Composite positive electrode material and preparation method and application thereof

By using composite positive electrode materials in high nickel-based all-solid state batteries, using fluorine-containing chloride electrolytes and high ionic conductivity halide electrolytes or sulfide electrolytes to form a stable electrochemical interface, which solves the easy decomposition of chloride electrolytes and the easy decomposition of chloride electrolytes and The problem of large interface impedance achieves high capacity and stable cycling performance of the battery at large magnification.

CN119008892AInactive Publication Date: 2024-11-22HUAZHONG UNIV OF SCI & TECH

Patent Information

Application Number
CN202411101642.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

High-nickel-based all-solid-state batteries have solid-solid interface problems during the charge and discharge cycle, resulting in problems such as unstable positive electrode structure, physical contact failure of interface, chemical/electrochemical side reactions and space charge layer interfaces. The chloride electrolyte is easy to decompose. The interface resistance is large, and the battery capacity drops rapidly at large magnification.

Method used

Using a composite positive electrode material, including a core, a first cladding layer and a second cladding layer, the first cladding layer uses a fluorine-containing chloride electrolyte, and the second cladding layer uses a halide electrolyte and/or a sulfide electrolyte, through Mixed ball mill preparation to form a stable electrochemical interface and reduce interface impedance.

Benefits of technology

It improves electrochemical stability and ionic conductivity, maintains a high charge and discharge capacity at large magnification, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008892A_ABST
    Figure CN119008892A_ABST
Patent Text Reader

Abstract

The invention discloses a composite positive electrode material and a preparation method and application thereof. The composite positive electrode material comprises an inner core, a first coating layer and a second coating layer, the surface of the inner core is coated with the first coating layer, and the surface of the first coating layer is coated with the second coating layer; wherein the chemical formula of the inner core is LiNixCoyMnzO2, x + y + z = 1, the first coating layer comprises fluorine-containing chloride electrolyte, and the second coating layer comprises halide electrolyte and / or sulfide electrolyte. The fluorine-containing chloride electrolyte is used as the first coating layer, and the halide electrolyte and / or the sulfide electrolyte are / is used as the second coating layer material, so that the obtained composite positive electrode material has relatively high electrochemical stability and relatively high ionic conductivity at the same time, and rapid charging and discharging can be realized at a high rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of positive electrode materials, and in particular relates to a composite positive electrode material and a preparation method and application thereof. Background Art

[0002] The energy density of the battery is mainly calculated by the theoretical capacity of the positive electrode material, the voltage and the mass or volume of the battery. To achieve high energy density and improve the theoretical capacity of the positive electrode material has become a key factor. 0.90 Mn 0.05 Co 0.05 O2(NCM911) cathode material has a high theoretical capacity (≥200 mAh g -1 ) and energy density (about 800 Wh kg -1 ), due to its low Co content, low cost and low toxicity, it has become one of the mainstream research directions of positive electrode materials. However, studies have found that as the Ni content increases, it will bring some problems between the "solid-solid" interface with the electrolyte: (1) During the battery charging process, the Ni of NCM911 3+ and Ni 2+ Oxidized to strong oxidizing Ni 4+ , which is very easy to undergo oxidation reaction with sulfide electrolytes to generate inert phases such as phosphates, sulfates and metal sulfides, which increase the positive electrode interface impedance; (2) During cyclic charge and discharge, the positive electrode material will undergo a series of phase changes, and the lattice will change to varying degrees. In particular, when the voltage is greater than 4.0 V, the amount of lithium ions released increases, the c-axis will shrink sharply, and strong internal stress will be generated. Repeated stress and strain will not only cause serious microcracks in the positive electrode particles, leading to breakage, but also make it easy for the positive electrode particles and the electrolyte to produce interface contact failure, thereby causing battery failure; (3) Ni in the NCM911 lattice 3+ The ions are unstable, and some Ni 3+ Easily reduced to Ni 2+ Ion, Ni 2+ With Li + The similar ionic radius of Li / Ni makes it easy for Li / Ni to be mixed. + Entering the transition metal layer, Ni 2+ Ions easily enter Li + layer, which makes the structure unstable, causing the lattice oxygen to be lost and become free oxygen. Oxygen and sulfide electrolyte react to generate PO4 3- The byproduct increases the interface impedance. In addition, the cathode with lost lattice oxygen will degenerate into spinel phase or rock salt phase, resulting in changes in the interface ion and electron transport.

[0003] In order to solve the solid-solid interface problem of high nickel-based all-solid-state batteries during the charge and discharge cycle, the problems of poor positive electrode structure stability, interface physical contact failure, chemical / electrochemical side reactions and space charge layer interface are solved. At present, chloride electrolytes are commonly used in all-solid-state batteries to contact the positive electrode. However, under high voltage, the chloride electrolyte will decompose slightly, and the oxygen in the positive electrode will react to form ClO compounds under high voltage, increasing the interface impedance. The decomposition of the electrolyte and the reaction at the interface severely limit the battery's ability to charge and discharge at high currents, causing the battery capacity to drop rapidly at high rates. Summary of the invention

[0004] In view of the above deficiencies in the prior art, the purpose of the present invention is to provide a composite positive electrode material and a preparation method and application thereof, so as to solve the problems that the existing chloride electrolyte is easy to decompose, the interface resistance is large, and the capacity of the battery decreases rapidly at a high rate.

[0005] To achieve the above object, the present invention is implemented through the following technical solutions: In a first aspect, the present invention provides a composite positive electrode material, comprising a core, a first coating layer, and a second coating layer; the first coating layer is coated on the surface of the core, and the second coating layer is coated on the surface of the first coating layer; Among them, the chemical formula of the core is LiNi x Co y Mn z O2, x+y+z=1, the first coating layer includes a fluorine-containing chloride electrolyte, and the second coating layer includes a halide electrolyte, and / or a sulfide electrolyte.

[0006] Preferably, the oxidation potential of the fluorine-containing chloride electrolyte is ≥4.3V.

[0007] Preferably, the fluorine-containing chloride electrolyte comprises Li2ZrCl 6-x F x , Li2HfCl 6-x F x , Li3YCl 6-x F x , LiTaCl 6-x F x , LiNbCl 6-x F x , LiTaOCl 3-x F x , LiNbOCl 3-x F x One or more of , where 0<x≤3.

[0008] Preferably, the ionic conductivity of the halide electrolyte and the sulfide electrolyte is greater than 1.0 mS cm -1 , oxidation potential ≤4.2V.

[0009] Preferably, the halide electrolyte includes at least one of Li2ZrCl6, Li2HfCl6, Li3YCl6, LiTaCl6, LiNbCl6, LiTaOCl4, and LiNbOCl4; the sulfide electrolyte includes Li6PS5Cl, Li 5.5 PS 4.5 Cl 1.5 , Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 At least one of .

[0010] In a second aspect, the present invention provides a method for preparing a composite positive electrode material, comprising the following steps: Mixing and ball-milling the first coating layer material and the core material under inert gas conditions to obtain a first coated positive electrode material; The first coating positive electrode material and the second coating layer material are mixed and ball-milled under inert gas conditions to obtain a composite positive electrode material.

[0011] Preferably, the first coating layer material and the core material are mixed and ball-milled under inert gas conditions at a ball-milling speed of 250-400 r / min and a ball-milling time of 1-3 h.

[0012] Preferably, the first coated positive electrode material and the second coated layer material are mixed and ball-milled under inert gas conditions at a ball-milling speed of 150-250 r / min and a ball-milling time of 1-2 h.

[0013] Preferably, the mass ratio of the core material, the first coating layer material and the second coating layer material is (50-85): (5-15): (10-35).

[0014] Preferably, the process of mixing the first coated positive electrode material and the second coating layer material under inert gas conditions and ball milling also includes adding a conductive additive. The type of the conductive additive is not limited, and it can be vapor grown carbon fiber (VGCF), carbon nanotubes (CNT), conductive carbon black, etc. The mass percentage of the conductive additive in the composite positive electrode material is less than 10%.

[0015] In a third aspect, the present invention further provides a positive electrode plate, comprising the composite positive electrode material as described in the first aspect or the composite positive electrode material prepared by the preparation method of the composite positive electrode material as described in the second aspect.

[0016] In a fourth aspect, the present invention further provides a secondary battery, comprising the positive electrode sheet as described in the third aspect.

[0017] The beneficial effects of the present invention are: The present invention adopts a fluorine-containing chloride electrolyte as the first coating layer. The fluorine-containing chloride electrolyte has the characteristics of oxidation resistance, and can form a chemically stable buffer layer between the inner core lithium-based oxide material and other solid electrolyte materials, so that the positive electrode material still maintains the original structure at a high charging potential, and the electrochemical stability is enhanced. Since the introduction of fluorine will inevitably reduce the ionic conductivity of the chloride electrolyte, the second coating layer uses a halide electrolyte and / or a sulfide electrolyte with high ionic conductivity, thereby maintaining a high ionic conductivity while ensuring the electrochemical stability of the positive electrode material, and reducing the interface impedance, so that the battery still maintains a high charge and discharge capacity at a high rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings of the embodiment are briefly introduced below.

[0019] Figure 1 This is a cycle performance diagram of the composite cathode material prepared in Example 1 of the present application at a rate of 1C; Figure 2 This is a cycle performance diagram of the composite positive electrode material prepared in Example 2 of the present application at a rate of 1C; Figure 3 This is a cycle performance diagram of the positive electrode material prepared in Example 3 of the present application at a rate of 1C; Figure 4 This is a cycle performance diagram of the positive electrode material prepared in Comparative Example 1 of the present application at a rate of 1C; Figure 5 This is a cycle performance diagram of the positive electrode material prepared in Comparative Example 2 of the present application at a rate of 1C; Figure 6 This is a cycle performance diagram of the positive electrode material prepared in Comparative Example 3 of the present application at a rate of 1C. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The embodiment of the present invention provides a composite positive electrode material, comprising a core, a first coating layer and a second coating layer; the first coating layer is coated on the surface of the core, and the second coating layer is coated on the surface of the first coating layer; wherein the chemical formula of the core is LiNi x Coy Mn z O2, x+y+z=1, the first coating layer includes a fluorine-containing chloride electrolyte, and the second coating layer includes a halide electrolyte, and / or a sulfide electrolyte.

[0022] The composite positive electrode material provided by the present invention has both high electrochemical stability and high ion conductivity, and has a high capacity retention rate at a high rate.

[0023] In some embodiments, the oxidation potential of the fluorine-containing chloride electrolyte is ≥ 4.3 V. In the positive electrode material, the higher the charging potential, the more lithium ions are released, and the greater the capacity obtained. However, due to the limitations of the positive electrode material itself, the current charging cut-off voltage is around 4.3 V. However, the high-voltage stability of current solid electrolytes (such as sulfide and halide electrolytes) is less than 4.2 V, and it is difficult to maintain stability under high voltage. When charged to 4.3 V, both sulfides and halides are prone to decomposition reactions to form decomposition products with poor ionic conductivity. This embodiment selects a fluorine-containing chloride electrolyte with oxidation resistance stability above 4.3 V, so that the original structure can still be maintained when the charging cut-off voltage of 4.3 V is reached, and it has a higher ionic conductivity.

[0024] In some embodiments, the fluorine-containing chloride electrolyte comprises Li2ZrCl 6-x F x , Li2HfCl 6-x F x , Li3YCl 6- x F x , LiTaCl 6-x F x , LiNbCl 6-x F x , LiTaOCl 3-x F x , LiNbOCl 3-x F x One or more of , wherein 0 < x ≤ 3. Preferably, 0.5 ≤ x ≤ 2. In some embodiments, the oxidation limit potential of the halide electrolyte and the sulfide electrolyte of the second coating layer is ≤ 4.2 V, and the ionic conductivity is greater than 1.0 mS cm -1, which is conducive to the rapid migration of lithium ions, reduces the polarization voltage of the battery, and improves the charge and discharge efficiency. Halide electrolytes include but are not limited to at least one of Li2ZrCl6, Li2HfCl6, Li3YCl6, LiTaCl6, LiNbCl6, LiTaOCl4, and LiNbOCl4; sulfide electrolytes include but are not limited to Li6PS5Cl, Li 5.5 PS 4.5 Cl 1.5 , Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 At least one of .

[0025] The present invention is further described in detail below through specific examples.

[0026] Example 1 Positive electrode core material: LiCoO2 (voltage range: 3.0-4.4 V); Conductive additives: vapor grown carbon fiber (VGCF); The first coating layer material is Li2ZrCl4F2, with an oxidation potential of 4.4 V and an ionic conductivity of 0.4 mS cm -1 ; Second coating material: Li2ZrCl6, oxidation potential is 3.8 V, ionic conductivity is 1.1 mS cm -1 .

[0027] The method for preparing a composite positive electrode material comprises the following steps: (1) Mix the Li2ZrCl4F2 electrolyte and the LiCoO2 core. First, mix the materials at a high speed of 300 rpm and ball mill for 2 hours. The ball milling is performed under the protection of high-purity argon (99.999%) to obtain the Li2ZrCl4F2-coated LiCoO2 positive electrode material.

[0028] (2) Li2ZrCl6 and VGCF were mixed with Li2ZrCl4F2 coated LiCoO2 positive electrode materials, and the mixing was carried out at a low speed of 200 rpm. The ball milling time was 1 hour, and the ball milling was carried out under the protection of high-purity argon (99.999%) to obtain a composite positive electrode material coated with two electrolytes. The mass ratio of LiCoO2 positive electrode core: Li2ZrCl4F2 electrolyte: Li2ZrCl6 electrolyte: VGCF conductive additive was 70:10:18:2.

[0029] Example 2 Cathode core material: LiNi 0.9 Co 0.05 Mn 0.05 O2 (voltage range: 2.7-4.3 V); Conductive additives: vapor grown carbon fiber (VGCF); The first coating layer material is Li2ZrCl4F2, with an oxidation potential of 4.3 V and an ionic conductivity of 0.4 mS cm -1 ; Second coating material: LiTaCl6, oxidation potential 4.2 V, ionic conductivity 5.6 mS cm -1 .

[0030] The method for preparing a composite positive electrode material comprises the following steps: (1) Li2ZrCl4F2 electrolyte and LiNi 0.9 Co 0.05 Mn 0.05 The materials were first mixed at a high speed of 300 rpm and the ball milling time was 1 hour. The ball milling was carried out under the protection of high-purity argon (99.999%) to obtain Li2ZrCl4F2 coated LiNi 0.9 Co 0.05 Mn 0.05 O2 positive electrode material.

[0031] (2) LiTaCl6 and VGCF and Li2ZrCl4F2 coated LiNi 0.9 Co 0.05 Mn 0.05 O2 positive electrode materials were mixed, and the mixing was carried out at a low speed of 200 rpm. The ball milling time was 1 hour, and the ball milling was carried out under the protection of high-purity argon (99.999%) to obtain two types of electrolyte-coated composite positive electrode materials. Among them, LiNi 0.9 Co 0.05 Mn 0.05 The mass ratio of O2:Li2ZrCl4F2:LiTaCl6:VGCF is 70:10:17:3.

[0032] Example 3 Positive electrode core material: LiCoO2 (voltage range: 3.0-4.4 V); Conductive additives: vapor grown carbon fiber (VGCF); The first coating layer material is Li2ZrCl4F2, with an oxidation potential of 4.3 V and an ionic conductivity of 0.4 mS cm -1 ; Second coating layer material: Li 5.5 PS 4.5 Cl1.5 , the oxidation potential is 2.8 V, and the ionic conductivity is 9.5 mS cm -1 .

[0033] The method for preparing a composite positive electrode material comprises the following steps: (1) Mixing Li2ZrCl4F2 electrolyte and LiCoO2 positive electrode. First, the mixture is mixed at a high speed of 300 rpm and the ball milling time is 1 hour. The ball milling is carried out under the protection of high-purity argon (99.999%) to obtain Li2ZrCl4F2 coated LiCoO2 positive electrode material.

[0034] (2) Li 5.5 PS 4.5 Cl 1.5 VGCF and Li2ZrCl4F2 coated LiCoO2 positive electrode material were mixed, and the mixing was carried out at a low speed of 200 rpm. The ball milling time was 1 hour, and the ball milling was carried out under the protection of high-purity argon (99.999%) to obtain two types of electrolyte-coated composite positive electrode materials. Among them, LiCoO2: Li2ZrCl4F2: Li 5.5 PS 4.5 Cl 1.5 : The mass ratio of VGCF is 70:10:17:3.

[0035] Comparative Example 1 Positive electrode core material: LiCoO2 (voltage range: 3.0-4.4 V); Conductive additives: vapor grown carbon fiber (VGCF); The first coating layer material is Li2ZrCl6, with an oxidation potential of 3.8 V and an ionic conductivity of 1.1 mS cm -1 .

[0036] The method for preparing a composite positive electrode material comprises the following steps: Li2ZrCl6 electrolyte and VGCF were mixed with LiCoO2 positive electrode. The materials were first mixed at a low speed of 200 rpm and the ball milling time was 1 hour. The ball milling was carried out under the protection of high-purity argon (99.999%) to obtain Li2ZrCl6 coated LiCoO2 positive electrode material. The mass ratio of LiCoO2:Li2ZrCl6:VGCF was 70:28:2.

[0037] Comparative Example 2 Compared with Example 2, in Comparative Example 2, only the first coating layer is provided on the surface of the inner core.

[0038] Cathode core material: LiNi 0.9 Co 0.05 Mn 0.05O2 (voltage range: 2.7-4.3 V); Conductive additives: vapor grown carbon fiber (VGCF); The first coating layer material is Li2ZrCl4F2, with an oxidation potential of 4.3 V and an ionic conductivity of 0.4 mS cm -1 .

[0039] The method for preparing a composite positive electrode material comprises the following steps: Li2ZrCl4F2 electrolyte and VGCF with LiNi 0.9 Co 0.05 Mn 0.05 The mixture was first mixed at a high speed of 300 rpm and the ball milling time was 2 hours. The ball milling was carried out under the protection of high-purity argon (99.999%) to obtain Li2ZrCl4F2 coated LiNi 0.9 Co 0.05 Mn 0.05 O2 positive electrode material. Among them, LiNi 0.9 Co 0.05 Mn 0.05 The mass ratio of O2:Li2ZrCl4F2:VGCF is 70:27:3.

[0040] Comparative Example 3 Compared with Example 2, in Comparative Example 3, only the second coating layer material is disposed on the surface of the inner core.

[0041] Cathode core material: LiNi 0.9 Co 0.05 Mn 0.05 O2 (voltage range: 2.7-4.3 V); Conductive additives: vapor grown carbon fiber (VGCF); Coating material: LiTaCl6, oxidation potential 4.2 V, ionic conductivity 5.6 mS cm -1 .

[0042] The method for preparing a composite positive electrode material comprises the following steps: LiTaCl6 and VGCF with LiNi 0.9 Co 0.05 Mn 0.05 The mixture was first mixed at a high speed of 300 rpm and the ball milling time was 2 hours. The ball milling was carried out under the protection of high-purity argon (99.999%) to obtain LiTaCl6 coated LiNi 0.9 Co 0.05 Mn 0.05 O2 positive electrode material. Among them, LiNi 0.9 Co0.05 Mn 0.05 The mass ratio of O2:LiTaCl6:VGCF is 70:27:3.

[0043] Battery preparation and performance testing Assembling all-solid-state batteries: Weigh a certain amount of Li in the glove box 5.5 PS 4.5 Cl 1.5 The electrolyte powder is cold pressed in a mold with a pressure of 10 MPa to 100 MPa to form the first electrolyte layer. Then a certain amount of electrolyte powder is weighed and cold pressed on one side of the first electrolyte layer in a mold with a pressure of 10 MPa to 100 MPa to form the second electrolyte layer. At this time, a double electrolyte layer (second electrolyte layer / Li 5.5 PS 4.5 Cl 1.5 Electrolyte layer). When the positive electrode has a second coating layer, the type of the second layer of electrolyte powder is the same as the second positive electrode coating layer; that is, when the positive electrode material of Example 1 is assembled into a solid-state battery, the second electrolyte material used in the double electrolyte layer is Li2ZrCl6; when the positive electrode material of Example 2 is assembled into a solid-state battery, the second electrolyte material used in the double electrolyte layer is LiTaCl6; when the positive electrode material of Example 3 is assembled into a solid-state battery, the second electrolyte used in the double electrolyte layer is Li 5.5 PS 4.5 Cl 1.5 .

[0044] When there is only one coating layer on the positive electrode, the type of the second electrolyte powder is the same as the coating layer material; that is, when the positive electrode material of comparative example 1 is assembled into a solid-state battery, the second electrolyte material used in the double electrolyte layer is Li2ZrCl6; when the positive electrode material of comparative example 2 is assembled into a solid-state battery, the second electrolyte material used in the double electrolyte layer is Li2ZrCl4F2; when the positive electrode material of comparative example 3 is assembled into a solid-state battery, the second electrolyte material used in the double electrolyte layer is LiTaCl6.

[0045] The composite positive electrode materials prepared in the embodiment and the comparative example were weighed and added to one side of the cold-pressed second electrolyte layer, and cold-pressed in a mold with a pressure controlled at 10 MPa to 350 MPa. Subsequently, the Li-In alloy sheet was attached to the other side of the first electrolyte layer and cold-pressed at a pressure of 10 MPa to 100 MPa to obtain 6 solid-state batteries. The charge and discharge tests were carried out at a rate of 1C, and the ratio of the capacity after 20 cycles to the initial capacity was the capacity retention rate after the cycle. The test results are shown in Figure 2. Figures 1 to 6 And as shown in Table 1.

[0046] Table 1

[0047] Depend on Figures 1 to 6 As shown in Table 1, the composite positive electrode material provided by the present invention has both high electrochemical stability and high ionic conductivity, and still maintains a high charge and discharge capacity at a high rate.

[0048] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.

[0049] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A composite positive electrode material, characterized in that: It comprises a core, a first coating layer and a second coating layer; the first coating layer is coated on the surface of the core, and the second coating layer is coated on the surface of the first coating layer; Wherein, the chemical formula of the core is LiNi x Co y Mn z O2, x+y+z=1, the first coating layer includes a fluorine-containing chloride electrolyte, and the second coating layer includes a halide electrolyte and / or a sulfide electrolyte.

2. The composite positive electrode material according to claim 1, characterized in that The oxidation potential of the fluorine-containing chloride electrolyte is ≥ 4.3 V.

3. The composite positive electrode material according to claim 2, characterized in that The fluorine-containing chloride electrolyte includes Li2ZrCl 6-x F x , Li2HfCl 6-x F x , Li3YCl 6-x F x , LiTaCl 6-x F x , LiNbCl 6-x F x , LiTaOCl 3-x F x , LiNbOCl 3-x F x One or more of , where 0 < x ≤ 3.

4. The composite positive electrode material according to claim 1, characterized in that The ionic conductivity of the halide electrolyte and the sulfide electrolyte is greater than 1.0 mS cm -1 , its oxidation potential is ≤ 4.2V.

5. The composite positive electrode material according to claim 4, characterized in that: The halide electrolyte includes at least one of Li2ZrCl6, Li2HfCl6, Li3YCl6, LiTaCl6, LiNbCl6, LiTaOCl4, and LiNbOCl4; The sulfide electrolyte includes Li6PS5Cl, Li 5.5 PS 4.5 Cl 1.5 , Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 At least one of .

6. The method for preparing a composite positive electrode material according to any one of claims 1 to 5, characterized in that: The following steps are involved: Mixing and ball-milling the first coating layer material and the core material under inert gas conditions to obtain a first coated positive electrode material; The first coated positive electrode material and the second coated layer material are mixed and ball-milled under inert gas conditions to obtain the composite positive electrode material.

7. The method for preparing a composite positive electrode material according to claim 6, characterized in that: The first coating layer material and the core material are mixed and ball-milled under inert gas conditions at a ball-milling speed of 250 to 400 r / min for a ball-milling time of 1 to 3 h; The first coated positive electrode material and the second coated layer material are mixed and ball-milled under inert gas conditions at a ball-milling speed of 150-250 r / min and a ball-milling time of 1-2 h.

8. The method for preparing a composite positive electrode material according to claim 6, characterized in that: The mass ratio of the core material, the first coating layer material and the second coating layer material is (50-85): (5-15): (10-35).

9. A positive electrode sheet, characterized in that: Comprising the composite positive electrode material as described in any one of claims 1 to 5.

10. A secondary battery, characterized in that: Comprising the positive electrode sheet as described in claim 9.

Citation Information

Patent Citations

  • Chalcogenide solid electrolyte composite oxide positive electrode material as well as preparation method and application thereof

    CN116230860A

  • Positive electrode for all-solid secondary battery and all-solid secondary battery including the same

    US20210280865A1

  • Positive electrode active material and preparation therefor, positive electrode sheet, and secondary battery

    WO2024073883A1

Cited By

  • Halide sulfide double-layer coated positive electrode material as well as preparation method and application thereof

    CN120727807A