Carbon-coated sodium vanadium fluorophosphate positive electrode material and preparation method thereof, positive electrode plate and secondary battery
By covering the carbon shell layer on the surface of the sodium vanadium fluorine phosphate positive electrode material and controlling the carbon element content, the problems of poor electron conductivity and low power density of sodium ion batteries are solved, the energy density and cycle stability of the battery are improved, and the energy density and cycling stability of the battery are enhanced, which is enhanced. Prospects of grid-level energy storage applications.
Patent Information
- Application Number
- CN202411139879.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
AI Technical Summary
The poor electron conductivity and low power density of the positive electrode material of sodium ion battery limit their wide application in grid-level energy storage applications.
By covering the carbon shell layer on the surface of the positive electrode material of vanadium fluorine phosphate, electron conductivity is improved, and by controlling the mass fraction and particle size of carbon elements, the particle contact area is increased, the migration of sodium ions and the charging and discharge specific capacity of the battery is improved, and the charging and discharge capacity of the battery is improved. .
It significantly improves the electronic conductivity and energy density of the positive electrode material, improves the power density and cycling stability of the secondary battery, and enhances its prospects for grid-level energy storage applications.
Smart Images

Figure CN119008903A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of secondary batteries, and in particular to a sodium vanadium fluorophosphate positive electrode material and a preparation method thereof, a positive electrode sheet and a secondary battery. Background Art
[0002] Sodium-ion batteries (SIBs) are the most likely alternative to lithium-ion batteries for grid-scale energy storage because their working principles are similar to those of mainstream lithium-ion batteries (LIBs) and sodium ions are abundant and inexpensive in the earth's crust. However, electrode materials for SIBs still face some challenges, such as difficult-to-overcome structural instability, slow ion diffusion, low operating voltage, and low energy / power density. To address these issues, scientists studying SIBs are mainly committed to designing and preparing new electrode materials with high adaptability and reversibility during sodium ion intercalation / extraction. For the positive electrode materials of SIBs, transition metal oxides (TMOs) and polyanionic compounds (PACs) are the two most promising candidate materials. In contrast, PACs generally have longer cycle lives because the structural stability of the polyanionic framework is higher than that of TMOs. One of the main potential applications of SIBs is grid-scale energy storage, and ultra-long cycle life is one of its most basic requirements. Therefore, it can be inferred that if the comprehensive electrochemical properties of PACs, such as rate performance, specific capacity, and operating voltage, are improved, their prospects in the application field of SIBs will be very broad.
[0003] Sodium superionic conductor (NASICON) is one of the representative PAC materials, in which there is a stable three-dimensional (3D) open framework composed of PO tetrahedrons and MO octahedrons (M represents transition metal), which enables the rapid migration of Na+. The energy density that NASICON can provide is significantly lower than the theoretical value of phosphate-based cathode materials in LIBs. Therefore, a major challenge facing NASICON is to improve the energy density and thus narrow the gap between current values and practical applications. In order for NASICON to achieve higher energy density, it is easier to increase the operating voltage than to increase the capacity. Compared with NASICON without fluorine, NASICON doped with F generally has a higher operating voltage. For example, the typical NASICON Na 3 V 2 (PO 4 ) 2 F 3 (NVPF) can provide an average operating voltage of up to 3.95V and a theoretical capacity of 128mAh g -1 , the corresponding theoretical energy density is as high as 507Wh·kg -1However, as a member of the NASICON family, NVPF also inherits the defect of low electronic conductivity, which limits the rate performance of the battery, thus having a certain impact on the power density and hindering its application. Summary of the invention
[0004] In view of the technical problems existing in the background technology, the present application provides a carbon-coated sodium vanadium fluorophosphate positive electrode material and a preparation method thereof, a positive electrode plate and a secondary battery, aiming to solve the problem of poor electronic conductivity of the sodium vanadium fluorophosphate positive electrode material.
[0005] In the first aspect, the embodiment of the present application provides a carbon-coated sodium vanadium fluorophosphate positive electrode material, including a core layer and a shell layer; wherein the material of the core layer includes sodium vanadium fluorophosphate, and the material of the shell layer includes carbon; in the carbon-coated sodium vanadium fluorophosphate positive electrode material, the mass fraction of the carbon element is 1.8%-3%, and its D50 particle size is 3μμm-10μμm, and the compaction density is 1.8g / cm 3 -2.1g / cm 3 .
[0006] In the technical solution of the embodiment of the present application, the electronic conductivity of the positive electrode material can be improved by carbon-coating sodium vanadium fluorophosphate; in addition, controlling the mass fraction of the carbon element and the D50 particle size is helpful for the migration of sodium ions and improving the charge capacity and discharge capacity of the battery.
[0007] In some embodiments, the mass fraction of carbon element in the carbon-coated sodium vanadium fluorophosphate positive electrode material is 2.4%-2.8%.
[0008] In this embodiment, by further controlling the mass fraction of the carbon element, the charge specific capacity and discharge specific capacity of the battery can be further improved.
[0009] In some embodiments, the BET specific surface area of the carbon-coated sodium vanadium fluorophosphate positive electrode material is 14 m 2 / g-18.5m 2 / g.
[0010] In this embodiment, the BET specific surface area of the carbon-coated sodium vanadium fluorophosphate positive electrode material is controlled to increase the contact area between the positive electrode material and the electrolyte, thereby increasing the sodium ion deintercalation rate in the positive electrode material.
[0011] In some embodiments, the chemical formula of sodium vanadium fluorophosphate is Na 3 V 2 (PO 4 ) 2 F 3 .
[0012] In this embodiment, the cycle performance of the carbon-coated sodium vanadium fluorophosphate positive electrode material can be improved by controlling the type of sodium vanadium fluorophosphate.
[0013] In a second aspect, the present application provides a method for preparing a carbon-coated sodium vanadium fluorophosphate positive electrode material, comprising the following steps:
[0014] A carbon-coated sodium vanadium fluorophosphate precursor is prepared using vanadium phosphate crystals, a fluorine source, a sodium source and a carbon source;
[0015] calcining the carbon-coated sodium vanadium fluorophosphate precursor to obtain the carbon-coated sodium vanadium fluorophosphate positive electrode material;
[0016] The carbon-coated sodium vanadium fluorophosphate positive electrode material comprises a core layer and a shell layer, the material of the core layer comprises sodium vanadium fluorophosphate, the material of the shell layer comprises carbon, and the mass fraction of the carbon element in the carbon-coated sodium vanadium fluorophosphate positive electrode material is 1.8%-3%, the D50 particle size is 3μm-10μm, and the compaction density is 1.8g / cm 3 -2.1g / cm 3 .
[0017] In the technical solution of the embodiment of the present application, by first preparing vanadium phosphate crystals, and then preparing carbon-coated sodium vanadium fluorophosphate with a fluorine source, a sodium source and a carbon source, a compacted density of 1.8 g / cm 3 -2.1g / cm 3 The positive electrode material comprises a shell layer including carbon and a core layer including sodium vanadium fluorophosphate.
[0018] In some embodiments, the vanadium phosphate crystals are in an orthorhombic form.
[0019] In this embodiment, the orthorhombic vanadium phosphate has high ion conductivity and can effectively improve the performance and cycle life of the battery.
[0020] In some embodiments, the method for preparing vanadium phosphate crystals comprises the following steps:
[0021] The vanadium source, the reducing agent, water and the phosphorus source are mixed and reacted under heating conditions to obtain a mixed material;
[0022] Drying the mixture to obtain a vanadium phosphate precursor;
[0023] The vanadium phosphate precursor is calcined to obtain vanadium phosphate crystals.
[0024] In this embodiment, vanadium phosphate crystals with high purity can be obtained by calcination.
[0025] In some embodiments, in the above-mentioned vanadium phosphate crystals, fluorine source, sodium source, and carbon source, the molar ratio of vanadium phosphate, fluorine element, sodium element, and carbon element is 1:(1.4-1.6):(1.4-1.6):(0.55-0.65).
[0026] In this embodiment, the above-mentioned control of the ratio of each component is helpful to prepare a carbon-coated sodium vanadium fluorophosphate positive electrode material with a complete sodium vanadium phosphate crystal structure.
[0027] In some embodiments, the specific preparation method of the carbon-coated sodium vanadium fluorophosphate precursor is: after mixing vanadium phosphate crystals, a fluorine source, a sodium source, and a carbon source, ethanol is added, and the mixture is ball-milled for 5h-24h to obtain the carbon-coated sodium vanadium fluorophosphate precursor.
[0028] In this embodiment, the materials can be mixed more evenly by ball milling, and the composition of the prepared positive electrode material is also more uniform.
[0029] In some embodiments, the temperature for calcining the carbon-coated sodium vanadium fluorophosphate precursor is 600° C.-800° C., and the calcination time is 0.5 h-5 h.
[0030] In this embodiment, the above-mentioned control of the calcination conditions is helpful to prepare a carbon-coated sodium vanadium fluorophosphate positive electrode material with a complete structure, which is beneficial to improving the cycle life of the carbon-coated sodium vanadium fluorophosphate positive electrode material.
[0031] In some embodiments, the carbon source is at least one of glucose, PEG-2000, and sucrose.
[0032] In this embodiment, the above materials are selected as carbon sources to form a shell layer with good conductivity.
[0033] In the third aspect, an embodiment of the present application provides a positive electrode plate, which includes a current collector and a positive electrode active material, a conductive agent, and a binder located on one side or both sides of the current collector; wherein the positive electrode active material is the carbon-coated sodium vanadium fluorophosphate positive electrode material of the first aspect of the present application or the sodium vanadium fluorophosphate positive electrode material prepared by the preparation method of the second aspect of the present application.
[0034] In this embodiment, the positive electrode plate includes the above-mentioned carbon-coated sodium vanadium fluorophosphate positive electrode material, and thus has the advantages of high energy density and good rate performance.
[0035] In a fourth aspect, an embodiment of the present application provides a secondary battery, which includes the positive electrode plate of the third aspect of the present application.
[0036] In this embodiment, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantages of high power density and good comprehensive electrochemical performance.
[0037] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0039] Figure 1 is the XRD pattern of the vanadium phosphate crystal in Example 1;
[0040] Figure 2 This is a scanning electron microscope image of the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1;
[0041] Figure 3 The XRD pattern of the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1;
[0042] Figure 4 This is a test diagram of the cycle performance of a secondary battery using the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1 as the positive electrode active material;
[0043] Figure 5 This is a rate performance test diagram of a secondary battery using the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1 as the positive electrode active material;
[0044] Figure 6 This is a rate performance test diagram of a secondary battery using the sodium vanadium fluorophosphate positive electrode material in Comparative Example 2 as the positive electrode active material. DETAILED DESCRIPTION
[0045] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0047] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0048] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0049] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0050] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0051] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0052] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0053] Due to the low cost of sodium sources, sodium-ion batteries are considered to be able to replace lithium-ion batteries and become a new generation of secondary batteries. However, the radius of sodium ions is larger than that of lithium ions, their diffusion rate is slower, and the positive electrode material of sodium-ion batteries has poor electronic conductivity, resulting in low power density, making it difficult to use on a large scale.
[0054] In order to solve the technical problems of poor electronic conductivity and low power density of positive electrode materials of sodium ion batteries, the present application provides a carbon-coated sodium vanadium fluorophosphate positive electrode material and a preparation method thereof, a positive electrode plate and a secondary battery, wherein the electronic conductivity of the positive electrode material can be improved by coating the surface of the sodium vanadium fluorophosphate core layer with a carbon shell layer, thereby improving its power density; in addition, by controlling the D50 particle size and compaction density of the carbon-coated sodium vanadium fluorophosphate positive electrode material, it is helpful to improve its energy density, improve the comprehensive electrochemical properties of the positive electrode material, and thus improve the electrochemical properties of the positive electrode plate and the secondary battery.
[0055] In the first aspect, the embodiment of the present application provides a carbon-coated sodium vanadium fluorophosphate positive electrode material, including a core layer and a shell layer; wherein the material of the core layer includes sodium vanadium fluorophosphate, and the material of the shell layer includes carbon; in the carbon-coated sodium vanadium fluorophosphate positive electrode material, the mass fraction of the carbon element is 1.8%-3%, specifically 1.8%, 2%, 2.4%, 2.5%, 2.8%, 3%, 3.5%, etc., or other values within the above range, which are not limited here; its D50 particle size is 3μm-10μm, specifically 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 10μm, etc., or other values within the above range, which are not limited here; its compacted density is 1.8g / cm 3 -2.1g / cm 3 , specifically 1.85g / cm 3 , 1.9g / cm 3 , 1.95g / cm 3 , 2g / cm 3 , 2.05g / cm 3 , 2.06g / cm 3 , 2.1g / cm 3 The value may also be other values within the above range and is not limited here.
[0056] In the description of this application, the term "D50 particle size" refers to the value at which 50% of the particles in the particle distribution have diameters less than or equal to this value, and the D50 particle size is measured using a Malvern laser particle size analyzer.
[0057] In the description of the present application, the term "compacted density" refers to the density of a material tested by a compacted density meter after compaction under a pressure of 3.0 T.
[0058] The conductivity of carbon materials is relatively high. By coating the surface of the sodium vanadium fluorophosphate core layer with a carbon shell layer of appropriate thickness, the electronic conductivity of the sodium vanadium fluorophosphate positive electrode material can be effectively improved. In addition, controlling the D50 particle size and compaction density of the carbon-coated sodium vanadium fluorophosphate positive electrode material helps to increase the contact area between the particles, which is beneficial to further improve its charge and discharge specific capacity and improve the power density.
[0059] Furthermore, in some embodiments, the mass fraction of carbon element in the carbon-coated sodium vanadium fluorophosphate positive electrode material is 2.4%-2.8%, specifically 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, etc., or other values within the range, which are not limited here.
[0060] In the technical solution of the embodiment of the present application, by further optimizing the content of carbon element, on the one hand, it helps to improve the conductivity of the positive electrode material, and on the other hand, it can make it easier for sodium ions to be embedded and deintercalated in the positive electrode material.
[0061] Furthermore, in some embodiments, the BET specific surface area of the carbon-coated sodium vanadium fluorophosphate positive electrode material is 9 m 2 / g-22m 2 / g. Preferably, the BET specific surface area of the carbon-coated sodium vanadium fluorophosphate positive electrode material is 14 m 2 / g-18.5m 2 / g, specifically 14m 2 / g, 14.5m 2 / g, 15m 2 / g, 16m 2 / g, 17m 2 / g, 18.5m 2 / g, etc., and may also be other values within this range, which are not limited here.
[0062] In the technical solution of the embodiment of the present application, controlling the BET specific surface area helps to control the contact area between the positive electrode material and the electrolyte, thereby improving the ion diffusion rate and helping to increase the power density of the positive electrode material.
[0063] Further, in some embodiments, the chemical formula of sodium vanadium fluorophosphate is Na 3 V 2 (PO 4 ) 2 F 3 .
[0064] In the technical solution of the embodiment of the present application, Na 3 V 2 (PO 4 ) 2 F 3This is because the carbon-coated sodium vanadium fluorophosphate positive electrode material prepared with it has higher charge and discharge specific capacity and cycle stability, and is more safe.
[0065] In a second aspect, the present application provides a method for preparing a carbon-coated sodium vanadium fluorophosphate positive electrode material, comprising the following steps:
[0066] A carbon-coated sodium vanadium fluorophosphate precursor is prepared using vanadium phosphate crystals, a fluorine source, a sodium source and a carbon source;
[0067] calcining the carbon-coated sodium vanadium fluorophosphate precursor to obtain the carbon-coated sodium vanadium fluorophosphate positive electrode material;
[0068] The carbon-coated sodium vanadium fluorophosphate positive electrode material comprises a core layer and a shell layer, the material of the core layer comprises sodium vanadium fluorophosphate, the material of the shell layer comprises carbon, and the mass fraction of the carbon element in the carbon-coated sodium vanadium fluorophosphate positive electrode material is 1.8%-3%, the D50 particle size is 3μm-10μm, and the compaction density is 1.8g / cm 3 -2.1g / cm 3 .
[0069] In the technical scheme of the embodiment of the present application, by first preparing vanadium phosphate crystals and then preparing a carbon-coated sodium vanadium fluorophosphate positive electrode material, the charge and discharge specific capacity of the obtained carbon-coated sodium vanadium fluorophosphate positive electrode material can be significantly improved, the charge and discharge curve polarization is small, and the power density is high; and it is easier to control the content of carbon element in the obtained carbon-coated sodium vanadium fluorophosphate positive electrode material and the size of the obtained carbon-coated sodium vanadium fluorophosphate; in addition, mixing vanadium phosphate crystals with a fluorine source, a sodium source, and a carbon source to prepare a carbon-coated sodium vanadium fluorophosphate precursor can prepare a compacted density of 1.8 g / cm 3 -2.1g / cm 3 The carbon-coated sodium vanadium fluorophosphate positive electrode material is beneficial to improving the energy density of the carbon-coated sodium vanadium fluorophosphate positive electrode material.
[0070] In some embodiments, the method for preparing the carbon-coated sodium vanadium fluorophosphate positive electrode material is used to prepare the carbon-coated sodium vanadium fluorophosphate positive electrode material as described above.
[0071] Furthermore, in some embodiments, the crystal form of the vanadium phosphate crystals is an orthorhombic crystal form.
[0072] In the technical solution of the embodiment of the present application, by selecting orthorhombic vanadium phosphate crystals to prepare carbon-coated sodium vanadium fluorophosphate positive electrode material, the charge-discharge specific capacity and cycle life thereof are higher.
[0073] Furthermore, in some embodiments, the method for preparing vanadium phosphate crystals comprises the following steps:
[0074] The vanadium source, the reducing agent, water and the phosphorus source are mixed and reacted under heating conditions to obtain a mixed material;
[0075] Drying the mixed material to obtain a vanadium phosphate precursor;
[0076] The vanadium phosphate precursor is calcined to obtain vanadium phosphate crystals.
[0077] In the technical solution of the embodiment of the present application, vanadium phosphate crystals with high purity can be prepared by calcination, which can be applied on an industrial scale.
[0078] Further, in some embodiments, the drying method is evaporation, the temperature is 80°C-160°C, for example, it can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, or other values within the range, which is not limited here; the time is 5h-24h, for example, it can be 6h, 8h, 10h, 12h, 13h, 15h, 16h, 18h, 20h, or other values within the range, which is not limited here.
[0079] The drying method is simple, quick, does not require the use of special equipment, and is suitable for industrial application.
[0080] Furthermore, in some embodiments, the calcination temperature of the vanadium phosphate precursor is 700° C.-800° C., and the calcination time is 6 h-10 h.
[0081] In some embodiments, the calcination temperature of the vanadium phosphate precursor may be 710°C, 720°C, 730°C, 750°C, 760°C, 780°C, 790°C, or other values within the range, which are not limited herein.
[0082] In some embodiments, the calcination time of the vanadium phosphate precursor can be 6.5 h, 7 h, 7.5 h, 8 h, 8.5 h, 9 h, 9.5 h, or other values within the range, which are not limited here.
[0083] In the technical solution of the embodiment of the present application, controlling the calcination conditions of the vanadium phosphate precursor helps to prepare orthorhombic vanadium phosphate crystals with higher purity.
[0084] Further, in some embodiments, the vanadium source includes one or both of vanadium pentoxide and ammonium metavanadate; the reducing agent includes one or both of oxalic acid and citric acid; the phosphorus source includes one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphoric acid; and the water includes deionized water, distilled water, pure water, etc., which are not limited here.
[0085] In the technical solution of the embodiment of the present application, the vanadium source and the reducing agent are both selected from common and readily available materials, and the above-mentioned vanadium source, reducing agent and phosphorus source are easily reacted to generate a vanadium phosphate precursor.
[0086] In the technical scheme of the embodiment of the present application, the molar ratio of the vanadium element in the vanadium source and the acid is 1:(1-10), for example, the molar ratio of the vanadium element in the vanadium source and the acid can be 1:2, 1:3, 1:5, 1:6, 1:7, 1:8, 1:9, or other values within the range, which are not limited here; the molar ratio of the vanadium element in the vanadium source and the phosphorus element in the phosphorus source is 1:(0.8-1.2), for example, the molar ratio of the vanadium element in the vanadium source and the phosphorus element in the phosphorus source can be 1:0.85, 1:0.9, 1:0.95, 1:1, 1:1.2, 1:1.15, 1:1.18, or other values within the range, which are not limited here.
[0087] The vanadium phosphate precursor is prepared under the above conditions without causing waste of raw materials.
[0088] Furthermore, in some embodiments, in the above-mentioned vanadium phosphate crystals, fluorine source, sodium source, and carbon source, the molar ratio of the vanadium phosphate crystals, fluorine element, sodium element, and carbon element is 1:(1.4-1.6):(1.4-1.6):(0.55-0.65). For example, in the above-mentioned vanadium phosphate crystals, fluorine source, sodium source and carbon source, the molar ratio of the vanadium phosphate crystals, fluorine element, sodium element and carbon element can be 1:1.4:1.4:0.55, 1:1.4:1.4:0.6, 1:1.4:1.4:0.65, 1:1.5:1.5:0.55, 1:1.5:1.5:0.6, 1:1.5:1.5:0.65, 1:1.6:1.6:0.55, 1:1.6:1.6:0.6, 1:1.6:1.6:0.65, and it can also be other ratios within this range, which is not limited here.
[0089] In the technical solution of the embodiment of the present application, by controlling the amount ratio of vanadium phosphate, fluorine element, sodium element and carbon element, it is helpful to prepare a phosphate having a chemical formula of Na 3 V 2 (PO 4 ) 2 F 3 Sodium vanadium fluorophosphate core layer material.
[0090] Furthermore, in some embodiments, the specific preparation method of the carbon-coated sodium vanadium fluorophosphate precursor is: after mixing vanadium phosphate crystals, a fluorine source, a sodium source, and a carbon source, ethanol is added, and the carbon-coated sodium vanadium fluorophosphate precursor is obtained by ball milling for 5h-24h.
[0091] In some embodiments, the ball milling time can be 6 h, 8 h, 10 h, 12 h, 15 h, 17 h, 20 h, 22 h, or other values within the range, which are not limited here.
[0092] In the technical solution of the embodiment of the present application, the above method can be used to make the composition uniformity of the carbon-coated sodium vanadium fluorophosphate precursor higher.
[0093] Furthermore, in some embodiments, the temperature for calcining the carbon-coated sodium vanadium fluorophosphate precursor is 600° C.-800° C., and the calcination time is 0.5 h-5 h.
[0094] In some embodiments, the temperature of calcining the carbon-coated sodium vanadium fluorophosphate precursor can be 650°C, 680°C, 700°C, 720°C, 750°C, 780°C, or other values within this range, which is not limited herein; the time for calcining the carbon-coated sodium vanadium fluorophosphate precursor can be 0.6h, 0.8h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, or other values within this range, which is not limited herein.
[0095] In the technical solution of the embodiment of the present application, the calcined product has higher crystallinity and better cycle stability.
[0096] Furthermore, in some embodiments, the carbon source is at least one of glucose, PEG-2000, and sucrose, and the fluorine source and sodium source are sodium fluoride.
[0097] In the technical solution of the embodiment of the present application, no other impurities will be introduced and the carbon coating effect is good.
[0098] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising the carbon-coated sodium vanadium fluorophosphate positive electrode material of the first aspect of the present application or the carbon-coated sodium vanadium fluorophosphate prepared by the preparation method of the second aspect of the present application.
[0099] In a fourth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode sheet of the third aspect of the present application.
[0100] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0101] 1. Preparation method
[0102] Example 1
[0103] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is as follows:
[0104] (1) 0.1 mol of vanadium pentoxide and 0.3 mol of oxalic acid are added to 500 mL of deionized water, heated at 80° C., and stirred for 1 hour until completely dissolved, and then 0.2 mol of diammonium dihydrogen phosphate is added, stirred for 3 hours, and reacted under stirring to obtain a mixed material;
[0105] (2) evaporating the mixture at 120° C. to obtain a vanadium phosphate precursor;
[0106] (3) calcining the vanadium phosphate precursor in an inert atmosphere at a calcination temperature of 750° C. for 8 h, and naturally cooling to room temperature after the calcination to obtain vanadium phosphate crystals;
[0107] (4) adding 0.04 mol of vanadium phosphate crystals, 0.06 mol of sodium fluoride and 0.00382 mol of glucose into a ball mill, and adding 10 mL of anhydrous ethanol, and ball milling at a rate of 400 r / min for 20 h to obtain a carbon-coated sodium vanadium fluorophosphate precursor;
[0108] (5) The carbon-coated sodium vanadium fluorophosphate precursor was calcined in an inert atmosphere at a temperature of 750° C. for 2 h. After the calcination, it was naturally cooled to room temperature and pulverized by air flow to obtain a carbon-coated sodium vanadium fluorophosphate positive electrode material.
[0109] Example 2
[0110] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is as follows:
[0111] (1) 0.2 mol of ammonium metavanadate and 0.6 mol of citric acid were added to 500 mL of deionized water, heated at 80° C., and stirred for 1 h until completely dissolved, and then 0.2 mol of diammonium hydrogen phosphate was added, stirred for 3 h, and reacted under stirring to obtain a mixed material;
[0112] (2) evaporating the mixture at 120° C. to obtain a vanadium phosphate precursor;
[0113] (3) calcining the vanadium phosphate precursor in an inert atmosphere at a calcination temperature of 750° C. for 8 h, and naturally cooling to room temperature after the calcination to obtain vanadium phosphate crystals;
[0114] (4) adding 0.04 mol of vanadium phosphate crystals, 0.056 mol of sodium fluoride and 0.00408 mol of glucose into a ball mill, and adding 10 mL of anhydrous ethanol, and ball milling at a rate of 400 r / min for 5 h to obtain a carbon-coated sodium vanadium fluorophosphate precursor;
[0115] (5) The carbon-coated sodium vanadium fluorophosphate precursor was calcined in an inert atmosphere at a temperature of 750° C. for 2 h. After the calcination, it was naturally cooled to room temperature and pulverized by air flow to obtain a carbon-coated sodium vanadium fluorophosphate positive electrode material.
[0116] Example 3
[0117] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is as follows:
[0118] (1) adding 0.1 mol of vanadium pentoxide and 0.3 mol of oxalic acid to 500 mL of deionized water, heating at 80° C., stirring for 1 hour until completely dissolved, then adding 0.2 mol of phosphoric acid, stirring for 3 hours, and reacting under stirring to obtain a mixed material;
[0119] (2) evaporating the mixture at 120° C. to obtain a vanadium phosphate precursor;
[0120] (3) calcining the vanadium phosphate precursor in an inert atmosphere at a calcination temperature of 750° C. for 8 h, and naturally cooling to room temperature after the calcination to obtain vanadium phosphate crystals;
[0121] (4) adding 0.04 mol of vanadium phosphate crystals, 0.064 mol of sodium fluoride and 0.00378 mol of glucose into a ball mill, and adding 10 mL of anhydrous ethanol, and ball milling at a rate of 400 r / min for 24 h to obtain a carbon-coated sodium vanadium fluorophosphate precursor;
[0122] (5) The carbon-coated sodium vanadium fluorophosphate precursor was calcined in an inert atmosphere at a temperature of 750° C. for 2 h. After the calcination, it was naturally cooled to room temperature and pulverized by air flow to obtain a carbon-coated sodium vanadium fluorophosphate positive electrode material.
[0123] Example 4
[0124] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is different from that of Example 1 only in that, in step (4), the amount of glucose added is 0.00353 mol.
[0125] Example 5
[0126] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is different from that of Example 1 only in that, in step (4), the amount of glucose added is 0.00429 mol.
[0127] Example 6
[0128] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is different from that of Example 1 only in that, in step (4), the amount of sodium fluoride added is 0.04 mol.
[0129] Example 7
[0130] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is different from that of Example 1 only in that in step (5), the calcination temperature is 600° C. and the calcination time is 3 h.
[0131] Example 8
[0132] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is different from that of Example 1 only in that in step (5), the calcination temperature is 800° C. and the calcination time is 0.5 h.
[0133] Example 9
[0134] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is different from that of Example 1 only in that in step (5), the calcination temperature is 600° C. and the calcination time is 1 hour.
[0135] Example 10
[0136] An embodiment of the carbon-coated sodium vanadium fluorophosphate positive electrode material of the present application, the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material of this embodiment is different from that of Example 1 only in that in step (5), the calcination temperature is 800° C. and the calcination time is 4 hours.
[0137] Comparative Example 1
[0138] A carbon-coated sodium vanadium fluorophosphate positive electrode material, the preparation method of which is different from that of Example 1 only in that, in step (4), the amount of glucose added is 0.007 mol.
[0139] Comparative Example 2
[0140] A sodium vanadium fluorophosphate positive electrode material, the preparation method of which is different from that of Example 1 only in that glucose is not added in step (4).
[0141] Comparative Example 3
[0142] A carbon-coated sodium vanadium fluorophosphate positive electrode material, the preparation method of which is different from that of Example 1 only in that the timing of adding glucose is different. In step (3), a vanadium phosphate precursor and glucose are mixed, and carbon-coated vanadium phosphate crystals are obtained by calcining at 750° C. for 8 hours; and glucose is not added in step (4).
[0143] 2. Test Method
[0144] 1. Property test of vanadium phosphate crystals
[0145] Crystal structure: The test was conducted using a D8 Focus X-ray powder diffractometer from Bruker, Germany, using Cu-Kα as the radiation source with a wavelength of 1.5046λ; using a Ni filter, a tube current of 40 mA, a tube voltage of 40 KV, a scanning range of 5°-90°, a scanning speed of 5° / min, and a step length of 0.05°. The material was placed on a glass slide and flattened, and the glass slide was embedded in the center of the instrument experimental slot for testing; the identification of the physical phase and the crystal structure information were analyzed by JADE 6.0 software.
[0146] 2. Properties test of carbon-coated sodium vanadium fluorophosphate positive electrode material and sodium vanadium fluorophosphate positive electrode material
[0147] Morphology: The morphology test was carried out using a SU-3500 scanning electron microscope produced by HITACHI with an acceleration voltage of 15KV.
[0148] Mass fraction of carbon element: infrared C / S analyzer;
[0149] D50 particle size: tested using Malvern laser particle size analyzer;
[0150] BET specific surface area: tested using the American Micromeritics company's specific surface area analyzer TriStar II3030plus;
[0151] Compacted density: compacted under 3.0T pressure, pressing time is 30s, and tested using a compacted density meter.
[0152] 3. Battery property test
[0153] Battery assembly: The positive electrode materials in the embodiment and the comparative example are respectively used as the positive electrode active materials of the sodium ion battery, the positive electrode active materials are mixed with the binder polyvinylidene fluoride (PVDF) and the conductive agent conductive carbon black (Super P) in a mass ratio of 7:2:1, and then dimethyl pyrrolidone (NMP) is added as a solvent to mix and stir into a uniform slurry, the slurry is evenly applied on an aluminum foil, and after drying, it is cut into thin sheets as the positive electrode, metallic sodium is used as the negative electrode, and a glass fiber membrane is used as a separator. The solvent in the electrolyte is a mixed solvent formed by ethylene carbonate, polycarbonate, and fluoroethylene carbonate in a volume ratio of 0.45:0.45:0.05, and the solute is NaClO 4 , with a concentration of 1.0 mol / L, and assembled into CR2032 button cells in an argon glove box.
[0154] Electrochemical performance test: The button cells assembled above were tested using the Land battery tester produced by Wuhan Jinnuo Electronics Co., Ltd. The test conditions are as follows:
[0155] Discharge specific capacity and cycle performance: Constant current charge and discharge test was carried out under 0.5C conditions, and the charge and discharge voltage range was 2V-4.3V.
[0156] Rate performance: Rate performance tests were carried out under 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, and 10C conditions in sequence, and the charge and discharge voltage range was 2V-4.3V.
[0157] III. Analysis of test results of various embodiments and comparative examples
[0158] Figure 1 : This is the XRD spectrum of the vanadium phosphate crystals in Example 1. It can be seen from the figure that the position of the diffraction peak of the vanadium phosphate crystals corresponds to the diffraction peak position of the orthorhombic vanadium phosphate on the standard card (JCPDS: 01-076-2023), indicating that the vanadium phosphate crystals in Example 1 are orthorhombic crystals.
[0159] Table 1 is a table showing the performance test results of the positive electrode materials in the embodiments and comparative examples.
[0160] Table 1
[0161]
[0162]
[0163] Figure 2 This is a scanning electron microscope image of the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1. It can be seen from the image that its structure is spherical or quasi-spherical.
[0164] Figure 3 This is the XRD diagram of the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1. There is no impurity peak in the XRD diagram, which is a pure phase of sodium vanadium fluorophosphate, indicating that the material of the core layer of the carbon-coated sodium vanadium fluorophosphate positive electrode material prepared by the method disclosed in the present application is high in purity.
[0165] Table 2 is a table of battery performance test results, in which the charge specific capacity and discharge specific capacity are tested under 0.5C conditions.
[0166] Table 2
[0167]
[0168]
[0169] As shown in Table 2, the initial discharge specific capacity of the carbon-coated sodium vanadium fluorophosphate positive electrode materials obtained in Examples 1-10 is higher than 105 mAh·g-1 After 200 cycles, the discharge capacity is 99 mAh g -1 The above, and the capacity retention rate after 200 cycles is higher than 88%, indicating that the carbon-coated sodium vanadium fluorophosphate positive electrode material has a high energy density and good cycle stability. The carbon coating amount of the positive electrode material in Comparative Example 1 is too much, which affects the ion migration speed and reduces its discharge specific capacity; the positive electrode material in Comparative Example 2 has no carbon coating layer, poor electronic conductivity, and worse electrochemical performance; the carbon element of the positive electrode material in Comparative Example 3 is added when preparing vanadium phosphate, and its compaction density is relatively low, and the specific capacity and cycle performance of the obtained battery are relatively poor.
[0170] In addition, it can be seen from the test results of Examples 1-5 that when the mass fraction of carbon element in the carbon-coated sodium vanadium fluorophosphate positive electrode material is 2.4%-2.8%, its discharge specific capacity and cycle performance are better.
[0171] From the test results of Examples 1-3 and Example 6, it can be seen that when the molar ratio of vanadium phosphate crystals, fluorine element, sodium element and carbon element is 1:(1.4-1.6):(1.4-1.6):(0.55-0.65), the electrochemical performance is significantly better.
[0172] From the performance test results of Examples 1 and 7-10, it can be seen that the BET specific surface area of the carbon-coated sodium vanadium fluorophosphate positive electrode material is 14 m 2 / g-18.5m 2 / g, the electrochemical performance of the prepared battery is better.
[0173] Figure 4 This is a test graph of the cycle performance of the battery made from the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1 under 0.5C conditions, which is consistent with Table 2, has a good specific capacity and good cycle stability.
[0174] Figure 5-6 They are rate performance test graphs of secondary batteries using the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1 and the sodium vanadium fluorophosphate positive electrode material in Comparative Example 2 as positive electrode active materials. It can be seen from the graph that the secondary battery prepared from the carbon-coated sodium vanadium fluorophosphate positive electrode material in Example 1 has good rate performance. When the rate is increased to 5C, it still has a relatively high discharge specific capacity. In addition, when the rate is increased to 10C and then reduced to 0.1C, its discharge specific capacity is almost the same as the initial discharge specific capacity. The result shows that the carbon-coated sodium vanadium fluorophosphate positive electrode material prepared by the present invention has good stability.
[0175] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A carbon-coated sodium vanadium fluorophosphate positive electrode material, characterized in that: The invention comprises a core layer and a shell layer, wherein the material of the core layer comprises sodium vanadium fluorophosphate, the material of the shell layer comprises carbon, and the mass fraction of the carbon element in the carbon-coated sodium vanadium fluorophosphate positive electrode material is 1.8%-3%, the D50 particle size is 3μm-10μm, and the compaction density is 1.8g / cm 3 -2.1g / cm 3 .
2. The carbon-coated sodium vanadium fluorophosphate positive electrode material according to claim 1, characterized in that: In the carbon-coated sodium vanadium fluorophosphate positive electrode material, the mass fraction of the carbon element is 2.4%-2.8%.
3. The carbon-coated sodium vanadium fluorophosphate positive electrode material according to claim 1, characterized in that: The BET specific surface area of the carbon-coated sodium vanadium fluorophosphate positive electrode material is 14 m 2 / g-18.5m 2 / g.
4. The carbon-coated sodium vanadium fluorophosphate positive electrode material according to any one of claims 1 to 3, characterized in that: The chemical formula of the sodium vanadium fluorophosphate is Na3V2(PO4)2F3.
5. A method for preparing a carbon-coated sodium vanadium fluorophosphate positive electrode material, characterized in that: The steps include: A carbon-coated sodium vanadium fluorophosphate precursor is prepared using vanadium phosphate crystals, a fluorine source, a sodium source and a carbon source; calcining the carbon-coated sodium vanadium fluorophosphate precursor to obtain the carbon-coated sodium vanadium fluorophosphate positive electrode material; The carbon-coated sodium vanadium fluorophosphate positive electrode material comprises a core layer and a shell layer, the material of the core layer comprises sodium vanadium fluorophosphate, the material of the shell layer comprises carbon, and the mass fraction of the carbon element in the carbon-coated sodium vanadium fluorophosphate positive electrode material is 1.8%-3%, the D50 particle size is 3μm-10μm, and the compaction density is 1.8g / cm 3 -2.1g / cm 3 .
6. The method for preparing the carbon-coated sodium vanadium fluorophosphate positive electrode material according to claim 5, characterized in that: The crystal form of the vanadium phosphate crystal is an orthorhombic crystal form.
7. The method for preparing the carbon-coated sodium vanadium fluorophosphate positive electrode material according to claim 6, characterized in that: In the vanadium phosphate crystals, the fluorine source, the sodium source and the carbon source, the molar ratio of vanadium phosphate, fluorine element, sodium element and carbon element is 1:(1.4-1.6):(1.4-1.6):(0.55-0.65).
8. The method for preparing the carbon-coated sodium vanadium fluorophosphate positive electrode material according to claim 5, characterized in that: The step of preparing a carbon-coated sodium vanadium fluorophosphate precursor using vanadium phosphate crystals, a fluorine source, a sodium source and a carbon source comprises: mixing the vanadium phosphate crystals, the fluorine source, the sodium source and the carbon source, and ball milling for 5h-24h to obtain the carbon-coated sodium vanadium fluorophosphate precursor; and / or In the step of calcining the carbon-coated sodium vanadium fluorophosphate precursor, the calcination temperature is 600° C.-800° C., and the calcination time is 0.5 h-5 h; and / or The method for preparing the vanadium phosphate crystals comprises the following steps: The vanadium source, the reducing agent, water and the phosphorus source are mixed and reacted under heating conditions to obtain a mixed material; Drying the mixture to obtain a vanadium phosphate precursor; The vanadium phosphate precursor is calcined to obtain vanadium phosphate crystals.
9. A positive electrode sheet, characterized in that: It comprises a current collector and a positive electrode active material, a conductive agent, and a binder located on one side or both sides of the current collector; the positive electrode active material comprises the carbon-coated sodium vanadium fluorophosphate positive electrode material according to any one of claims 1 to 4, or the carbon-coated sodium vanadium fluorophosphate positive electrode material prepared by the preparation method of the carbon-coated sodium vanadium fluorophosphate positive electrode material according to any one of claims 5 to 8.
10. A secondary battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the positive electrode sheet is the positive electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Method for preparing a Na3V2(PO4)2F3 material
CN108349738A
Positive electrode material and preparation method and application thereof
CN112701285A
Porous carbon coated sodium vanadium fluorophosphate positive electrode material and preparation method thereof
CN116544394A
Preparation method of sodium-ion battery positive electrode material sodium vanadium fluorophosphate based on spray drying
CN118458734A
Foldable laptop computer stand
KR102516286B1
Cited By
Sodium battery positive electrode material and preparation method and application thereof
CN119786573A
Preparation method of positive electrode material, pole piece and battery
CN119864403A
A method for preparing positive electrode material, a pole piece, and a battery
CN119864403B
Phosphate-based positive electrode material and preparation method therefor, positive electrode sheet, and secondary battery
EP4804251A4
Carbon-coated sodium vanadium fluorophosphate positive electrode material and preparation method therefor, positive electrode sheet, and secondary battery