobornyl methacrylate. Alternatively, the polymer can include vinyl polymer and ethyl methacrylate. Alternatively, the polymer can include ethyl methacrylate. Alternatively, the polymer can include isobornyl methacrylate. Alternatively, the polymer can include polyethyl acrylate and polystyrene. Alternatively, the polymer can include polyacrylamide. Alternatively, the polymer can include polyisopropyl methacrylate. Alternatively, the polymer can include polyisobornyl methacrylate and polymethacrylate. Alternatively, the polymer can include methyl isoacrylamide and acrylate.

[0071] It can be understood that due to the different components in the photocurable ink, the polymers formed by the polymerization of the photocurable ink are also diverse. Exemplarily, the polymer has a network structure.

[0072] The formulation of the photocurable ink is described below by way of example.

[0073] Formula 1: alkyl methacrylate, tetrahydrofuran acrylate, 2-phenoxyethyl acrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, active amine 002.

[0074] Formula 2: alkyl methacrylate, dimethyl acrylamide, 1,6-hexanediol dimethacrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, active amine 008.

[0075] Formula 3: dimethylacrylamide, isobornyl acrylate, tetrahydrofuran acrylate, 2-hydroxy-2-methylphenylacetone, and active amine 002.

[0076] Formula 4: dimethylacrylamide, isobornyl acrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and active amine 008.

[0077] Formula 5: 2-phenoxyethyl acrylate, dipropylene glycol diacrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 1-hydroxycyclohexyl phenyl ketone, active amine 008.

[0078] Formula 6: isobornyl acrylate, dipropylene glycol diacrylate, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and active amine 002.

[0079] Formula 7: isobornyl acrylate, 1,6-hexanediol dimethacrylate, 2-hydroxy-2-methylphenylacetone, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and active amine 002.

[0080] Formula 8: dipropylene glycol diacrylate, tetraethylene glycol-diacrylate oligoethylene glycol, 2-hydroxy-2-methylphenylacetone, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and active amine 008.

[0081] Formula 9: dipropylene glycol diacrylate, alkyl methacrylate, 2-hydroxy-2-methylphenylacetone, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, and active amine 002.

[0082] Formula 10: dipropylene glycol diacrylate, dimethyl acrylamide, 2-hydroxy-2-methylphenylacetone, 1-hydroxycyclohexyl phenyl ketone, and active amine 008.

[0083] Formula 11: dipropylene glycol diacrylate, tetrahydrofuran acrylate, 2-hydroxy-2-methylphenylacetone, 1-hydroxycyclohexyl phenyl ketone, and active amine 008.

[0084] Formulation 12: tetraethylene glycol-diacrylate oligoethylene glycol, tetrahydrofuran acrylate, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, and active amine 002.

[0085] Formulation 13: tetraethylene glycol-diacrylate oligoethylene glycol, tetrahydrofuran acrylate, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, and active amine 002.

[0086] Formulation 14: dipropylene glycol diacrylate, dimethyl acrylamide, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenyl ketone, and active amine 002.

[0087] In the embodiment of the present application, the above formula is adopted, and after the light-curable ink is sprayed on the cell and cured, the isolation layer formed can have a spectral transmittance of more than 80% under the irradiation of light with a wavelength of 300nm, thereby improving the conversion efficiency of the cell. In addition, the attenuation of the spectral transmittance of the isolation layer after aging treatment is small, thereby extending the service life of the cell.

[0088] The following is an explanation using Formula 6 as an example.

[0089] In Formula 6, the mass percentage of isobornyl acrylate can be 70-80% (for example, 75%), the mass percentage of dipropylene glycol diacrylate can be 10-15% (for example, 12%), the mass percentage of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide can be 1-5% (for example, 4%), the mass percentage of phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide can be 1-5% (for example, 4%), and the mass percentage of active amine 002 can be 1-5% (for example, 5%).

[0090] like Figure 8 As shown, the sample obtained based on formula 6 (referred to as sample #A) was tested for near-infrared spectral transmittance, and the test wavelength was 400nm to 600nm. It can be seen that the near-infrared spectral transmittance of sample #A is greater than 94.3%.

[0091] When the near infrared spectral transmittance of sample #A meets the preset condition (for example, the preset condition is ≥80%), the sample #A is further subjected to UV aging treatment to obtain sample #B. For example, the UV aging treatment condition is 1200 mJ and irradiation for 200 hours. Fig. 9 As shown, the near infrared spectral transmittance of sample #B was tested at a wavelength of 400nm to 600nm. It can be seen that the near infrared spectral transmittance of sample #B is greater than 91%. It can be seen that the near infrared spectral transmittance attenuation of sample #A after UV aging treatment is less than 5%.

[0092] Further, the sample #B is subjected to heat aging treatment to obtain sample #C. For example, the heat aging treatment is performed at 150°C for 15 minutes, repeated four times, and then heated at 300°C for 100 seconds. Fig. 9 As shown, the near infrared spectral transmittance test of sample #C was carried out at a wavelength of 400nm to 600nm. It can be seen that the near infrared spectral transmittance of sample #C at a wavelength of 480nm to 600nm is greater than 90%. It can be seen that the attenuation of the near infrared spectral transmittance of sample #B after thermal aging treatment is also less than 5%.

[0093] It is understandable that the formulation of the photocurable ink has a great influence on the near-infrared spectral transmittance of the cured sample. For comparison, the present application also provides several other formulations (recorded as formulations A to C), and the samples of these formulations are tested for near-infrared spectral transmittance under the same test conditions. The test results can be seen in Table A below.

[0094] Formula A: 1,6-hexanediol diacrylate (87%), active amine 008 (5%), and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (8%).

[0095] Formulation B: trimethylolpropane trimethacrylate (87%), active amine 002 (5%), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (8%).

[0096] Formula C: tripropylene glycol diacrylate (87%), active amine 002 (2%), active amine 008 (3%), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (8%).

[0097] Table A

[0098] Near infrared spectrum transmittance test results Recipe A Less than 71% Recipe B Less than 65% Recipe C Less than 68%

[0099] Since the near-infrared spectral transmittance test results corresponding to Formula A to Formula C do not meet the preset conditions, there is no need to perform UV aging tests and thermal aging tests on Formula A to Formula C.

[0100] It can be seen that different formulas (for example, the type of monomer in the formula) have a great influence on the near-infrared spectral transmittance test results. The present application can significantly improve the spectral transmittance by setting a suitable formula, thereby improving the conversion efficiency of the battery cell, and reduce the attenuation of the spectral transmittance, thereby extending the service life of the battery cell.

[0101] In addition, the present application also provides a solar cell assembly, including the above-mentioned back-contact solar cell, wherein an isolation layer is arranged on the top layer of the front side of the back-contact solar cell, and the isolation layer is formed by curing photocurable ink.

[0102] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A back contact solar cell, characterized in that: The back-contact solar cell comprises an isolation layer arranged on a top layer of the front side of the back-contact solar cell, wherein the isolation layer is formed by curing a photocurable ink.

2. The back contact solar cell according to claim 1, characterized in that: The isolation layer is a planar structure.

3. The back contact solar cell according to claim 1, characterized in that: The isolation layer consists of a plurality of evenly distributed isolation lines.

4. The back contact solar cell according to claim 1, characterized in that: The plurality of isolation lines are perpendicular to the back side fine grid lines of the back contact solar cell.

5. The back contact solar cell according to claim 1, characterized in that: The isolation layer is composed of a plurality of evenly distributed isolation points.

6. The back contact solar cell according to claim 5, characterized in that: Some of the plurality of isolation points form a plurality of equilateral triangles, and each of the plurality of equilateral triangles is composed of three adjacent isolation points.

7. The back contact solar cell according to claim 6, characterized in that: The side length of the equilateral triangle is 0.5-4 mm.

8. The back-contact solar cell according to any one of claims 1 to 5, characterized in that: The back side of the back-contact solar cell includes a welding point, and the isolation layer is not provided at a position corresponding to the welding point on the front side of the back-contact solar cell.

9. The back-contact solar cell according to any one of claims 1 to 5, characterized in that: The thickness of the isolation layer is 3 to 100 microns.

10. A solar cell module, characterized in that: A back-contact solar cell comprising the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Solar cell and photovoltaic module

    CN119866111A

  • Solar cell and photovoltaic module

    CN119997623A

  • Back contact cell and manufacturing method thereof, laminated cell and photovoltaic module

    CN122094240A

  • Back contact cell and method of manufacturing the same, stacked cell, photovoltaic module

    CN122094240B

  • Solar cell and photovoltaic system

    WO2026214068A1