Positive electrode additive and preparation method and application thereof
By preparing plate-like cathode additives and composite cathode materials using active ionic salts with low relative crystallinity, the problems of first-time irreversible capacity loss and cycle performance degradation in lithium-ion batteries have been solved. This has enabled safe and efficient replenishment of active ions, improving the electrochemical performance and lifespan of electrochemical devices.
Patent Information
- Application Number
- CN202310573250.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
Existing lithium-ion batteries suffer from irreversible capacity loss and cycle performance degradation during the first charge-discharge cycle due to the formation of the SEI film on the negative electrode. Furthermore, existing methods for replenishing lithium on the positive electrode pose safety risks and present harsh processing conditions.
Using active ionic salts with low relative crystallinity as positive electrode additives, sheet-like positive electrode additives and composite positive electrode materials are prepared by freeze-drying. These are coated on the surface of the positive electrode active material to form a core-shell structure, which decomposes at a lower potential to generate active ions and replenish the active ions in the electrochemical device.
It improves the initial charge-discharge specific capacity and cycle performance of lithium-ion batteries, reduces the decomposition voltage, enhances safety and adaptability to processing environments, and extends the service life of electrochemical devices.
Smart Images

Figure CN119008944A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy technology, and in particular to a positive electrode additive and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have been widely used in consumer electronics and electric vehicle products due to their high energy efficiency, environmental friendliness, and high energy density, and have attracted much attention as a key technology for large-scale energy storage systems. Lithium-ion batteries include relatively arranged positive and negative electrodes. During the first charge and discharge process, lithium ions will form a passivation film, namely, SEI film, on the surface of the negative electrode, thereby causing the first irreversible capacity loss of the lithium-ion battery and reducing the first charge and discharge specific capacity and cycle performance of the lithium-ion battery. In order to compensate for the loss of active lithium caused by the formation of SEI film on the negative electrode during the first charge and discharge process of the lithium-ion battery, and to improve the first charge and discharge specific capacity and cycle performance of the lithium-ion battery, it is necessary to replenish lithium for the lithium-ion battery. However, the existing methods for replenishing lithium for the negative electrode have high safety risks and are very demanding on the processing environment. Summary of the invention
[0003] The embodiment of the present application provides a positive electrode additive, which can be used to safely and efficiently replenish active ions in an electrochemical device, thereby improving the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0004] The embodiment of the present application provides a method for preparing the above-mentioned positive electrode additive, which has a simple process and is suitable for wide promotion and application.
[0005] An embodiment of the present application provides a composite positive electrode material, which, when used in an electrochemical device, can improve the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0006] The embodiment of the present application provides a method for preparing a composite positive electrode material, which is used to prepare the above-mentioned composite positive electrode material. The preparation method has a simple preparation process and helps to save manufacturing costs.
[0007] An embodiment of the present application provides a positive electrode sheet, comprising the above-mentioned positive electrode additive and / or the above-mentioned composite positive electrode material. When the positive electrode sheet is used in an electrochemical device, it helps to improve the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0008] An embodiment of the present application provides an electrochemical device, which includes the above-mentioned positive electrode sheet, so the electrochemical device has excellent initial charge and discharge specific capacity and cycle performance.
[0009] An embodiment of the present application provides an electronic device, which includes the above-mentioned electrochemical device, so the electronic device has excellent initial charge and discharge specific capacity and service life, and excellent user experience.
[0010] The present application provides a positive electrode additive, wherein the positive electrode additive is an active ion salt with a relative crystallinity of 0-95%.
[0011] The positive electrode additive as described above, wherein the positive electrode additive is a sheet structure formed by a first nano-active ion salt;
[0012] The size of the first nano-active ion salt is less than 150 nm;
[0013] The size of the positive electrode additive is less than 10 μm.
[0014] The present application provides a method for preparing the positive electrode additive as described above, which comprises: performing a first freeze-drying treatment on a first raw material system including the active ion salt raw material to obtain the positive electrode additive.
[0015] In the method for preparing the positive electrode additive as described above, the first raw material system further includes a surfactant.
[0016] The method for preparing the positive electrode additive as described above, wherein the mass ratio of the active ion salt raw material to the surfactant is (100-1000):1; and / or,
[0017] In the first freeze-drying process, the temperature is -100 to -50°C and the time is 2 to 6 hours.
[0018] The present application provides a composite positive electrode material, wherein the composite positive electrode material comprises a core and a coating layer coated on at least a portion of the surface of the core;
[0019] The core includes a positive electrode active material, and the coating layer includes an active ion salt;
[0020] The relative crystallinity of the coating layer is 0-95%.
[0021] The composite positive electrode material as described above, wherein the coating layer comprises a first coating layer;
[0022] The first coating layer includes a second nanometer active ion salt, and the size of the second nanometer active ion salt is 1 nm-20 μm.
[0023] The composite positive electrode material as described above, wherein the positive electrode active material is a polycrystalline positive electrode active material, and the coating layer further comprises a second coating layer, and the second coating layer is coated on at least a portion of the surface of the inner core and / or the first coating layer;
[0024] The second coating layer includes a third nanometer active ion salt, and the size of the third nanometer active ion salt is 1-500 nm.
[0025] The composite positive electrode material as described above, wherein the size of the positive electrode active material is 0.5-100 μm.
[0026] The composite positive electrode material as described above, wherein in the composite positive electrode material, the mass ratio of the core to the coating layer is 1:(0.005-0.5).
[0027] The present application provides a method for preparing the composite positive electrode material as described above, which comprises: performing a second freeze-drying treatment on a second raw material system comprising the positive electrode active material and an active ion salt raw material to obtain the composite positive electrode material;
[0028] The positive electrode active material forms a core, and the active ion salt raw material forms a coating layer that covers at least a portion of the surface of the core.
[0029] In the method for preparing the composite positive electrode material as described above, the second raw material system further includes a surfactant.
[0030] The method for preparing the positive electrode additive as described above, wherein the mass ratio of the total mass of the active ion salt raw material and the positive electrode active material to the surfactant is (100-1000): 1; and / or,
[0031] In the second freeze-drying treatment, the temperature is -100 to -50°C and the time is 2 to 6 hours.
[0032] The present application provides a positive electrode sheet, which includes the positive electrode additive as described above, and / or the composite positive electrode material as described above.
[0033] The positive electrode sheet as described above, wherein the mass percentage of the positive electrode additive in the positive electrode active layer of the positive electrode sheet is ≤10%.
[0034] The present application provides an electrochemical device, which includes the positive electrode sheet as described above.
[0035] The present application provides an electronic device, wherein a driving source or an energy storage source of the electronic device includes the electrochemical device as described above.
[0036] The positive electrode additive provided in the embodiment of the present application has a low relative crystallinity. When the positive electrode additive is applied to an electrochemical device, it can be decomposed at a low potential to generate active ions, replenish active ions for the electrochemical device, and improve the initial charge and discharge specific capacity and cycle performance of the electrochemical device. Moreover, the positive electrode additive is safe and efficient when used to replenish active ions for the electrochemical device.
[0037] The preparation method of the positive electrode additive provided in the embodiment of the present application can prepare the above-mentioned positive electrode additive. The preparation method also has the advantage of simple process, which is conducive to wide promotion and application.
[0038] The composite positive electrode material provided in the embodiment of the present application has a coating layer with a low relative crystallinity. When the composite positive electrode material is used in an electrochemical device, the coating layer can be decomposed at a low potential to generate active ions, thereby replenishing the active ions for the electrochemical device and improving the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0039] The method for preparing the composite positive electrode material provided in the embodiment of the present application is used to prepare the above-mentioned composite positive electrode material. The preparation method has a simple process and low manufacturing cost.
[0040] The positive electrode sheet provided in the embodiment of the present application, including the above-mentioned positive electrode additive and / or composite positive electrode material, when used in an electrochemical device, can improve the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0041] The electrochemical device provided in the embodiment of the present application has an excellent initial charge and discharge specific capacity while having a long service life due to the use of the aforementioned positive electrode sheet.
[0042] The electronic device provided in the embodiment of the present application is driven or stores energy through the aforementioned electrochemical device, so it has excellent service life and first charge and discharge specific capacity, and provides an excellent user experience. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 is a schematic diagram of the structure of the positive electrode additive in some embodiments of the present application;
[0044] Figure 2 is a schematic diagram of the structure of a composite positive electrode material in some embodiments of the present application;
[0045] Figure 3 is a schematic diagram of the structure of the composite positive electrode material in other embodiments of the present application;
[0046] Figure 4 is a SEM image of the positive electrode additive A in Example 1a of the present application at a magnification;
[0047] Figure 5 is a SEM image of the positive electrode additive A in Example 1a of the present application at another magnification;
[0048] Figure 6 is the XRD pattern of the positive electrode additive A in Example 1a of the present application;
[0049] Figure 7 is a SEM image of the positive electrode additive B in Example 2a of the present application;
[0050] Figure 8 is a SEM image of the positive electrode additive C in Example 3a of the present application;
[0051] Fig. 9 is a SEM image of the positive electrode additive D in Example 4a of the present application;
[0052] Fig.10 is a SEM image of the composite positive electrode material A1 in Example 1b of the present application;
[0053] Fig.11 It is the XRD diagram of the composite positive electrode material in Examples 1b and 2b of the present application and the positive electrode active material in Comparative Example 1;
[0054] Fig.12 is a SEM image of the composite positive electrode material A2 in Example 2b of the present application;
[0055] Fig.13 is a SEM image of the composite positive electrode material A3 in Example 3b of the present application;
[0056] Fig.14 is a SEM image of the composite positive electrode material B1 in Example 4b of the present application;
[0057] Fig.15 is a SEM image of the composite positive electrode material B2 in Example 5b of the present application;
[0058] Fig.16 is a SEM image of the composite positive electrode material C1 in Example 6b of the present application;
[0059] Fig.17 is a SEM image of the composite positive electrode material C2 in Example 7b of the present application;
[0060] Fig.18 is a SEM image of the composite positive electrode material D1 in Example 8b of the present application;
[0061] Fig.19 is a SEM image of the composite positive electrode material D2 in Example 9b of the present application;
[0062] Fig. 20is a SEM image of the positive electrode additive a in Comparative Example 5 of the present application;
[0063] Fig.21 This is a SEM image of the positive electrode additive b in Comparative Example 6 of the present application;
[0064] Fig. 22 is a SEM image of the positive electrode additive c in Comparative Example 7 of the present application;
[0065] Fig.23 is a SEM image of the positive electrode additive d in Comparative Example 8 of the present application;
[0066] Fig.24 This is the first charging curve of the positive electrode additive A of Example 1a of the present application.
[0067] Description of reference numerals:
[0068] 1: Composite cathode material;
[0069] 11: cathode additives;
[0070] 12: kernel;
[0071] 111: the first nano-active ion salt;
[0072] 112: second nano-active ion salt;
[0073] 113: The third nano-active ion salt. DETAILED DESCRIPTION
[0074] The terms used in the implementation method part of this application are only used to explain the specific embodiments of this application, and are not intended to limit this application. The implementation method of the embodiments of this application will be described in detail below with reference to the accompanying drawings.
[0075] Since lithium replenishment for negative electrode sheets has a high safety risk and has very demanding requirements on the processing environment, the current main method is to replenish lithium for positive electrode sheets to improve the overall performance of lithium-ion batteries.
[0076] For example, the paper "A high-energy-density and long-life initial anode-free lithium battery enabled by a Li2O sacrificial agent, DOI: 10.1038 / s41560-021-00839-0" introduces the method of ball milling to coat the Li2O lithium supplement agent on the LiNi 0.8 Co 0.1 Mn 0.1O2 (NCM) ternary positive electrode active material surface, thereby achieving lithium replenishment of the positive electrode sheet. However, Li2O lithium replenisher is unstable in the air and easily reacts with water and CO2. The lithium replenisher is also easy to react with the electrolyte to produce gas, which is not conducive to the cycle performance and safety performance of the battery; and because the lithium replenisher is highly alkaline, it is easy to make the positive electrode active slurry jelly in the process of preparing the positive electrode active slurry, which is not conducive to the preparation of the positive electrode sheet.
[0077] CN114497553A discloses a positive electrode additive, which includes a specific content of a conductive catalyst molybdenum sulfide and a gas-generating lithium-rich material. Although the positive electrode additive can achieve safe and efficient lithium replenishment for lithium-ion batteries to a certain extent, its decomposition voltage is relatively high, reaching about 4.5V, and its lithium replenishment effect is limited; and molybdenum sulfide will reduce the energy density of the battery and catalyze the decomposition of the electrolyte, which is not conducive to the cycle performance and safety performance of the battery.
[0078] From the above, it can be seen that in the existing methods for replenishing lithium for positive electrode sheets, on the one hand, in the process of preparing the positive electrode active slurry, the positive electrode lithium replenishing material will form jelly, which is not conducive to the coating of the positive electrode active slurry; on the other hand, during the cycle of the lithium-ion battery, the positive electrode lithium replenishing material is easy to react with the electrolyte to produce gas, affecting the cycle performance and safety performance of the lithium-ion battery.
[0079] Based on the above-mentioned defects, a first aspect of an embodiment of the present application provides a positive electrode additive, which is an active ion salt with a relative crystallinity of 0-95%.
[0080] In the present application, the relative crystallinity can be understood as the degree of amorphism. The relative crystallinity of the present application is obtained by performing an XRD test on the positive electrode additive and calculating it. The relative crystallinity is equal to the relative area of the crystalline peak in the XRD spectrum × 100% / (relative area of the crystalline peak + relative area of the amorphous peak), wherein the sum of the relative area of the crystalline peak and the relative area of the amorphous peak is the total peak area of the positive electrode additive excluding the impurity peak. In some embodiments, the positive electrode additive can be subjected to an XRD test to obtain the XRD spectrum of the positive electrode additive, and then the diffraction peak with a half-width (FWHM) greater than 3° in the XRD spectrum is calibrated as an amorphous peak (amorphous peak), and the data is imported into the fitting software Jade, and the diffraction peaks within the test range are fitted with the entire spectrum, and the pseudo-Voigt function is used to describe the diffraction peaks; for phases with PDF, PDF is directly used for fitting; if not, a straight line background is used to find the peak and fit it. Finally, the integral area value (peak area) of the crystalline peak and the integral area value of the amorphous peak are obtained to calculate the crystallinity. For example, the relative crystallinity of the cathode additive of the present application can be 5%, 10%, 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 85%.
[0081] Active ion salt refers to a salt that can provide active ions. In the present application, the active ions can be specifically selected according to the actual application, and the active ions can be lithium ions, sodium ions, potassium ions or calcium ions; correspondingly, the active ion salt can be a lithium salt, a sodium salt, a potassium salt, a magnesium salt or a calcium salt. Exemplarily, when the positive electrode additive is applied to a lithium ion battery, the active ion can be a lithium ion, and the active ion salt can be a lithium salt.
[0082] In some embodiments, the active ion salt may be an organic salt, and the organic salt may be selected from at least one of carbonate, oxalate, acetate, squarate, citrate, tartrate, ketomalonate and succinate.
[0083] Since the positive electrode additive of the present application is an active ion salt with low relative crystallinity, when applied to an electrochemical device, the positive electrode additive can be decomposed at a lower potential to produce active ions (for example, lithium ions, sodium ions, potassium ions or calcium ions), thereby replenishing the active ions consumed by the electrochemical device during the first charge and discharge and subsequent cycles, and improving the first charge and discharge specific capacity and cycle performance of the electrochemical device. And the positive electrode additive also has the advantages of safety and efficiency when used to replenish active ions in an electrochemical device.
[0084] It is understandable that the lower the relative crystallinity of the positive electrode additive, the higher its decomposition voltage, and the more conducive it is to safely and efficiently replenish active ions for the electrochemical device. However, in practical applications, it is difficult to make the relative crystallinity of the positive electrode additive infinitely low. Therefore, in order to further simplify the preparation process and improve the efficiency of the positive electrode additive in replenishing active ions, the relative crystallinity of the positive electrode additive can be 5-85%.
[0085] In the present application, in order to improve the efficiency of replenishing active ions of the positive electrode additive and improve the initial charge and discharge specific capacity and cycle performance of the electrochemical device, the microscopic morphology of the positive electrode additive may also be specifically selected. Figure 1 Schematic diagram of the structure of the composite positive electrode material in some embodiments of the present application. Figure 1 As shown, in some embodiments of the present application, the positive electrode additive 11 is a sheet structure formed by a first nano-active ion salt 111;
[0086] The size of the first nano-active ion salt 111 is less than 150 nm;
[0087] The size of the positive electrode additive 11 is less than 10 μm.
[0088] Exemplarily, the size of the first nano-active ion salt 111 can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm or 140nm; the size of the positive electrode additive 11 can be 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm or 9μm.
[0089] In the present application, the difference between the first nano-active ion salt 111 and the active ion salt is only the difference in microscopic morphology. It can be understood that in some embodiments, the positive electrode additive 11 is an active ion salt formed by the agglomeration of the first nano-active ion salt 111 with a size of less than 150nm, and the active ion salt is a sheet structure with a size of less than 10μm. The size of the first nano-active ion salt 111 refers to the average particle size of the first nano-active ion salt 111. In some embodiments, multiple particle sizes of the first nano-active ion salt 111 in different directions can be obtained respectively, and their average values can be calculated; the size of the positive electrode additive 11 refers to the average length of the sheet structure. In some embodiments, such as Figure 1 As shown, the sizes of the sheet structure in different directions can be obtained respectively and the average value can be calculated. In some embodiments of the present application, the positive electrode additive 11 can be subjected to SEM testing to obtain a SEM image of the positive electrode additive 11, and the size of the positive electrode additive and the size of the first nano-active ion salt 111 can be obtained based on the SEM image of the positive electrode additive 11.
[0090] The positive electrode additive 11 of the present application has the above-mentioned microscopic morphology, which can further reduce the relative crystallinity of the positive electrode additive 11, thereby reducing the decomposition overpotential of the positive electrode additive 11 and improving the active ion replenishment effect of the positive electrode additive 11; and in the charge and discharge cycle of the electrochemical device, the positive electrode additive 11 with a special microscopic morphology can shorten the transmission path of the active ions, improve the transmission efficiency of the active ions, further reduce the overpotential of the active ions to escape, and improve the active ion replenishment effect.
[0091] A second aspect of an embodiment of the present application provides a method for preparing the positive electrode additive of the first aspect, comprising: performing a first freeze-drying treatment on a first raw material system including an active ion salt raw material to obtain the positive electrode additive.
[0092] In the present application, the active ion salt raw material can form an active ion salt (positive electrode additive) with a relative crystallinity of 0-95%. For example, the active ion salt raw material can be an active ion salt (with high relative crystallinity) sold on the market.
[0093] The present application performs a first freeze-drying treatment on the first raw material system including the active ion salt raw material, which can reduce the relative crystallinity of the active ion salt raw material, thereby obtaining a positive electrode additive with low relative crystallinity. The preparation method of the present application is simple to operate and suitable for wide promotion and application.
[0094] In some embodiments of the present application, when the first raw material system further includes a surfactant, the relative crystallinity of the active ion raw material can be further reduced, thereby quickly obtaining a positive electrode additive with low relative crystallinity.
[0095] Furthermore, the surfactant may be hexadecyltrimethylammonium bromide.
[0096] The present application may further select the mass ratio of the active ion salt raw material to the surfactant and the process parameters of the first freeze-drying treatment in order to obtain a positive electrode additive with excellent performance.
[0097] In some embodiments of the present application, the mass ratio of the active ion salt raw material to the surfactant is (100-1000): 1; and / or,
[0098] In the first freeze-drying process, the temperature is -100 to 50°C and the time is 2 to 6 hours.
[0099] Further, the mass ratio of the active ion salt raw material to the surfactant is 500:1;
[0100] In the first freeze-drying treatment, the temperature was -80°C and the time was 3 hours.
[0101] Figure 2is a schematic diagram of the structure of a composite positive electrode material in some embodiments of the present application; Figure 3 Schematic diagram of the structure of composite positive electrode materials in other embodiments of the present application. Figure 2 or Figure 3 As shown, a third aspect of the embodiment of the present application provides a composite positive electrode material 1, the composite positive electrode material 1 includes a core 12 and a coating layer coated on at least a portion of the surface of the core 12;
[0102] The core 12 includes a positive electrode active material, and the coating layer includes an active ion salt;
[0103] The relative crystallinity of the coating layer is 0-95%.
[0104] It can be understood that the coating layer can cover at least a portion of the surface of the core 12, or can cover the entire surface of the core 12. The coating layer can be continuous or discontinuous; and the coating layer can be a single layer or multiple layers.
[0105] The composite positive electrode material 1 of the present application is a core-shell structure, which includes a core 12 and a coating layer from the inside to the outside. In some embodiments, the composite positive electrode material may include a positive electrode active material and an active ion salt with low relative crystallinity from the inside to the outside.
[0106] The present application does not specifically limit the positive electrode active material, which can be a commonly used positive electrode active material in the art. The positive electrode active material can be a lithium ion battery positive electrode active material, a sodium ion battery positive electrode active material, a potassium ion battery positive electrode active material, a magnesium ion battery positive electrode active material or a calcium ion battery positive electrode active material. Exemplarily, the positive electrode active material of the lithium ion battery can be selected from at least one of lithium cobalt oxide, nickel cobalt manganese ternary material, nickel cobalt aluminum ternary material, lithium manganate and lithium iron phosphate; the positive electrode active material of the sodium ion battery can be selected from at least one of layered transition metal oxides, polyanionic compounds and Prussian blue and its analogs; the positive electrode active material of the potassium ion battery can be selected from at least one of polyanionic compounds and Prussian blue and its analogs; the positive electrode active material of the magnesium ion battery can be selected from at least one of Prussian blue and its analogs and Chevrel phase Mo6S8 materials; the positive electrode active material of the calcium ion battery can be selected from at least one of Prussian blue and its analogs, V2O5, CaCo2O4, α-MoO3 and heterocyclic organic compounds.
[0107] In some embodiments, when the positive electrode active material is a lithium ion battery active material, the active ion salt of the coating layer is a lithium salt; when the positive electrode active material is a sodium ion battery active material, the active ion salt of the coating layer is a sodium salt; when the positive electrode active material is a potassium ion battery active material, the active ion salt of the coating layer is a potassium salt; when the positive electrode active material is a magnesium ion battery active material, the active ion salt of the coating layer is a magnesium salt; when the positive electrode active material is a calcium ion battery active material, the active ion salt of the coating layer is a calcium salt.
[0108] In the composite positive electrode material in the embodiment of the present application, the core 12 can provide a growth substrate for the active ion salt in the coating layer, and can catalyze the decomposition of the active ion salt in the coating layer, reduce the decomposition voltage of the active ion salt, and effectively improve the supplement effect of the active ions. And because the relative crystallinity of the coating layer is low, when the composite positive electrode material is applied to an electrochemical device, the coating layer can be decomposed at a lower potential to generate active ions, thereby supplementing the active ions for the electrochemical device and improving the first discharge specific capacity and cycle performance of the electrochemical device.
[0109] like Figure 2 As shown, in some embodiments of the present application, the coating layer includes a first coating layer;
[0110] The first coating layer includes a second nanometer active ion salt 112 , and the size of the second nanometer active ion salt 112 is 1 nm-20 μm.
[0111] In the present application, the second nanometer active ion salt 112 is different from the first nanometer active ion salt 111 and the active ion salt only in the microscopic morphology. It is understood that in some embodiments of the present application, the composite positive electrode material includes a core 12 and a first coating layer including a second nanometer active ion salt 112 with a size of 1nm-20μm coated on at least a portion of the surface of the core 12.
[0112] In the present application, the size of the second nanometer active ion salt 112 refers to the average particle size of the second nanometer active ion salt 112. In some embodiments, multiple particle sizes of the second nanometer active ion salt 112 in different directions can be obtained respectively, and the average value thereof can be calculated. In some embodiments of the present application, a SEM test can be performed on the composite positive electrode material to obtain a SEM image of the composite positive electrode material 1, and the size of the second nanometer active ion salt 112 in the composite positive electrode material can be obtained based on the SEM image of the composite positive electrode material 1.
[0113] In the present application, the second nanometer active ion salt 112 of a special size can shorten the transmission path of active ions during the charge and discharge process of the electrochemical device, improve the transmission efficiency of active ions, reduce the overpotential of active ion escape, and improve the replenishment effect of active ions. In addition, the first coating layer formed by the second nanometer active ion salt 112 of a special size can be in closer contact with the core, so that the core 12 can catalyze the decomposition of the first coating layer, thereby improving the replenishment effect of active ions.
[0114] In practical applications, the size of the second nano-active ion salt 112 can be further selected according to the type of positive electrode active material, in order to further improve the supplement effect of active ions and improve the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0115] When the positive electrode active material is a single crystal positive electrode active material, the size of the second nanometer active ion salt 112 may be 1 nm-10 μm. Further, the size of the second nanometer active ion salt 112 may be 20-200 nm. Exemplarily, the size of the second nanometer active ion salt 112 may be 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0116] When the positive electrode active material is a polycrystalline positive electrode active material, the size of the second nano-active ion salt 112 can be 1nm-10μm. Further, the size of the second nano-active ion salt 112 can be 200-900nm. Exemplarily, the size of the second nano-active ion salt 112 can be 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm or 900nm.
[0117] like Figure 2 As shown, in some embodiments of the present application, the positive electrode active material is a polycrystalline positive electrode active material, and the coating layer further includes a second coating layer, which is coated on at least a portion of the surface of the core 12 and / or the first coating layer;
[0118] The second coating layer includes a third nanometer active ion salt 113 , and the size of the third nanometer active ion salt 113 is 1-500 nm.
[0119] In the present application, the third nanometer active ion salt 113 is different from the first nanometer active ion salt 111, the second nanometer active ion salt 112 and the active ion salt only in the microscopic morphology. When the positive electrode active material is a polycrystalline positive electrode active material, the coating layer also includes a second coating layer, and the second coating layer can only be coated on at least part of the surface of the core 12, or only on at least part of the surface of the first coating layer, or can be coated on at least part of the surface of the core 12 and at least part of the surface of the first coating layer at the same time.
[0120] When the composite positive electrode material 1 also includes a second coating layer, during the charge and discharge process of the electrochemical device, the second coating layer can produce more active ions, further replenishing the active ions for the electrochemical device; and because the size of the third nano-active ion salt 113 in the second coating layer is 1-500nm, the transmission distance of the active ions can be shortened, and the decomposition performance of the composite positive electrode material can be improved; at the same time, the second coating layer including the third nano-active ion salt 113 of a special size can be in close contact with the first coating layer and / or the inner core 12, promoting the catalytic decomposition of the first coating layer and / or the second coating layer by the inner core 12.
[0121] Furthermore, the particle size of the third nano-active ion salt 113 may be 5-50 nm.
[0122] The composite positive electrode material of the present application includes a core having a positive electrode active material and a coating layer covering at least a portion of the surface of the core. Therefore, the performance of the positive electrode active material, the content of the core and the coating layer will have a crucial impact on the performance of the composite positive electrode material.
[0123] Therefore, the present application can further select the particle size of the positive electrode active material in order to further improve the comprehensive performance of the composite positive electrode material. In some embodiments of the present application, the size of the positive electrode active material is 0.5-100 μm.
[0124] In the present application, the size of the positive electrode active material refers to the average particle size of the positive electrode active material. For example, the size of the positive electrode active material can be 0.5 μm, 1 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm.
[0125] When the particle size of the positive electrode active material meets the above range, the positive electrode active material can better provide a growth base for the coating layer, so that the positive electrode active material and the coating layer are more closely combined, catalyzing the decomposition of the coating layer, reducing the decomposition voltage, and effectively improving the replenishment effect of active ions.
[0126] In some embodiments of the present application, the mass ratio of the core and the coating layer can be further selected to further improve the comprehensive performance of the composite positive electrode material. In some embodiments of the present application, in the composite positive electrode material, the mass ratio of the core and the coating layer is 1: (0.005-0.5).
[0127] The fourth aspect of the present application provides a method for preparing the composite positive electrode material of the third aspect, comprising: subjecting a second raw material system including a positive electrode active material and an active ion salt raw material to a second freeze-drying treatment to obtain a composite positive electrode material;
[0128] The positive electrode active material forms a core, and the active ion salt raw material forms a coating layer that covers at least a portion of the surface of the core.
[0129] Specifically, a second raw material system including a positive electrode active material and an active ion salt raw material is subjected to a second freeze-drying treatment, so that the positive electrode active material forms an inner core, and the active ion salt raw material forms a coating layer with a relative crystallinity of 0-95% that is coated on at least part of the surface of the inner core, thereby obtaining the composite positive electrode material of the present application. The preparation method of the composite positive electrode material of the present application has a simple process and low manufacturing cost.
[0130] In some embodiments of the present application, when the second raw material system further includes a surfactant, the relative crystallinity of the active ion raw material can be further reduced, thereby quickly obtaining a positive electrode additive with low relative crystallinity. The surfactant can be hexadecyltrimethylammonium bromide.
[0131] The present application may further select the mass ratio of the total mass of the active ion salt raw material and the positive electrode active material to the mass ratio of the surfactant and the process parameters of the second freeze-drying treatment in order to obtain a positive electrode additive with excellent performance.
[0132] In some embodiments of the present application, the mass ratio of the total mass of the active ion salt raw material and the positive electrode active material to the surfactant is (100-1000): 1; and / or,
[0133] In the second freeze-drying process, the temperature is -100 to 50°C and the time is 2 to 6 hours.
[0134] A fifth aspect of an embodiment of the present application provides a positive electrode sheet, comprising the positive electrode additive of the first aspect of the present application, and / or the composite positive electrode material of the third aspect of the present application.
[0135] Exemplarily, the positive electrode additive, the positive electrode active material, the conductive agent and the binder can be mixed to form a positive electrode active slurry, the positive electrode active slurry is disposed on at least one surface of the positive electrode collector, and the positive electrode sheet including the positive electrode active layer is obtained after drying; the composite positive electrode material, the conductive agent and the binder can be mixed to form a positive electrode active slurry, the positive electrode active slurry is disposed on at least one surface of the positive electrode collector, and the positive electrode sheet including the positive electrode active layer is obtained after drying; the positive electrode additive, the composite positive electrode active material, the conductive agent and the binder can be mixed to form a positive electrode active slurry, the positive electrode active slurry is disposed on at least one surface of the positive electrode collector, and the positive electrode sheet including the positive electrode active layer is obtained after drying.
[0136] Since the positive electrode sheet of the present application includes the positive electrode additive of the first aspect and / or the composite positive electrode material of the third aspect, the positive electrode sheet has an excellent active ion replenishing effect and can improve the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0137] In some embodiments of the present application, when the positive electrode sheet contains a positive electrode additive, the mass percentage of the positive electrode additive in the positive electrode active layer of the positive electrode sheet is ≤10%, which can save the positive electrode additive and fully replenish the active ions of the positive electrode sheet, thereby improving the initial charge and discharge specific capacity and cycle performance of the electrochemical device.
[0138] A sixth aspect of an embodiment of the present application provides an electrochemical device, comprising the positive electrode sheet of the fifth aspect.
[0139] The present application does not specifically limit the electrochemical device. The electrochemical device may be a secondary battery, and the secondary battery may be, for example, a lithium-ion battery or a sodium-ion battery.
[0140] In addition to the positive electrode sheet, the secondary battery of the embodiment of the present application also includes a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte.
[0141] Secondary batteries mainly rely on the reversible insertion and extraction of active ions (for example, lithium ions, sodium ions or potassium ions) to provide energy, so the amount of active ions directly restricts the initial charge and discharge specific capacity of the secondary battery, and the continuous loss of active ions during the cycle will also lead to the decay of the cycle life of the secondary battery. The secondary battery in the embodiment of the present application, because it includes the positive electrode sheet of the fifth aspect, can replenish the active ions consumed during the charge and discharge process during the charge and discharge cycle, which can effectively improve the initial charge and discharge specific capacity and cycle life of the secondary battery, especially the initial charge and discharge specific capacity and cycle life of the secondary battery including the negative electrode sheet containing at least one of silicon, hard carbon, phosphorus and tin.
[0142] Taking a lithium-ion secondary battery including a silicon-based negative electrode sheet as an example, the theoretical capacity of a silicon-based negative electrode sheet can be as high as 4200mAh / g, but the silicon-based material will consume a portion of active lithium ions during the first charging process, and the SEI film that is repeatedly broken and reorganized during the charge and discharge cycle will also consume a portion of active lithium ions. Therefore, the first charge and discharge specific capacity and cycle life of this type of secondary battery are poor. The secondary battery in the embodiment of the present application, because it includes the fifth aspect positive electrode sheet, can replenish the lithium active ions consumed during the charge and discharge process during the charge and discharge cycle of the secondary battery, which can effectively improve the first charge and discharge specific capacity and cycle life of the secondary battery.
[0143] A seventh aspect of the present application provides an electronic device, wherein a driving source or an energy storage source of the electronic device includes the electrochemical device of the sixth aspect.
[0144] Among them, electronic devices may include but are not limited to consumer products, vehicles, communication equipment, base stations, etc. Specifically, they may be mobile phones, tablet computers, laptops, ultra-mobile personal computers (ultra-mobile personal computers, UMPCs), handheld computers, walkie-talkies, netbooks, POS machines, personal digital assistants (personal digital assistants, PDAs), wearable devices, virtual reality equipment, base station power supplies, energy storage power stations, new energy vehicles, trams, high-speed rail emergency power supplies, UPS power supplies, flexible wearable devices, and other mobile or fixed terminals with batteries.
[0145] In some embodiments, the electronic device further comprises an electrical component, and the electrochemical device is used to provide power to the electrical component. It is understood that the electronic device may further comprise a housing, and the electrical component and the electrochemical device are located in the housing.
[0146] The electronic device of the embodiment of the present application uses the aforementioned electrochemical device as a driving source or energy storage unit, and therefore has an excellent service life and high user satisfaction.
[0147] The following is a detailed introduction to the embodiments of the present application through specific examples.
[0148] Example 1a
[0149] The positive electrode additive A of this embodiment is prepared by a method comprising the following steps:
[0150] Lithium oxalate was dissolved in water, and then a certain amount of N-methylpyrrolidone (NMP) and hexadecyltrimethylammonium bromide were added, stirred for 10 minutes, and then freeze-dried to obtain a positive electrode additive A;
[0151] Wherein, the mass ratio of lithium oxalate to hexadecyltrimethylammonium bromide is 1000:2;
[0152] The freeze-drying process was carried out at -80°C for 3 hours.
[0153] The positive electrode additive A is subjected to a SEM test to obtain a SEM image of the positive electrode additive A. Figure 4 is a SEM image of the positive electrode additive A in Example 1a of the present application at a magnification; Figure 5 is a SEM image of the positive electrode additive A in Example 1a of the present application at another magnification, from Figure 4 and Figure 5 It can be seen that the positive electrode additive A in Example 1a of the present application is a 2 μm flake structure, and the positive electrode additive A is agglomerated from nano lithium oxalate with a particle size of less than 100 nm;
[0154] An XRD test is performed on the positive electrode additive A to obtain an XRD graph of the positive electrode additive A. Figure 6 is the XRD pattern of the positive electrode additive A in Example 1a of the present application, according to Figure 6 The relative crystallinity of the positive electrode additive A was calculated. After calculation, the relative crystallinity of the positive electrode additive A in Example 1a of the present application was 80%.
[0155] The positive electrode additive A is prepared into a button cell, specifically comprising the following:
[0156] The positive electrode additives A, SP, and PVDF were mixed evenly in a ratio of 8:1:1 and dispersed in an NMP solution to form a slurry. The slurry was coated on the surface of an aluminum foil with a thickness of 9 μm, dried, compacted by a roller press, and then cut into original sheets with a diameter of 13 mm. Lithium metal sheets were used as the negative electrode, and button batteries (charging cut-off voltage was 5 V) were made in a glove box with a diaphragm and an electrolyte.
[0157] The positive electrode additive A is prepared into a full battery, specifically including the following:
[0158] The positive electrode additive A, PVDF particles, SP and CNTs are weighed in a ratio of 94:2:3:1. PVDF is first dissolved in NMP solvent to make a glue, and then CNTs are added and dispersed evenly, and then SP and positive electrode additive A are added at the same time. After uniform dispersion, the viscosity is adjusted to be within the range of 3000-8000mPa.s, and the fineness is less than 25μm before the material is discharged, filtered, coated, dried, rolled, and die-cut to make a pole piece;
[0159] The negative electrode is matched with a silicon-graphite negative electrode (the capacity of the button battery is 500mAh / g, and the first efficiency is 83%), and an electrolyte of 1mol / LLiPF6 is used. The solvent in the electrolyte includes EC and DEC with a volume ratio of 1:1. A PP-PE-PP separator is used to make a 2270mAh soft-pack battery. The soft-pack battery is subjected to a formation treatment. A large amount of gas will be generated in the formation stage. The generated gas can be discharged in the exhaust process, and the battery can be sealed after the air bag is cut off.
[0160] Example 2a
[0161] The preparation method of the positive electrode additive B in this embodiment is basically the same as the preparation method of the positive electrode additive A in Example 1a, except that lithium oxalate is replaced by lithium carbonate to obtain the positive electrode additive B.
[0162] The positive electrode additive B is subjected to a SEM test to obtain a SEM image of the positive electrode additive B. Figure 7 is a SEM image of the positive electrode additive B in Example 2a of the present application. Figure 7It can be seen that the positive electrode additive B in Example 2a of the present application is a 4 μm flake structure, and the positive electrode additive B is agglomerated by nano lithium carbonate with a particle size of less than 300 nm;
[0163] An XRD test is performed on the positive electrode additive B to obtain the XRD graph of the positive electrode additive B. The relative crystallinity of the positive electrode additive B is calculated based on the XRD graph of the positive electrode additive B. After calculation, the relative crystallinity of the positive electrode additive B in Example 2a of the present application is 80%.
[0164] The positive electrode additive A in Example 1a was replaced with the positive electrode additive B to obtain a button cell.
[0165] The positive electrode additive A in Example 1a was replaced with the positive electrode additive B to obtain a full battery.
[0166] Example 3a
[0167] The preparation method of the positive electrode additive C of this embodiment is basically the same as the preparation method of the positive electrode additive A in Example 1a, except that lithium oxalate is replaced by sodium oxalate to obtain the positive electrode additive C.
[0168] The positive electrode additive C is subjected to a SEM test to obtain a SEM image of the positive electrode additive C. Figure 8 is a SEM image of the positive electrode additive C in Example 3a of the present application. Figure 8 It can be seen that the positive electrode additive C in Example 3a of the present application is a 4 μm flake structure, and the positive electrode additive C is agglomerated by nano sodium oxalate with a particle size of less than 200 nm;
[0169] An XRD test was performed on the positive electrode additive C to obtain the XRD graph of the positive electrode additive C. The relative crystallinity of the positive electrode additive C was calculated based on the XRD graph of the positive electrode additive C. After calculation, the relative crystallinity of the positive electrode additive C in Example 3a of the present application was 85%.
[0170] The positive electrode additive A in Example 1a was replaced with the positive electrode additive C, and the lithium metal sheet was replaced with a sodium metal sheet to obtain a button cell (with a charge cutoff voltage of 4.5 V).
[0171] Example 4a
[0172] The preparation method of the positive electrode additive D in this embodiment is basically the same as the preparation method of the positive electrode additive C in Example 1c, except that lithium oxalate is replaced by sodium carbonate to obtain the positive electrode additive D.
[0173] The positive electrode additive D is subjected to a SEM test to obtain a SEM image of the positive electrode additive D. Fig. 9 is a SEM image of the positive electrode additive D in Example 4a of the present application. Fig. 9It can be seen that the positive electrode additive D in Example 4a of the present application is a 6 μm flake structure, and the positive electrode additive D is agglomerated by nano sodium carbonate with a particle size of less than 200 nm;
[0174] An XRD test was performed on the positive electrode additive D to obtain the XRD graph of the positive electrode additive D. The relative crystallinity of the positive electrode additive D was calculated based on the XRD graph of the positive electrode additive D. After calculation, the relative crystallinity of the positive electrode additive D in Example 4a of the present application was 82%.
[0175] The positive electrode additive C in Example 1c was replaced with the positive electrode additive D to obtain a button cell.
[0176] Example 1b
[0177] The composite positive electrode material A1 of this embodiment is prepared by a method comprising the following steps:
[0178] Lithium oxalate is dissolved in water, and then added to a mixed solution of a certain amount of N-methylpyrrolidone (NMP), hexadecyltrimethylammonium bromide and 8-series single crystal NCM positive electrode material, stirred for 10 minutes, and freeze-dried to obtain a composite positive electrode material A1, wherein the single crystal NCM forms an inner core, and lithium oxalate forms a coating layer covering at least a portion of the surface of the inner core;
[0179] Among them, the mass ratio of single crystal NCM to lithium oxalate is 97:3 (in the composite positive electrode material, the mass percentage of the coating layer is 3%);
[0180] The mass ratio of the total mass of lithium oxalate and single crystal NCM to the mass of hexadecyltrimethylammonium bromide is 1000:2;
[0181] The freeze-drying process was carried out at -80°C for 3 hours.
[0182] The composite positive electrode material A1 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material A1. Fig.10 is a SEM image of the composite positive electrode material A1 in Example 1b of the present application. Fig.10 It can be seen that the composite positive electrode material A1 in Example 1b of the present application includes a core and a coating layer, and the coating layer includes nano lithium oxalate with a particle size of less than 100 nm;
[0183] An XRD test is performed on the composite positive electrode material A1 to obtain an XRD graph of the composite positive electrode material A1. Fig.11 It is the XRD diagram of the composite positive electrode material in Examples 1b and 2b of the present application and the positive electrode active material in Comparative Example 1. According to the XRD diagram of the composite positive electrode material A1, the relative crystallinity of lithium oxalate (coating layer) in the composite positive electrode material A1 is calculated to be 75%.
[0184] The preparation method of the button cell of this embodiment is basically the same as the preparation method of the button cell in Example 1a, except that the positive electrode additive A in Example 1a is replaced by the composite positive electrode material A1, and the cut-off voltage of the button cell is 4.25V.
[0185] The preparation method of the full battery in this embodiment is basically the same as the preparation method of the full battery in Example 1a, except that the positive electrode additive A in Example 1a is replaced by the composite positive electrode material A1. After the soft-pack battery is formed, the residue of the composite positive electrode material is NCM particles, and the particle size (the particle size of the inner core) is 50nm-20μm.
[0186] Example 2b
[0187] The preparation method of the composite positive electrode material A2 of this embodiment is basically the same as that of embodiment 1b, except that the ratio of the single crystal NCM to the positive electrode additive A is 98:2.
[0188] The composite positive electrode material A2 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material A2. Fig.12 This is a SEM image of the composite positive electrode material A2 in Example 2b of the present application. It can be seen that Fig.12 The morphology of the composite cathode material Fig.10 The morphology of the composite cathode material is similar. Fig.12 It can be seen that the composite positive electrode material A2 in Example 2b of the present application includes a core and a coating layer, and the coating layer includes nano lithium oxalate with a particle size of less than 100 nm;
[0189] Perform XRD test on the composite positive electrode material A2 to obtain the XRD pattern of the composite positive electrode material A2, such as Fig.11 According to the XRD pattern of the composite positive electrode material A2, the relative crystallinity of lithium oxalate in the composite positive electrode material A2 is calculated to be 69%.
[0190] The preparation method of the button cell of this embodiment is substantially the same as the preparation method of the button cell in Embodiment 1b, except that the composite positive electrode material A1 in Embodiment 1b is replaced by the composite positive electrode material A2.
[0191] The preparation method of the full battery of this embodiment is basically the same as the preparation method of the full battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material A2.
[0192] Example 3b
[0193] The preparation method of the composite positive electrode material A3 of this embodiment is substantially the same as that of embodiment 1b, except that 8-series polycrystalline NCM is used to replace 8-series single-crystalline NCM.
[0194] The composite positive electrode material A3 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material A3. Fig.13 is a SEM image of the composite positive electrode material A3 in Example 3b of the present application. Fig.13 It can be seen that the composite positive electrode material A3 in Example 3b of the present application includes a core and a coating layer, the coating layer includes a first coating layer and a second coating layer coated on the surface of the first coating layer and the core, the first coating layer includes nano-lithium oxalate with a particle size of 500 nm, and the second coating layer includes nano-lithium oxalate with a particle size of 20 nm;
[0195] The composite positive electrode material A3 is subjected to an XRD test to obtain an XRD graph of the composite positive electrode material A3. According to the XRD graph of the composite positive electrode material A3, the relative crystallinity of lithium oxalate in the composite positive electrode material A3 is calculated to be 78%.
[0196] The preparation method of the button cell of this embodiment is substantially the same as the preparation method of the button cell in Embodiment 1b, except that the composite positive electrode material A1 in Embodiment 1b is replaced by the composite positive electrode material A3.
[0197] The preparation method of the full battery of this embodiment is basically the same as the preparation method of the full battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material A3.
[0198] Example 4b
[0199] The preparation method of the composite positive electrode material B1 of this embodiment is basically the same as that of embodiment 1b, except that the positive electrode additive B is used to replace the positive electrode additive A.
[0200] The composite positive electrode material B1 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material B1. Fig.14 is a SEM image of the composite positive electrode material B1 in Example 4b of the present application. Fig.14 It can be seen that the composite positive electrode material B1 in Example 4b of the present application includes a core and a coating layer, and the coating layer includes nano lithium carbonate with a particle size of 200-300 nm;
[0201] The composite positive electrode material B1 was subjected to an XRD test to obtain an XRD graph of the composite positive electrode material B1. According to the XRD graph of the composite positive electrode material B1, the relative crystallinity of the lithium carbonate in the composite positive electrode material B1 was calculated to be 79%.
[0202] The preparation method of the button cell of this embodiment is substantially the same as the preparation method of the button cell in Embodiment 1b, except that the composite positive electrode material A1 in Embodiment 1b is replaced by the composite positive electrode material B1.
[0203] The preparation method of the full battery of this embodiment is basically the same as the preparation method of the full battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material B1.
[0204] Example 5b
[0205] The preparation method of the composite positive electrode material B2 of this embodiment is basically the same as that of embodiment 4b, except that 8-series polycrystalline NCM is used to replace 8-series single-crystalline NCM.
[0206] The composite positive electrode material B2 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material B2. Fig.15 is a SEM image of the composite positive electrode material B2 in Example 5b of the present application. Fig.15 It can be seen that the composite positive electrode material B2 in Example 5b of the present application includes a core and a coating layer, and the coating layer includes nano lithium carbonate with a particle size of 300 nm;
[0207] The composite positive electrode material B2 was subjected to an XRD test to obtain an XRD graph of the composite positive electrode material B2. According to the XRD graph of the composite positive electrode material B2, the relative crystallinity of the lithium carbonate in the composite positive electrode material B2 was calculated to be 79%.
[0208] The preparation method of the button battery in this embodiment is basically the same as the preparation method of the button battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material B2. The test results are shown in Table 1.
[0209] The preparation method of the full battery of this embodiment is basically the same as the preparation method of the full battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material B2.
[0210] Example 6b
[0211] The preparation method of the composite positive electrode material C1 of this embodiment is substantially the same as that of embodiment 1b, except that the positive electrode additive C is used to replace the positive electrode additive A, and the single crystal Prussian blue is used to replace the single crystal NCM.
[0212] The composite positive electrode material C1 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material C1. Fig.16 is a SEM image of the composite positive electrode material C1 in Example 6b of the present application. Fig.16 It can be seen that the composite positive electrode material C1 in Example 6b of the present application includes a core and a coating layer, and the coating layer includes nano sodium oxalate with a particle size of 300 nm;
[0213] The composite positive electrode material C1 is subjected to an XRD test to obtain an XRD graph of the composite positive electrode material C1. According to the XRD graph of the composite positive electrode material C1, it is calculated that the relative crystallinity of sodium oxalate in the composite positive electrode material C1 is 75%.
[0214] The preparation method of the button battery in this embodiment is basically the same as the preparation method of the button battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material C1, and the lithium metal sheet is replaced by the sodium metal sheet, and the charging cut-off voltage of the button battery is 4.2V.
[0215] Example 7b
[0216] The preparation method of the composite positive electrode material C2 of this embodiment is basically the same as that of embodiment 7b, except that: the layered oxide NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 replaces single crystal Prussian blue.
[0217] The composite positive electrode material C2 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material C2. Fig.17 is a SEM image of the composite positive electrode material C2 in Example 7b of the present application. Fig.17 It can be seen that the composite positive electrode material C2 in Example 7b of the present application includes a core and a coating layer, and the coating layer includes nano sodium oxalate with a particle size of 400 nm;
[0218] The composite positive electrode material C2 is subjected to an XRD test to obtain an XRD graph of the composite positive electrode material C2. According to the XRD graph of the composite positive electrode material C2, the relative crystallinity of the sodium oxalate in the composite positive electrode material C2 is calculated to be 79%.
[0219] The preparation method of the button-type battery in this embodiment is basically the same as the preparation method of the button-type battery in Example 6b, except that the composite positive electrode material C1 in Example 6b is replaced by the composite positive electrode material C2.
[0220] Example 8b
[0221] The preparation method of the composite positive electrode material D1 of this embodiment is basically the same as that of embodiment 6b, except that the positive electrode additive D is used to replace the positive electrode additive C.
[0222] The composite positive electrode material D1 was subjected to SEM testing to obtain a SEM image of the composite positive electrode material D1. Fig.18 is a SEM image of the composite positive electrode material D1 in Example 8b of the present application. Fig.18 It can be seen that the composite positive electrode material D1 in Example 8b of the present application includes a core and a coating layer, and the coating layer includes nano sodium carbonate with a particle size of 300 nm;
[0223] The composite positive electrode material D1 is subjected to an XRD test to obtain an XRD graph of the composite positive electrode material D1. According to the XRD graph of the composite positive electrode material D1, the relative crystallinity of the sodium carbonate in the composite positive electrode material D1 is calculated to be 74%.
[0224] The preparation method of the button cell of this embodiment is basically the same as the preparation method of the button cell in Embodiment 6b, except that the composite positive electrode material C1 in Embodiment 6b is replaced by the composite positive electrode material D1.
[0225] Example 9b
[0226] The preparation method of the composite positive electrode material D2 of this embodiment is basically the same as that of embodiment 7b, except that the positive electrode additive D is used to replace the positive electrode additive C.
[0227] The composite positive electrode material D2 is subjected to SEM testing to obtain a SEM image of the composite positive electrode material D2. Fig.19 is a SEM image of the composite positive electrode material D2 in Example 9b of the present application. Fig.19 It can be seen that the composite positive electrode material D2 in Example 9b of the present application includes a core and a coating layer, and the coating layer includes nano sodium carbonate with a particle size of 600 nm;
[0228] The composite positive electrode material D2 is subjected to an XRD test to obtain an XRD graph of the composite positive electrode material D2. According to the XRD graph of the composite positive electrode material D2, the relative crystallinity of the sodium carbonate in the composite positive electrode material D2 is calculated to be 74%.
[0229] The preparation method of the button type battery in this embodiment is basically the same as the preparation method of the button type battery in Example 7b, except that the composite positive electrode material C2 in Example 7b is replaced by the composite positive electrode material D2.
[0230] Example 10b
[0231] The preparation method of the button cell of this embodiment is basically the same as that of embodiment 1b, except that:
[0232] The composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material A4;
[0233] The composite positive electrode material A4 is prepared by a method comprising the following steps:
[0234] The positive electrode additive A and the 8-series single crystal NCM were physically mixed in a mass ratio of 97:3, and then ground in a mortar for 10 minutes to make them uniformly mixed, thereby obtaining a composite positive electrode material A4.
[0235] The preparation method of the full battery of this embodiment is basically the same as the preparation method of the full battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by the composite positive electrode material A4.
[0236] Comparative Example 1
[0237] The preparation method of the button cell of this comparative example is basically the same as the preparation method of the button cell in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by 8-series single crystal NCM.
[0238] The preparation method of the full battery of this comparative example is basically the same as the preparation method of the full battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by 8-series single crystal NCM.
[0239] Comparative Example 2
[0240] The preparation method of the button cell of this comparative example is basically the same as the preparation method of the button cell in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by 8-series polycrystalline NCM.
[0241] The preparation method of the full battery of this comparative example is basically the same as the preparation method of the full battery in Example 1b, except that the composite positive electrode material A1 in Example 1b is replaced by 8-series polycrystalline NCM.
[0242] Comparative Example 3
[0243] The preparation method of the button cell of this comparative example is basically the same as the preparation method of the button cell in Example 6b, except that the composite positive electrode material C1 in Example 6b is replaced by single crystal Prussian blue.
[0244] Comparative Example 4
[0245] The preparation method of the button cell of this comparative example is basically the same as that of the button cell of Example 6b, except that the composite positive electrode material C1 in Example 6b is replaced by the layered oxide NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
[0246] Comparative Example 5
[0247] In this comparative example, commercial lithium oxalate is used as the positive electrode additive a, and a SEM test is performed on the positive electrode additive a to obtain a SEM image of the positive electrode additive a. Fig. 20 This is a SEM image of the positive electrode additive a in Comparative Example 5 of the present application. Fig. 20 It can be seen that the positive electrode additive a in Comparative Example 5 of the present application is a particle of 30 μm.
[0248] An XRD test is performed on the positive electrode additive a to obtain the XRD graph of the positive electrode additive a. The relative crystallinity of the positive electrode additive a is calculated according to the XRD graph of the positive electrode additive a. After calculation, the relative crystallinity of the positive electrode additive a in Comparative Example 5 of the present application is 97%.
[0249] The preparation method of the button cell of this comparative example is basically the same as the preparation method of the button cell in Example 1a, except that the positive electrode additive A in Example 1a is replaced by positive electrode additive a.
[0250] The preparation method of the full battery of this comparative example is basically the same as the preparation method of the full battery in Example 1a, except that the positive electrode additive A in Example 1a is replaced by positive electrode additive a.
[0251] Comparative Example 6
[0252] In this comparative example, commercial lithium carbonate is used as the positive electrode additive b, and a SEM test is performed on the positive electrode additive b to obtain a SEM image of the positive electrode additive b. Fig.21 This is the SEM image of the positive electrode additive b in Comparative Example 6 of the present application. Fig.21 It can be seen that the particle size of the positive electrode additive b in Comparative Example 6 of the present application is 5-30 μm;
[0253] An XRD test is performed on the positive electrode additive b to obtain the XRD graph of the positive electrode additive b. The relative crystallinity of the positive electrode additive b is calculated according to the XRD graph of the positive electrode additive b. After calculation, the relative crystallinity of the positive electrode additive b in Comparative Example 6 of the present application is 98%.
[0254] The preparation method of the button cell of this comparative example is substantially the same as the preparation method of the button cell in Example 1a, except that the positive electrode additive A in Example 1a is replaced by the positive electrode additive b.
[0255] The preparation method of the full battery of this comparative example is basically the same as the preparation method of the full battery in Example 1a, except that the positive electrode additive A in Example 1a is replaced by the positive electrode additive b.
[0256] Comparative Example 7
[0257] In this comparative example, commercial sodium oxalate is used as the positive electrode additive c, and a SEM test is performed on the positive electrode additive c to obtain a SEM image of the positive electrode additive c. Fig. 22 This is a SEM image of the positive electrode additive c in Comparative Example 7 of the present application. Fig. 22 It can be seen that the positive electrode additive c in Comparative Example 7 of the present application is a large particle of 100 microns;
[0258] An XRD test is performed on the positive electrode additive c to obtain the XRD graph of the positive electrode additive c. The relative crystallinity of the positive electrode additive c is calculated according to the XRD graph of the positive electrode additive c. After calculation, the relative crystallinity of the positive electrode additive c in Comparative Example 7 of the present application is 97%.
[0259] The preparation method of the button cell of this comparative example is basically the same as the preparation method of the button cell in Example 3a, except that the positive electrode additive C in Example 3a is replaced by the positive electrode additive c.
[0260] Comparative Example 8
[0261] In this comparative example, commercial sodium carbonate is used as the positive electrode additive d, and a SEM test is performed on the positive electrode additive d to obtain a SEM image of the positive electrode additive d. Fig.23 This is a SEM image of the positive electrode additive d in Comparative Example 8 of the present application. Fig.23 It can be seen that the positive electrode additive d in Comparative Example 8 of the present application is a large particle larger than 100 microns;
[0262] An XRD test was performed on the positive electrode additive d to obtain the XRD graph of the positive electrode additive d. The relative crystallinity of the positive electrode additive d was calculated according to the XRD graph of the positive electrode additive d. After calculation, the relative crystallinity of the positive electrode additive c in Comparative Example 8 of the present application was 98%.
[0263] The preparation method of the button cell of this comparative example is basically the same as the preparation method of the button cell in Example 3a, except that the positive electrode additive C in Example 3a is replaced by the positive electrode additive d.
[0264] Performance Testing
[0265] 1. The button batteries in the embodiment and the comparative example were subjected to charge and discharge tests to obtain the first charge curve, the first charge specific capacity and the first discharge specific capacity, respectively, and the first charge voltage platform was obtained according to the first charge curve. The test results are shown in Table 1.
[0266] The test method of the first charge-discharge specific capacity is as follows: the battery is tested on a charge-discharge tester, the battery is set to a charging state (i.e., positive electrode desalination), the charging current density is 0.1C, and the charging is stopped when the corresponding charging cut-off voltage is reached, and the first charge specific capacity is calculated; after the above-mentioned first desalination is completed, the battery is set to a discharge state (i.e., positive electrode salt embedding), the discharge current density is 0.1C, and the discharge is stopped when the discharge reaches the cut-off voltage of 3V, and the first discharge specific capacity is calculated;
[0267] Among them, the first charge specific capacity (mAh / g) = the first desalination capacity / the mass of the sample to be tested; the first discharge specific capacity (mAh / g) = the first salt embedding capacity / the mass of the sample to be tested, and the sample to be tested is a positive electrode additive (Examples 1a-4a, Comparative Examples 5-8), a composite positive electrode material (Examples 1b-9b) or a positive electrode active substance (Example 19b, Comparative Examples 1-4).
[0268] Fig.24 This is the first charging curve of the positive electrode additive A of Example 1a of the present application, from Fig.24 It can be seen that the first charging voltage platform of the positive electrode additive A in Example 1a is 4.65V.
[0269] 2. The full batteries of Examples 1b-9b and Comparative Examples 1-4 were subjected to cycle performance tests. The test results are shown in Table 1:
[0270] The cycle performance test method is: the prepared full battery (soft pack battery) is subjected to a 1C charge / 1C discharge cycle test on a test machine, and the first discharge capacity is recorded as C1. If the discharge capacity during the cycle is less than 80% C1, the test is stopped. The number of cycles between C1 and 80% C1 is the cycle life of the battery cell.
[0271] The volume expansion test method is as follows: adjust the prepared soft-pack battery to 50% SOC state, then take points at a total of 5 points at the four corners and the center of the battery cell, measure its thickness and take the average value as the initial thickness of the battery cell and record it as D1. After the battery cell is cycled to 500 cycles, adjust the soft-pack battery to 100% SOC, and also take points at a total of 5 points at the four corners and the center of the battery cell to measure its thickness and take the average value as the thickness of the battery cell after 500 cycles and record it as D2, and record (D2-D1) / D1 as the battery cell thickness growth rate.
[0272] Table 1
[0273]
[0274]
[0275] According to Table 1, we can see that:
[0276] It can be seen from Examples 1a-4a and Comparative Examples 5-8 that the positive electrode additive of the present application has a more excellent first charge specific capacity; and the positive electrode additive of the embodiment has a lower first discharge specific capacity and a lower first charge voltage platform, indicating that it can more fully decompose to produce lithium ions at a lower voltage, thereby being able to better replenish lithium ions for the electrochemical device and improve the electrochemical performance of the electrochemical device.
[0277] It can be seen from the comparison of Examples 1b-10b with Comparative Examples 1-4 that the composite positive electrode material (Examples 1b-9b) or positive electrode additive (Example 10b) in the present application can improve the initial charge and discharge specific capacity and cycle life of the electrochemical device.
[0278] Further, the decomposition rate of the positive electrode additive can be calculated according to Table 1, decomposition rate = initial charge specific capacity / theoretical specific capacity (theoretical specific capacity can be obtained by searching professional materials). According to Examples 1a-4a compared with Comparative Examples 5-8, the decomposition voltage platforms of the commercial oxalate and carbonate in the comparative examples are 4.8 and 4.9V, respectively, and the decomposition rates charged to 5V are 57% and 49%, respectively, while the decomposition voltage platforms of the lithium oxalate and lithium carbonate in the examples of the present application are reduced to 4.75 and 4.65V, respectively, and the decomposition rates charged to 5V are also increased to 99% and 87%, respectively, indicating that the positive electrode additive of the present application can be fully decomposed at a lower voltage, which helps to improve the electrochemical performance of the electrochemical device.
[0279] Since the first discharge specific capacity of the electrochemical device in Examples 1b-10b is significantly greater than the first discharge specific capacity of the electrochemical device in Comparative Examples 1-4, it indicates that the decomposition of the coating layer or the positive electrode additive in the composite positive electrode material in Examples 1b-10b can improve the electrochemical performance of the electrochemical device, and according to calculations, the decomposition rate of the coating layer or the decomposition rate of the positive electrode additive in Examples 1b-10b is greater than or equal to 90%.
[0280] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A positive electrode additive, characterized in that: The positive electrode additive is an active ion salt with a relative crystallinity of 0-95%.
2. The positive electrode additive according to claim 1, characterized in that The positive electrode additive is a sheet structure formed by a first nanometer active ion salt; The size of the first nano-active ion salt is less than 150 nm; The size of the positive electrode additive is less than 10 μm.
3. A method for preparing the positive electrode additive according to claim 1 or 2, characterized in that: include: The positive electrode additive is obtained by subjecting a first raw material system including the active ion salt raw material to a first freeze-drying treatment.
4. The method for preparing the positive electrode additive according to claim 3, characterized in that: The first raw material system further includes a surfactant.
5. The method for preparing the positive electrode additive according to claim 4, characterized in that: The mass ratio of the active ion salt raw material to the surfactant is (100-1000): 1; and / or, In the first freeze-drying process, the temperature is -100 to -50°C and the time is 2 to 6 hours.
6. A composite positive electrode material, characterized in that: The composite positive electrode material comprises a core and a coating layer coated on at least a portion of the surface of the core; The inner core includes a positive electrode active material, and the coating layer includes an active ion salt; The relative crystallinity of the coating layer is 0-95%.
7. The composite positive electrode material according to claim 6, characterized in that: The coating layer includes a first coating layer; The first coating layer includes a second nanometer active ion salt, and the size of the second nanometer active ion salt is 1 nm-20 μm.
8. The composite positive electrode material according to claim 7, characterized in that: The positive electrode active material is a polycrystalline positive electrode active material, and the coating layer further includes a second coating layer, and the second coating layer is coated on at least a part of the surface of the core and / or the first coating layer; The second coating layer includes a third nanometer active ion salt, and the size of the third nanometer active ion salt is 1-500 nm.
9. The composite positive electrode material according to any one of claims 6 to 8, characterized in that: The size of the positive electrode active material is 0.5-100 μm.
10. The composite positive electrode material according to any one of claims 6 to 9, characterized in that: In the composite positive electrode material, the mass ratio of the core to the coating layer is 1:(0.005-0.5).
11. A method for preparing the composite positive electrode material according to any one of claims 6 to 10, characterized in that: include: Performing a second freeze-drying treatment on a second raw material system including the positive electrode active material and an active ion salt raw material to obtain the composite positive electrode material; The positive electrode active material forms a core, and the active ion salt raw material forms a coating layer that covers at least a portion of the surface of the core.
12. The method for preparing a composite positive electrode material according to claim 11, characterized in that: The second raw material system further includes a surfactant.
13. The method for preparing a composite positive electrode material according to claim 12, characterized in that: The mass ratio of the total mass of the active ion salt raw material and the positive electrode active material to the surfactant is (100-1000): 1; and / or, In the second freeze-drying treatment, the temperature is -100 to -50°C and the time is 2 to 6 hours.
14. A positive electrode sheet, characterized in that: It comprises the positive electrode additive according to any one of claims 1 to 2, and / or the composite positive electrode material according to any one of claims 6 to 10.
15. The positive electrode sheet according to claim 14, characterized in that: In the positive electrode active layer of the positive electrode sheet, the mass percentage of the positive electrode additive is ≤10%.
16. An electrochemical device, characterized in that: Including the positive electrode sheet as described in claim 14 or 15.
17. An electronic device, characterized in that: The driving source or energy storage source of the electronic device includes the electrochemical device according to claim 16.