Lithium supplement additive, preparation method thereof and secondary battery

By using low crystallinity lithium supplement materials and catalysts in lithium-ion batteries, combined with the preparation method of conductive agents, the irreversible capacity loss caused by solid electrolyte interface masks and the high lithium-ion potential of lithium supplement additives are solved, and the problem of lithium supplementation additives is high. More efficient lithium ion release and battery performance improvements.

CN119008935APending Publication Date: 2024-11-22SHENZHEN DYNANONIC INNOVAZONE NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411051520.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the first charging and discharging process of lithium-ion batteries, the irreversible capacity loss is caused by the formation of solid electrolyte interface film, which reduces the energy density and charging and discharging efficiency of lithium-ion secondary batteries, and the lithium-release potential of existing lithium supplement additives is too high. Increased application difficulty.

Method used

Provided a lithium supplement additive, which includes a low crystallinity lithium supplement material (crystalline less than 50%) and a catalyst, making lithium ions easier to deliver by reducing the crystallinity of the lithium supplement material and using a catalyst to reduce the deliquency voltage platform. , and use conductive agents during the preparation process to improve stability and conductivity.

Benefits of technology

It effectively reduces the deliquency potential platform of lithium supplement material, improves the performance and safety performance of lithium-ion secondary batteries, simplifies the application difficulty of lithium supplement material, and increases the total capacity and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008935A_ABST
    Figure CN119008935A_ABST
Patent Text Reader

Abstract

The invention provides a lithium supplement additive, a preparation method thereof and a secondary battery. The lithium supplement additive comprises a lithium supplement material, the chemical general formula of the lithium supplement material is LixCyOz, x is more than 1 and less than 3, y is more than 0 and less than 8, z is more than 1 and less than 10, the crystallinity of the lithium supplement material is less than 50%, and the lithium removal voltage platform of the lithium supplement material is lower than 4V. According to the lithium supplement material, the crystallinity of the lithium supplement material is reduced, and the proportion of the amorphous lithium supplement material in the lithium supplement material is large, namely, the crystallinity of the lithium supplement material is smaller than 50%, so that the lithium removal voltage platform of the lithium supplement material is lower than 4V. The lithium removal voltage platform of the lithium supplement material is greatly reduced, lithium ions in the lithium supplement material are more easily removed, the application difficulty of the lithium supplement material is reduced, and the safety performance of the lithium supplement material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a lithium supplement additive, a preparation method thereof, and a secondary battery. Background Art

[0002] Lithium-ion batteries have the advantages of high operating voltage and energy density, relatively small self-discharge level, ultra-long cycle life, no memory effect, no pollution by heavy metal elements such as lead and cadmium, etc., and are widely used in many aspects such as electric vehicles, power tools, mobile electronic consumer products and energy storage. However, during the first charge and discharge process of lithium-ion batteries, a large amount of solid electrolyte interface film will be produced on the surface of the negative electrode of the battery, consuming the limited lithium ions and electrolyte in the battery, causing irreversible capacity loss, reducing the energy density of lithium-ion secondary batteries and reducing the charge and discharge efficiency of electrode materials, limiting the application of lithium-ion batteries.

[0003] Positive electrode lithium supplement additives can make up for the irreversible capacity loss caused by the formation of solid electrolyte interface film during the first charge of lithium-ion batteries. It is one of the key technologies to improve the performance of lithium-ion batteries and has a broad application market and development prospects. However, the commonly used lithium supplement additives currently have the problem of high lithium release potential, which even exceeds the commonly used operating voltage range of existing battery systems, increasing the difficulty of applying lithium supplement additives. Summary of the invention

[0004] The present application provides a lithium supplement additive and a preparation method thereof and a secondary battery, aiming to reduce the lithium release potential of the lithium supplement additive.

[0005] In a first aspect, the present application provides a lithium supplement additive, the lithium supplement additive comprising a lithium supplement material, the chemical formula of the lithium supplement material is Li x C y O z , wherein 1<x<3, 0<y<8, 1<z<10, the crystallinity of the lithium supplement material is less than 50%, and the lithium desorption voltage platform of the lithium supplement material is lower than 4V.

[0006] In the present application, by reducing the crystallinity of the lithium supplement material itself, the proportion of amorphous lithium supplement material in the lithium supplement material is relatively large, that is, the crystallinity of the lithium supplement material is less than 50%, so that the lithium de-lithiation voltage platform of the lithium supplement material is lower than 4 V. The lithium de-lithiation voltage platform of the lithium supplement material is greatly reduced, and the lithium ions in the lithium supplement material are easier to be removed, which is conducive to reducing the difficulty of application of the lithium supplement material and improving the safety performance of the lithium supplement material.

[0007] In one embodiment, the crystallinity of the lithium supplementing material is in the range of 10%-50%.

[0008] In one embodiment, the lithium supplement material includes at least one of Li2C2O4, Li2CO3, Li2C4O4, Li2C3O5, Li2C4O6, and Li2C6O6.

[0009] In one embodiment, the difference between the delithiation voltage platform of the lithium supplementing material having a crystallinity of less than 50% and the delithiation voltage platform of the lithium supplementing material having a crystallinity of more than 98% is greater than 0.4V.

[0010] In one embodiment, the lithium-replenishing material has a lithium-removal platform potential of p and a crystallinity of c (0 < c ≤ 0.5), and p and c have the following relationship: When 0 < c < 0.1, p = 40c 2 -8c+4.32; when 0.1≤c≤0.2, p=12c 2 -4.8c+4.28; when 0.2<c<0.5, p=0.6c+3.68.

[0011] In one embodiment, the X-ray diffraction pattern of the lithium supplementing material includes a peak, and the half-peak width of the peak is in the range of 2°-10°.

[0012] In one embodiment, the 2θ angle with the maximum peak intensity corresponding to the envelope peak is 34°, and the 2θ angle corresponding to the envelope peak is 25°-43°.

[0013] In one embodiment, the diffraction peak area of ​​the lithium supplement material with a crystallinity of less than 50% at a 2θ angle of 25°-43° is 3-50 times the diffraction peak area of ​​the lithium supplement material with a crystallinity of more than 98% at a 2θ angle of 33°-35°.

[0014] In one embodiment, the lithium supplement additive further comprises a catalyst. During the preparation of the lithium supplement additive, the catalyst is used to improve the stability of the lithium supplement material.

[0015] In one embodiment, the lithium replenishing material is grown in situ on the outer surface of the catalyst.

[0016] In one embodiment, the catalyst includes at least one of Mo2C, Ti3C2, MnO, MnO2, NiO, CoO, Co3O4, Ru, RuO2, TiO2, MoS2, ZnS, CoS, Co3S4, NiS2, FeS2, and ReS2.

[0017] In one embodiment, the catalyst is also used to catalyze the decomposition of the lithium supplementing material to reduce the delithiation potential platform of the lithium supplementing material.

[0018] In one embodiment, the lithium supplement additive further includes a conductive agent, and the conductive agent is in-situ grown on the outer surface of the catalyst.

[0019] In one embodiment, the mass ratio of the lithium supplement material, the catalyst and the conductive agent is (70-95):(2-15):(3-15).

[0020] In one embodiment, the particle size of the lithium supplement material is 5nm-400nm.

[0021] In one embodiment, the particle size of the catalyst is 5 nm to 150 nm.

[0022] In one embodiment, the particle size of the conductive agent is 10 nm-200 nm.

[0023] In a second aspect, the present application provides a method for preparing a lithium supplement additive, the method for preparing the lithium supplement additive comprising:

[0024] providing or preparing a cathode;

[0025] Using lithium as an anode, assembling the anode and the cathode into a Li-CO2 battery;

[0026] Passing CO2 and / or CO gas into the cathode of the Li-CO2 battery, and obtaining discharge products at the cathode after the Li-CO2 battery is discharged;

[0027] collecting the discharge products and washing and drying the discharge products to obtain the lithium supplement additive;

[0028] The cut-off voltage of the Li-CO2 battery is 2V-2.5V, the discharge current density is 400mA / g-800mA / g, and the crystallinity of the lithium supplement material in the lithium supplement additive is less than 50%.

[0029] In one embodiment, the cathode includes at least one of a catalyst and a conductive agent.

[0030] In one embodiment, the method for preparing the cathode comprises:

[0031] adding a solvent to a catalyst source and a carbon source, and stirring to obtain a solution;

[0032] The solution is placed in an autoclave for hydrothermal reaction, and after washing, drying and calcining, a catalyst precursor is obtained;

[0033] Mixing the catalyst precursor and the conductive agent, and calcining them under an inert atmosphere to obtain a composite of the catalyst and the conductive agent;

[0034] The composite and the binder are mixed and then sprayed onto carbon paper, and then dried to obtain the cathode.

[0035] In a third aspect, the present application provides a secondary battery, which includes a negative electrode material, a separator and a positive electrode material, wherein the positive electrode material includes the lithium supplement additive as described above or the lithium supplement additive prepared by the preparation method of the lithium supplement additive as described above. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments of the present application will be described below.

[0037] Figure 1 This is the first charging curve of the lithium supplement additive provided in Comparative Example 1.

[0038] Figure 2 This is the first charging curve of the lithium supplement additive provided in Example 1 of the present application.

[0039] Figure 3 This is the TEM spectrum of the discharge product provided in Example 1 of the present application.

[0040] Figure 4 This is the SEM spectrum of the discharge product provided in Example 5 of the present application. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0042] In this document, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, "plurality" means two or more.

[0043] In addition, in this article, directional terms such as "upper" and "lower" are defined relative to the orientation of the structure schematically placed in the drawings. It should be understood that these directional terms are relative concepts. They are used for relative description and clarification, and they can change accordingly according to the change of the orientation of the structure.

[0044] For ease of understanding, the English abbreviations and related technical terms involved in the embodiments of the present application are explained and described below.

[0045] SEI membrane: Solid Electrolyte Interface, that is, solid electrolyte interface membrane.

[0046] Batteries such as lithium-ion secondary batteries usually include a positive electrode, a negative electrode and a separator. The positive electrode is used to provide active lithium ions for the battery, and the negative electrode can be used as a carrier of active lithium ions and electrons during the battery charging and discharging process. The separator is arranged between the positive electrode and the negative electrode to separate the positive electrode and the negative electrode, and the separator is used to allow active lithium ions to pass through and block the passage of electrons. The positive electrode includes a positive electrode active material, which is used to provide active lithium ions for the lithium-ion battery, and the active lithium ions migrate between the positive electrode and the negative electrode of the battery, thereby realizing the battery charging and discharging. During the first charging and discharging process of the battery, a large amount of solid electrolyte interface film (SEI film) will be generated on the surface of the electrode, consuming the limited lithium ions in the battery, so that the capacity of lithium ions is greatly reduced, resulting in irreversible capacity loss. Usually, the positive electrode also includes a lithium supplement material, which can provide lithium ions to offset the irreversible lithium loss caused by the formation of the SEI film, thereby increasing the total capacity and energy density of the battery. However, the delithiation potential of the existing lithium supplement additive is relatively high, which is difficult to match the commonly used working voltage of the existing battery system, increasing the difficulty of applying the lithium supplement additive, making it difficult for the capacity and performance of the positive electrode active material to play its due level.

[0047] The present application provides a lithium supplement additive, which is applied to the positive electrode of the battery to pre-lithiate the positive electrode, and to add lithium to the battery before the battery is operated to compensate for the lithium ions consumed by the formation of the SEI film. The lithium supplement additive provided by the present application has a low delithiation potential, and is applied to lithium-ion secondary batteries to effectively improve the performance of lithium-ion secondary batteries.

[0048] In one embodiment, when the lithium supplement additive is used, the lithium supplement additive can be applied to the outer surface of the positive electrode plate of the battery, or the lithium supplement additive can be embedded in the outer surface of the positive electrode plate of the battery. In one embodiment, the lithium supplement additive can also be used after being compounded with the positive electrode active material. In other embodiments, the lithium supplement additive can also be added during the preparation of the positive electrode slurry of the battery, so that the lithium supplement additive is dispersed on the outer surface and inside of the positive electrode plate of the battery.

[0049] The present application provides a lithium supplement additive, which includes a lithium supplement material. The crystallinity of the lithium supplement material is less than 50%, and the lithium desorption voltage platform of the lithium supplement material is less than 4V.

[0050] Among them, during the first charging process, the lithium (Li) in the lithium supplement material can be released and migrate to the negative electrode of the battery to offset the irreversible lithium loss caused by the formation of the SEI film, thereby increasing the total capacity and energy density of the battery.

[0051] Crystallinity refers to the percentage of crystalline phase in the lithium supplement material. Currently available lithium supplement materials are usually crystalline, and the crystallinity of lithium supplement materials is relatively high. For some lithium supplement materials, the crystallinity is relatively high, and the lithium desorption voltage platform is correspondingly relatively high. For example, when the lithium supplement material is lithium oxalate, it is usually in a crystalline state, and the lithium desorption voltage platform of lithium oxalate in a crystalline state is relatively high, up to 4.7V, and the lithium desorption voltage platform even exceeds the commonly used operating voltage range of existing battery systems, which increases the difficulty of applying lithium supplement materials. In addition, when the lithium-ion battery is charged and discharged for the first time, the higher voltage will also make the lithium supplement additives and the positive electrode active materials easily generate gas, and the generated gas will reduce the safety performance of the lithium-ion battery.

[0052] In the embodiment of the present application, by reducing the crystallinity of the lithium supplement material itself, the proportion of the lithium supplement material in the amorphous state in the lithium supplement material is relatively large, that is, the crystallinity of the lithium supplement material is less than 50%, so that the lithium de-lithiation voltage platform of the lithium supplement material is lower than 4 V. The lithium de-lithiation voltage platform of the lithium supplement material is greatly reduced, and the lithium ions in the lithium supplement material are easier to be removed, which is conducive to reducing the difficulty of applying the lithium supplement material and improving the safety performance of the lithium supplement material.

[0053] In one embodiment, the lithium-supplementing material has the general chemical formula Li x C y O z , where 1<x<3, 0<y<8, 1<z<10. Wherein, Li represents a lithium atom, C represents a carbon atom, and O represents an oxygen atom. x C y O z This type of lithium-supplementing compound has the advantages of high capacity, good air stability, excellent solvent compatibility and low cost. x C y O z As a lithium-supplementing material, by adjusting its crystallinity, the lithium-supplementing material not only has the advantages of high capacity and high stability, but also has a lower delithiation voltage platform, which makes the lithium-supplementing material have higher practical value.

[0054] In one embodiment, the lithium supplement material includes at least one of Li2C2O4, Li2CO3, Li2C4O4, Li2C3O5, Li2C4O6, and Li2C6O6. Among them, the above-mentioned lithium supplement compounds have the advantages of high capacity and high stability, but the above-mentioned lithium supplement compounds are easy to crystallize, and the commercially available products are usually crystalline, so that the lithium desorption voltage platform of the above-mentioned crystalline lithium supplement compounds is relatively high. In the embodiment of the present application, by reducing the crystallinity of the lithium supplement material, the lithium desorption voltage platform of the lithium supplement material is reduced, so that the lithium supplement material has a higher practical value.

[0055] In one embodiment, the crystallinity of the lithium supplement material ranges from 10% to 50%. That is, the crystallinity of the lithium supplement material is greater than 10% and less than 50%. Among them, the lower the crystallinity of the lithium supplement material, the lower the stability of the lithium supplement material. In the embodiment of the present application, the lower limit of the crystallinity of the lithium supplement material is restricted, so that the lithium supplement material not only has a lower delithiation voltage platform, but also has higher stability.

[0056] In one embodiment, the lithium de-lithiation voltage platform of the lithium supplement material with a crystallinity of less than 50% is lower than the lithium de-lithiation voltage platform of the lithium supplement material with a crystallinity of greater than 50%. For example, the lithium de-lithiation voltage platform of lithium oxalate with a crystallinity of less than 50% is lower than the lithium de-lithiation voltage platform of lithium oxalate with a crystallinity of greater than 50%. In the embodiment of the present application, the decrease in the crystallinity of the lithium supplement material directly reduces the lithium de-lithiation voltage platform of the lithium supplement material, which is conducive to reducing the difficulty of application of the lithium supplement material.

[0057] In one embodiment, the difference between the delithiation voltage platform of the lithium supplement material with a crystallinity of less than 50% and the delithiation voltage platform of the lithium supplement material with a crystallinity of greater than 98% is greater than 0.4V. Exemplarily, the delithiation voltage platform of the lithium supplement material with a crystallinity of greater than 98% is 4.7V (without catalyst), and when it contains a relevant catalyst, its delithiation potential is 4.46V, while when the crystallinity is reduced to 50%, the delithiation voltage platform of the lithium supplement material is 3.96V, and the delithiation voltage platform of the lithium supplement material is reduced by 0.48V (Note: For amorphous lithium oxalate, it contains the same catalyst as the above-mentioned crystalline lithium oxalate, which is convenient for comparison). In the embodiments of the present application, compared with commercially available materials, the present application reduces the crystallinity of the lithium supplement material to less than 50%, thereby greatly reducing the delithiation voltage platform of the lithium supplement material, so that the lithium supplement material has a higher practical value.

[0058] In one embodiment, the lithium-replenishing material has a lithium-removal platform potential of p and a crystallinity of c, and p and c have the following relationship: When 0<c<0.1, p=40c 2 -8c+4.32; when 0.1≤c≤0.2, p=12c 2 -4.8c+4.28; when 0.2<c<0.5, p=0.6c+3.68. It is worth noting that the relationship is summarized under the premise that the catalyst can play a catalytic role; when no catalyst is used at all, the influence of crystallinity on the delithiation platform potential plays a major role; when the catalyst can achieve normal catalysis, the influence of crystallinity can be approximately quantified according to the above relationship.

[0059] In one embodiment, the selected area electron diffraction of the lithium supplement material is ring-shaped and has a high degree of dispersion. Among them, the selected area electron diffraction of the lithium supplement material is ring-shaped, indicating that the lithium supplement material is amorphous. In this application, the amorphous lithium supplement material has a lower lithium desorption voltage platform, and the lithium ions in the lithium supplement material are easier to escape, which is conducive to reducing the difficulty of applying the lithium supplement material.

[0060] In one embodiment, the X-ray diffraction spectrum of the lithium supplement material includes a peak, and the half-peak width of the peak is greater than 2° and less than 10°. Among them, the X-ray diffraction spectrum of the lithium supplement material presents a large peak and no fine peak structure, indicating that the lithium supplement material is amorphous. In the present application, the lithium supplement material is amorphous, which reduces the lithium desorption voltage platform of the lithium supplement material.

[0061] In one embodiment, the 2θ angle corresponding to the envelope peak is 25°-43°. Among them, the 2θ angle of 33°-35° is the characteristic peak of the lithium supplement material crystal, and in the present application, the angle range of the envelope peak is 25°-43°, and the envelope peak covers the angle range of the crystal characteristic peak of 33°-35° and is larger than the angle range of the crystal characteristic peak, indicating that the lithium supplement material is in an amorphous state. Amorphous lithium supplement materials have a lower lithium desorption voltage platform.

[0062] In one embodiment, the diffraction peak area of ​​the lithium supplement material with a crystallinity of less than 50% at a 2θ angle of 25°-43° is 3-50 times the diffraction peak area of ​​the lithium supplement material with a crystallinity of greater than 98% at a 2θ angle of 33°-35°. The lithium supplement material provided in the present application has a larger diffraction peak area due to its lower crystallinity, which reduces the lithium de-lithiation voltage platform of the lithium supplement material.

[0063] In one embodiment, the lithium supplement additive further comprises a catalyst, and the lithium supplement material is in-situ grown on the outer surface of the catalyst. In the embodiment of the present application, the lithium supplement material is in close contact with the catalyst, which increases the contact area and contact stability between the lithium supplement material and the catalyst.

[0064] In one embodiment, during the preparation of the lithium supplement additive, the catalyst can be used to improve the stability of the lithium supplement material. Among them, compared with the lithium supplement material with higher crystallinity, the lithium supplement material in the present application has lower crystallinity, which reduces its stability. In the present application, the catalyst can be used to stabilize the lithium supplement material, avoid the lithium supplement material from transforming into a crystal, so that the lithium supplement material maintains a lower crystallinity during the long-term cycle, which is beneficial for the lithium supplement material to maintain a lower lithium de-lithiation voltage platform.

[0065] For example, the catalyst is Mo2C. Highly conductive Mo2C nanoparticles can easily capture CO2 and Li, promoting the reaction process to form unstable intermediate products Li2C2O4. 2-The free radicals can be connected to Mo2C by the Mo-O chemical bond through this metal-oxygen coupling. Due to the low valence state of Mo, the outer electrons (electron donors) of the highly conductive Mo2C can be transferred to the electronegative oxygen atoms (electron acceptors) in Li2C2O4, which increases the valence state of the Mo atoms and promotes the rapid stabilization of Li2C2O4 through delocalized electrons, while the electron transfer between Mo2C and Li2CO3 is not obvious.

[0066] In one embodiment, the catalyst includes at least one of NiO, MnO, CoO, Co3O4, Ti3C2, CoS, Co3S4, MoS2, and Ru. The above catalyst types can play a stabilizing effect or have a good stabilizing effect.

[0067] In one embodiment, the catalyst is also used to catalyze the decomposition of the lithium supplement material to reduce the lithium desorption potential platform of the lithium supplement material. In the present application, the catalyst not only has the function of stabilizing the structure of the lithium supplement material, but also has a catalytic effect, so that the lithium supplement material has higher stability and lower lithium desorption voltage platform.

[0068] It is understandable that in this application, the lithium-replenishing material is mainly reduced in crystallinity to reduce its lithium-replenishing voltage platform, and the role of the catalyst is mainly to stabilize the structure of the lithium-replenishing material. Even if the catalyst still has a catalytic effect, the amount of the catalyst is low and the catalytic effect of the catalyst is limited. If only the catalyst is used to reduce the lithium-replenishing material's lithium-replenishing voltage platform, the amount of the catalyst is large, which will affect the energy density of the lithium-replenishing additive, and the catalytic effect of the catalyst may also damage the electrode material, aluminum foil, etc.

[0069] In one embodiment, the catalyst includes at least one of Mo2C, Ti3C2, MnO, MnO2, NiO, CoO, Co3O4, Ru, RuO2, TiO2, MoS2, ZnS, CoS, CoS2, Co3S4, NiS2, FeS2, and ReS2. The above-mentioned types of catalysts can be used to prevent the lithium-supplementing material from transforming into a crystal, so that the lithium-supplementing material maintains a low crystallinity during long-term cycles, which is beneficial for the lithium-supplementing material to maintain a low delithiation voltage platform.

[0070] In particular, when the catalyst includes O or S atoms, there is an intermolecular force between the carbon atoms in the carbon dioxide and the oxygen or sulfur atoms in the catalyst. The LUMO energy level after the two are combined is lower than the original LUMO energy level, making it easier for reduction reactions to occur. The catalyst preferentially obtains electrons on the positive electrode material for conversion, and the converted mediator then reduces the carbon dioxide molecules. The reduction potential is higher than 2.8V, which hinders the growth of lithium carbonate and promotes the conversion of carbon dioxide to lithium oxalate.

[0071] In one embodiment, the lithium supplement additive also includes a conductive agent, which is grown in situ on the outer surface of the catalyst. The conductive agent has electrical conductivity. In the embodiment of the present application, the conductive agent can promote the transmission of electrons in the lithium supplement additive. The conductive agent can enhance the conductivity of the lithium supplement material and improve the electron transmission efficiency of the lithium supplement material, reduce the polarizability of the lithium supplement material and reduce the impedance of the lithium supplement additive, which is beneficial to improving the rate performance and cycle performance of the lithium supplement additive. The electronic conductive environment formed by the conductive agent is beneficial to the delithiation of the lithium supplement material. In addition, the conductive agent can act as a conductive bridge between the catalyst and the lithium supplement material, thereby improving the overall conductivity of the lithium supplement additive.

[0072] In one embodiment, the conductive agent includes at least one of carbon nanotubes, graphene, graphite, hard carbon, soft carbon, and carbon fiber.

[0073] In one embodiment, the mass ratio of lithium supplement material, catalyst and conductive agent is (70-95): (2-15): (3-15). The lithium supplement material accounts for 70%-95% of the mass of the lithium supplement additive. The catalyst accounts for 2%-15% of the mass of the lithium supplement additive. The mass fraction of the conductive agent is 3%-15%.

[0074] The relative contents of lithium supplement materials, catalysts and conductive agents affect the performance of lithium supplement additives. If the relative content of lithium supplement materials is high, the catalyst with a low content will not be able to stabilize the structure of the lithium supplement materials, and the conductive agent with a low content will not have a significant effect on improving the conductivity of the lithium supplement additive. If the relative content of lithium supplement materials is low, the lithium supplement effect of the lithium supplement materials is poor, and if the content of catalysts and conductive agents is too high, it will affect the energy density of the lithium supplement additive.

[0075] In the embodiment of the present application, by adjusting the mass ratio of the lithium replenishing material, the catalyst and the conductive agent to be in the range of (70-95):(2-15):(3-15), while maintaining a relatively high energy density, the lithium replenishing material can have a good lithium replenishing effect, the catalyst can better stabilize the structure of the lithium replenishing material, and the conductive environment formed by the conductive agent is more conducive to the delithiation of the lithium replenishing material.

[0076] In one embodiment, the mass ratio of the lithium supplement material, the catalyst and the conductive agent can be 95:2:3, 90:5:5, 90:7:3, 85:10:5, 85:5:10, 80:10:10, 80:5:15, 80:15:5, 75:10:15, 75:15:10 or 70:15:15.

[0077] In one embodiment, the lithium replenishing material accounts for 70%, 75%, 80%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% or 95% of the mass of the lithium replenishing additive.

[0078] In one embodiment, the catalyst accounts for 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15% of the mass of the lithium supplement additive.

[0079] In one embodiment, the mass fraction of the conductive agent is 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%.

[0080] In one embodiment, the particle size of the lithium supplement material is 5nm-400nm. The particle size of the lithium supplement material affects the performance of the lithium supplement additive. In the embodiment of the present application, the particle size of the lithium supplement material is controlled within the range of 5nm-400nm. The particle size of the lithium supplement material is small, which is conducive to the release of lithium ions in the lithium supplement material, so as to further reduce the lithium removal voltage platform of the lithium supplement material. It is also conducive to increasing the contact area between the lithium supplement material and the catalyst or conductive agent, which can effectively improve the stability and conductivity of the lithium supplement material.

[0081] In one embodiment, the particle size of the lithium supplementing material is 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm or 400 nm.

[0082] In one embodiment, the particle size of the catalyst is 5nm-150nm. In the embodiments of the present application, the particle size of the catalyst is kept within a suitable range, which helps the catalyst to better play the role of improving the stability of the lithium supplement material and is conducive to the preparation of the lithium supplement additive.

[0083] In one embodiment, the particle size of the conductive agent is 10nm-200nm. In the embodiment of the present application, the particle size of the conductive agent is kept within a suitable range, which helps the conductive agent to better play the role of improving the conductivity of the lithium supplement material and is conducive to the preparation of the lithium supplement additive.

[0084] The present application provides a method for preparing a lithium supplement additive, the method for preparing a lithium supplement additive comprises step S1, step S2, step S3 and step S4, and the specific steps are as follows:

[0085] Step S1, providing or preparing a cathode

[0086] Step S2, using lithium as the anode, assembling the anode and the cathode into a Li-CO2 battery;

[0087] Step S3, introducing CO2 and / or CO gas into the cathode of the Li-CO2 battery, and obtaining discharge products at the cathode after the Li-CO2 battery is discharged;

[0088] Step S4, collecting the discharge products and washing and drying the discharge products to obtain a lithium supplement additive.

[0089] The cut-off voltage of the Li-CO2 battery is 2V-2.5V, and the current density is 400mA / g-800mA / g. The crystallinity of the lithium supplement material in the lithium supplement additive is less than 50%.

[0090] The cathode of the Li-CO2 battery includes at least one of a carbon material, a metal and its metal oxide or carbide, and a metal organic framework compound. The separator may be a commercial glass fiber, and the electrolyte may be a 1M LiTFSI / DMSO (lithium bis(trifluoromethanesulfonyl)imide / dimethyl sulfoxide) organic electrolyte.

[0091] During the discharge process of Li-CO2 batteries, the lithium at the anode migrates to the cathode and reacts electrochemically with carbon dioxide and carbon monoxide to generate Li x C y O z Lithium-supplementing materials.

[0092] In the present application, the crystallinity of the lithium supplement material synthesized by electrochemical means is less than 50%, and the lithium supplement material with lower crystallinity can exist stably. When the lithium supplement material prepared in the present application is used as a positive electrode lithium supplement additive, due to the lower crystallinity of the lithium supplement material, its lithium desorption voltage platform is greatly reduced.

[0093] In one embodiment, the cathode includes at least one of a catalyst and a conductive agent. The catalyst and / or the conductive agent are added to the cathode so that the lithium supplement material can be deposited on the outer surface of the catalyst and / or the conductive agent through the discharge reaction of the Li-CO2 battery, and the obtained discharge product includes the lithium supplement material and the catalyst and / or the conductive agent, so that the lithium supplement material has excellent stability and higher electronic conductivity.

[0094] In one embodiment, the method for preparing a cathode includes step S1-1, step S1-2, step S1-3 and step S1-4, and the specific steps are as follows:

[0095] Step S1-1, adding a solvent to a catalyst source and a carbon source, and stirring to obtain a solution;

[0096] Step S1-2, placing the solution in an autoclave for hydrothermal reaction, washing, drying, and calcining to obtain a catalyst precursor;

[0097] Step S1-3, mixing the catalyst precursor and the conductive agent, and calcining them under an inert atmosphere to obtain a composite of the catalyst and the conductive agent;

[0098] Step S1-4, the composite material and the binder are mixed and sprayed onto carbon paper, and then dried to obtain a cathode.

[0099] The carbon source in step S1-1 is used to react with the catalyst source in step S1-2 to generate metal carbide. The composite of the catalyst and the conductive agent obtained in step S1-3 is bonded together by a binder, sprayed onto carbon paper and solidified to form a sheet-like cathode. The bonding effect of the binder is conducive to the stable connection of the catalyst and the conductive agent.

[0100] In the embodiment of the present application, the cathode of the Li-CO2 battery is composed of a catalyst and a conductive agent. After the Li-CO2 battery is discharged, the lithium replenishing material is deposited on the surface of the cathode. After the cathode of the Li-CO2 battery is washed and dried, a lithium replenishing additive composed of a lithium replenishing material, a composite conductive agent and a catalyst can be obtained.

[0101] The present application provides a positive electrode material, which includes a positive electrode active material and the lithium supplement additive as described above, or a positive electrode material which includes a positive electrode active material and the lithium supplement additive prepared by the preparation method of the lithium supplement additive as described above.

[0102] The present application provides a positive electrode plate, which includes the lithium supplement additive as described above, or includes the lithium supplement additive prepared by the preparation method of the lithium supplement additive as described above.

[0103] The present application provides a secondary battery, which includes a negative electrode material, a separator and a positive electrode material. The positive electrode material includes the lithium supplement additive as described above or includes the lithium supplement additive prepared by the preparation method of the lithium supplement additive as described above.

[0104] In order to illustrate the beneficial effects of the method of the present application, the present application also provides the following examples and comparative examples:

[0105] Example 1

[0106] Embodiment 1 provides a lithium supplement additive, which includes a lithium supplement material (lithium oxalate), a catalyst (Mo2C) and a conductive agent (carbon nanotubes). The crystallinity of lithium oxalate is 12%, and the mass ratio of lithium oxalate, Mo2C and carbon nanotubes is 90:5:5. The particle size of lithium oxalate is 100nm, the particle size of Mo2C is 10nm, and the diameter of carbon nanotubes is 30nm.

[0107] The preparation method of the lithium supplement additive comprises:

[0108] Step 1, add ammonium molybdate and glucose to a beaker at a mass ratio of 1:6, and then add pure water and ethylene glycol at a volume ratio of 1:2, and stir to obtain a colorless clear solution. The mixed solution is placed in an autoclave and hydrothermally reacted at 200°C for 10 hours. Then wash and freeze-dry. The freeze-dried material is placed in a quartz boat, and then placed in a tube furnace for high-temperature calcination. In a H2 / Ar (5%) atmosphere, the temperature is raised to 800°C at 10°C / min for 2 hours to obtain a Mo2C precursor. After that, CNT (carbon nanotube) is fully ground and coated with the Mo2C precursor and placed in a quartz boat. In a pure Ar atmosphere, the temperature is raised to 950°C at 10°C / min and calcined for 1 hour to obtain a composite of Mo2C and CNT, namely Mo2C / CNT powder.

[0109] Select carbon paper as the substrate, and use a button punch to cut out carbon paper with a diameter of 12 mm in advance. Then put the circular carbon paper (φ12×0.27mm) into an oven and dry it at 60°C for 12 hours. Put 0.25g PVDF into 10ml NMP and stir it thoroughly as a binder. Put 90wt% Mo2C / CNT powder and 10wt% 0.025g / mL PVDF / NMP binder solution into a mortar, grind it thoroughly for 1 hour, then put the mixed slurry into a spray brush, and use the spray brush to evenly spray the ground slurry on the circular carbon paper. Put the sprayed Mo2C / CNT cathode in a vacuum oven at 120°C and dry it for 12 hours to remove the residual solvent to obtain a Mo2C / CNT cathode.

[0110] Step 2: The embodiment of the present application uses a CR 2032 lithium-ion button battery case, and 13 small holes with a diameter of 1 mm are punched at the bottom of the battery case on the air electrode side to facilitate the contact and transmission of CO2 / CO gas.

[0111] Anode: Commercial lithium sheet is used.

[0112] Diaphragm: Commercial glass fiber (16 mm diameter).

[0113] Electrolyte: 10 ml of the electrolyte solvent DMSO was placed in a glass bottle, and 2.56 g of LiTFSI lithium salt was added to completely dissolve it to prepare a 1 M LiTFSI / DMSO organic electrolyte.

[0114] Air electrode: The air electrodes used are cathode electrode sheets prepared by the above method, with a diameter of 12 mm.

[0115] The anode and cathode are assembled into a Li-CO2 battery, and the assembly order is as follows: the battery porous shell, air electrode, glass fiber, lithium sheet (thickness 0.6mm), gasket, spring sheet and button battery shell cover are stacked in sequence from bottom to top.

[0116] Step 3, pure CO2 gas is introduced into the air electrode of the Li-CO2 battery assembled above, with a volume ratio of 1:1, the Li-CO2 battery is discharged, the cut-off voltage is 2V, the discharge current density is 500mA / g, and a discharge product is obtained at the cathode after discharge, and the discharge product contains amorphous lithium oxalate and carbon, both of which are attached to the Mo2C / CNT surface;

[0117] Step 4, disassembling the discharged battery, and washing and drying the cathode discharge product to obtain the required lithium supplement additive.

[0118] Example 2

[0119] Example 2 provides a lithium supplement additive, which is different from Example 1 in that the crystallinity of lithium oxalate in Example 2 is 45%.

[0120] The preparation steps of the lithium supplement additive in Example 2 are different from those in Example 1 in that the cut-off voltage of the Li-CO2 / CO battery in Step 2 of Example 2 is 2.3 V and the current density is 700 mA / g.

[0121] Example 3

[0122] Example 3 provides a lithium supplement additive, which is different from Example 1 in that the catalyst in Example 3 is changed from Mo2C to RuO2, and the other components remain unchanged, and the crystallinity of lithium oxalate is 15%.

[0123] Example 4

[0124] Example 4 provides a lithium supplement additive, which is different from Example 1 in that the gas introduced into the cathode is a mixed gas of 50% CO2 and 50% CO by volume, and the product contains amorphous lithium oxalate and carbon, and the crystallinity of the lithium oxalate is 20%.

[0125] Example 5

[0126] Example 5 provides a lithium supplement additive, which is different from Example 3 in that in Example 5, a mixed gas of 50% CO2 and 50% CO is introduced into the cathode, and the catalyst is pure RuO2 without CNT, and the discharge product includes amorphous lithium oxalate and carbon, the crystallinity of lithium oxalate is 25%, and the generated carbon replaces the CNT in Example 3 as a conductive carrier of the lithium supplement agent.

[0127] Example 6

[0128] Example 6 provides a lithium supplement additive, which is different from Example 3 in that the discharge current density in Example 6 is 800 mA / g, and the crystallinity of the corresponding product lithium oxalate is 50%.

[0129] The preparation steps of the lithium supplement additive in Example 6 are different from those in Example 1 in that the cut-off voltage of the Li-CO2 / CO battery in Step 2 of Example 6 is 2V and the current density is 800mA / g.

[0130] Example 7

[0131] Example 7 provides a lithium supplement, which is different from Example 1 in that the catalyst in Example 7 is ZnS, which can stabilize the amorphous lithium oxalate formed during the discharge process. The crystallinity of this lithium oxalate is 35%, but ZnS has no catalytic effect during the decomposition of lithium oxalate as a lithium supplement.

[0132] Comparative Example 1

[0133] Comparative Example 1 provides a lithium supplement additive. In Comparative Example 1, the lithium oxalate is commercially available lithium oxalate, the crystallinity of the commercially available lithium oxalate is 98%, and no catalyst or conductive agent is added.

[0134] Comparative Example 2

[0135] Comparative Example 2 provides a lithium supplement additive, which is different from Comparative Example 1 in that the lithium oxalate with a crystallinity of 98% in Comparative Example 2 is mixed and ground with the Mo2C / CNT prepared in Example 1 in the same ratio (90:5:5) when preparing the positive electrode lithium supplement agent electrode sheet.

[0136] Comparative Example 3

[0137] Comparative Example 3 provides a lithium supplement additive, which is different from Example 1 in that Zn / CNT used in Comparative Example 3 is used as a catalyst for the Li-CO2 / CO battery. During the discharge process, Zn cannot stabilize the intermediate product lithium oxalate, and the final product is lithium carbonate.

[0138] Comparative Example 4

[0139] Comparative Example 4 provides a lithium supplement additive, which is different from Example 3 in that the discharge current density in Comparative Example 4 is 1000 mA / g, and the crystallinity of the corresponding product, lithium oxalate, is 60%.

[0140] The difference between the preparation steps of the lithium supplement additive in Comparative Example 4 and that in Example 3 is that in step 2 of Comparative Example 4, the cut-off voltage of the Li-CO2 / CO battery is 2V and the current density is 1000mA / g.

[0141] The lithium supplement additives provided in the above examples and comparative examples are respectively assembled into positive electrode sheets and lithium ion batteries according to the following methods:

[0142] Positive electrode: The lithium supplement additive, polyvinylidene fluoride and SP-Li are mixed in a mass ratio of 80:8:12 by ball milling to obtain a positive electrode slurry, the positive electrode slurry is coated on the surface of aluminum foil, vacuum dried at 110°C overnight, and rolled to obtain a positive electrode sheet;

[0143] Negative electrode: Graphite, carboxymethyl cellulose (CMC), SBR and SP were mixed in a mass ratio of 95.8:1.2:2:1, and the mixture was ball-milled and stirred to obtain a negative electrode slurry. The negative electrode slurry was coated on the surface of copper foil, and vacuum dried at 110°C overnight to obtain a negative electrode sheet.

[0144] Electrolyte: The solvent is triethylene glycol dimethyl ether, and the solute is lithium bis(trifluoromethanesulfonyl imide) and lithium bis(fluorosulfonyl imide) (molar ratio is 2:3), and the electrolyte is formed according to a certain ratio;

[0145] Diaphragm: Polypropylene microporous separator;

[0146] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of graphite negative electrode sheet - separator - electrolyte - positive electrode sheet.

[0147] Related performance tests

[0148] Electrochemical performance test:

[0149] The electrochemical performance of each lithium ion battery assembled in the above lithium ion battery embodiment was tested as shown in Table 1, and the test conditions were as follows:

[0150] Constant current and constant voltage charging, the first cycle charge and discharge voltage is 2.0-4.7V, the current is 0.1C, and the cut-off current is 0.01C.

[0151] X-ray diffraction test:

[0152] A copper target is used, and the wavelength is The tube voltage and tube current are 40kV and 40mA respectively, and the angle range is

[0153] 10°-80°. Preparation before testing: Put the sample into the groove on the glass plate, fix it, and clamp the glass table with the sample on the instrument for testing.

[0154] The relevant performance test results are shown in Table 1 below:

[0155] Table 1 Performance test results

[0156]

[0157] By comparing Example 1, Example 2 and Comparative Example 1, Comparative Example 2, Figure 1 and Figure 2It can be seen that when the crystallinity of lithium oxalate in the present application is 10%-50%, the delithiation potential of lithium oxalate in the present application is 3.88V (such as Figure 2 Its delithiation potential is significantly lower than that of commercial lithium oxalate (4.70 V) and commercial lithium oxalate with Mo2C / CNT added (as shown in Figure 1 This is because the amorphization of lithium oxalate is beneficial to reducing its delithiation energy barrier, thereby reducing the delithiation potential.

[0158] Figure 3 A in FIG. 1 represents an amorphous lithium oxalate layer. Figure 3 It can be seen that the amorphous discharge product lithium oxalate in Example 1 evenly and completely covers the surface of Mo2C particles and carbon nanotubes.

[0159] from Figure 4 It can be seen that the discharge product of Example 5 adheres to the cathode surface to form an amorphous film.

[0160] By comparing Examples 1 to 3, 6 to 7 with Comparative Example 3, it can be found that the catalyst has a significant effect on the final product during the discharge process of the battery. The catalysts of Examples 1 to 3, 6 to 7 can all stabilize the lithium oxalate formed during the discharge process and maintain its amorphous state. However, the catalyst Zn in Comparative Example 3 cannot play such a role, resulting in the final product being lithium carbonate, which is more difficult to decompose. Therefore, its delithiation potential is very high (4.40 V) and its capacity is difficult to exert (346 mAh / g).

[0161] By comparing Examples 1 to 7 with Comparative Example 4, it can be found that even if they are all amorphous lithium oxalate, the crystallinity of lithium oxalate has a significant effect on the final delithiation potential. Under the premise that the catalyst and the conductive agent remain unchanged, the crystallinity is 20%, and its delithiation potential is the lowest. When the crystallinity is greater than 20%, the delithiation potential increases with the increase of crystallinity. When the crystallinity is less than 20%, the delithiation potential increases with the decrease of crystallinity. Of course, the delithiation potential is also affected by the catalyst and the conductive agent.

[0162] By comparing Example 1 and Example 4, it can be found that the gases introduced in the two experiments are different. The gas introduced in Example 4 contains CO, and amorphous carbon is newly generated during the discharge process. The generation of amorphous carbon makes lithium oxalate in a more complete conductive network, so its delithiation potential is lower than that of Example 3. Of course, since Example 4 introduces more carbon (inactive material), its charge capacity is slightly lower than that of Example 3.

[0163] The lithium supplement additive, preparation method thereof and secondary battery provided in the embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and embodiments of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for general technicians in this field, according to the idea of ​​the present application, there will be changes in the specific embodiments and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A lithium supplement additive, characterized in that: The lithium supplement additive includes a lithium supplement material, the general chemical formula of which is Li x C y O z , wherein 1<x<3, 0<y<8, 1<z<10, the crystallinity of the lithium-supplementing material is less than 50%, and the delithiation voltage platform of the lithium-supplementing material is lower than 4V.

2. The lithium supplement additive according to claim 1, characterized in that The crystallinity of the lithium supplementing material is in the range of 10%-50%; and / or The lithium supplement material includes at least one of Li2C2O4, Li2CO3, Li2C4O4, Li2C3O5, Li2C4O6, and Li2C6O6.

3. The lithium supplement additive according to claim 1, characterized in that The difference between the delithiation voltage platform of the lithium supplement material having a crystallinity of less than 50% and the delithiation voltage platform of the lithium supplement material having a crystallinity of greater than 98% is greater than 0.4 V; and / or The lithium-replenishing material has a delithiation platform potential of p and a crystallinity of c, and p and c have the following relationship: when 0<c<0.1, p=40c 2 -8c+4.32; when 0.1≤c≤0.2, p=12c 2 -4.8c+4.28; when 0.2<c<0.5, p=0.6c+3.

68.

4. The lithium supplement additive according to claim 1, characterized in that The X-ray diffraction pattern of the lithium supplementing material includes a peak, and the half-peak width of the peak is in the range of 2°-10°; and / or The 2θ angle of the maximum peak intensity corresponding to the envelope peak is 34°, and the angle range of the envelope peak is 25°-43°; and / or The diffraction peak area of ​​the lithium supplement material with a crystallinity of less than 50% at a 2θ angle of 25°-43° is 3-50 times that of the diffraction peak area of ​​the lithium supplement material with a crystallinity of more than 98% at a 2θ angle of 33°-35°.

5. The lithium supplement additive according to claim 1, characterized in that The lithium supplement additive further includes a catalyst, and the lithium supplement material is in-situ grown on the outer surface of the catalyst; and / or The lithium supplement additive further includes a conductive agent, which is in-situ grown on the outer surface of the catalyst.

6. The lithium supplement additive according to claim 5, characterized in that The catalyst comprises at least one of Mo2C, Ti3C2, MnO, MnO2, NiO, CoO, Co3O4, Ru, RuO2, TiO2, MoS2, ZnS, CoS, CoS2, Co3S4, NiS2, FeS2, and ReS2; and / or The catalyst is used for catalyzing the decomposition of the lithium-supplementing material to reduce the delithiation potential platform of the lithium-supplementing material.

7. The lithium supplement additive according to claim 5, characterized in that The mass ratio of the lithium supplement material, the catalyst and the conductive agent is (70-95): (2-15): (3-15); and / or The particle size of the lithium supplement material is 5nm-400nm; and / or The particle size of the catalyst is 5nm-150nm; and / or The particle size of the conductive agent is 10nm-200nm.

8. A method for preparing a lithium supplement additive, characterized in that: The preparation method of the lithium supplement additive comprises: providing or preparing a cathode; Using lithium as an anode, assembling the anode and the cathode into a Li-CO2 battery; introducing CO2 and / or CO gas into the cathode of the Li-CO2 battery, and obtaining discharge products at the cathode after the Li-CO2 battery is discharged; collecting the discharge products and washing and drying the discharge products to obtain the lithium supplement additive; The cut-off voltage of the Li-CO2 battery is 2V-2.5V, the discharge current density is 400mA / g-800mA / g, and the crystallinity of the lithium-supplementing material in the lithium-supplementing additive is less than 50%.

9. The method for preparing the lithium additive according to claim 8, characterized in that: The cathode includes at least one of a catalyst and a conductive agent: and / or The preparation method of the cathode includes: adding a solvent to a catalyst source and a carbon source, stirring to obtain a solution; placing the solution in an autoclave for hydrothermal reaction, washing, drying, and calcining to obtain a catalyst precursor; mixing the catalyst precursor with a conductive agent, and calcining under an inert atmosphere to obtain a composite of the catalyst and the conductive agent; mixing the composite with a binder and spraying it onto carbon paper, and drying to obtain the cathode.

10. A secondary battery, characterized in that: The secondary battery comprises a negative electrode material, a separator and a positive electrode material, wherein the positive electrode material comprises the lithium supplement additive according to any one of claims 1 to 7 or the lithium supplement additive prepared by the preparation method of the lithium supplement additive according to any one of claims 8 to 9.