Positive electrode and secondary battery including same

By using side-by-side single-wall carbon nanotube structures in the positive electrode of the lithium secondary battery, the problems of rolling damage and conductive agent migration are solved, and the input/output characteristics and life of the battery are improved.

CN119009064APending Publication Date: 2024-11-22LG ENERGY SOLUTION LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411225387.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-10-04
Filing Date
2020-09-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The positive electrode of existing lithium secondary batteries is easily damaged during the rolling process, resulting in reduced conductivity and weakened adhesion. When using carbon nanotube dispersion with low solid content, the conductive agent is easily migrated, affecting the input of the battery/ Output characteristics and lifespan.

Method used

Using a second positive electrode active material layer of a carbon nanotube structure including 2 to 5,000 single-walled carbon nanotube units side by side, combined with the first positive electrode active material layer, the pressure is dispersed and the positive electrode activity is maintained during rolling through the carbon nanotube structure. Materials to reduce the migration of conductive agents.

Benefits of technology

It effectively reduces damage to the positive electrode active material, improves the input/output characteristics and life characteristics of the battery, and enhances conductivity and adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009064A_ABST
    Figure CN119009064A_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode and a secondary battery comprising the same, the positive electrode comprising: a positive electrode current collector, a first positive electrode active material layer provided on the positive electrode current collector, and a second positive electrode active material layer provided on the first positive electrode active material layer; wherein the first positive electrode active material layer comprises a first positive electrode active material; wherein the second positive electrode active material layer includes a second positive electrode active material and a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are bonded side by side, and wherein a thickness of the second positive electrode active material layer is greater than or equal to a thickness of the first positive electrode active material layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with an application date of September 29, 2020, application number 202080033488.1, and invention name “Positive electrode and secondary battery including the positive electrode” (PCT / KR2020 / 013398, date of entry into the national phase on November 3, 2021).

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit of Korean Patent Application No. 10-2019-0123144, filed on October 4, 2019, the disclosure of which is incorporated herein by reference. Technical Field

[0004] The present invention relates to a positive electrode and a secondary battery including the positive electrode, wherein the positive electrode includes: a positive electrode collector, a first positive electrode active material layer disposed on the positive electrode collector and including a first positive electrode active material, and a second positive electrode active material layer disposed on the first positive electrode active material layer; wherein the second positive electrode active material layer includes: a second positive electrode active material; and a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are combined side by side, wherein the content of the carbon nanotube structure in the second positive electrode active material layer is 0.01 wt % to 1.0 wt %. Background Art

[0005] With the recent technological development and increased demand for mobile devices, the demand for batteries as energy sources has increased significantly, and various studies on batteries that can meet various needs have been carried out accordingly. In particular, as a power source for such devices, lithium secondary batteries with excellent life characteristics and cycle characteristics and high energy density have been actively studied.

[0006] A lithium secondary battery refers to a battery that includes a non-aqueous electrolyte containing lithium ions in an electrode assembly, the electrode assembly comprising: a positive electrode including a positive electrode active material capable of inserting / deinserting lithium ions, a negative electrode including a negative electrode active material capable of inserting / deinserting lithium ions, and a microporous separator disposed between the positive electrode and the negative electrode.

[0007] Since the conductivity of the positive electrode cannot be ensured only by the positive electrode active material, the resistance of the battery may be too high, and therefore, the positive electrode generally further includes a conductive agent. Generally, a point-type conductive agent such as carbon black is mainly used, and a linear conductive agent such as carbon nanotubes and carbon nanofibers has also been used to increase the battery capacity by further improving the conductivity.

[0008] Single-walled carbon nanotubes are one of the linear conductive agents, and due to their thin and elongated shape, the conductivity in the positive electrode active material layer is improved. Therefore, generally, a dispersion including single-walled carbon nanotube units is prepared, wherein the single-walled carbon nanotube units are completely dispersed so that the single-walled carbon nanotube units exist in a single chain form, and then the positive electrode slurry is prepared by using the dispersion, and the positive electrode active material layer is prepared by using the positive electrode slurry. Therefore, the single-walled carbon nanotube exists in the positive electrode active material layer as a unit (single chain). However, since the single-walled carbon nanotube unit is easy to break, it is difficult for the single-walled carbon nanotube unit to smoothly play a buffering role, which inhibits the damage (e.g., breakage) to the positive electrode active material during the rolling process during the preparation of the battery, and therefore, the damage to the positive electrode active material is accelerated. In addition, since the single-walled carbon nanotube unit has a small diameter and is easy to break, these units block the space between the positive electrode active materials, and therefore, the porosity of the positive electrode active material layer is low and the mobility of the electrolyte solution is suppressed, thereby reducing the lithium ion diffusion rate.

[0009] In the case of using carbon nanotubes as a conductive agent, in order to uniformly arrange the carbon nanotubes in the positive electrode active material layer, a carbon nanotube dispersion with a low solid content must be used. However, if a carbon nanotube dispersion with a low solid content is used, there is the following problem: since the binder and the conductive agent have a relatively lower density than the positive electrode active material, they are easily moved to the upper part of the positive electrode active material layer (away from the current collector) during drying of the positive electrode, that is, a migration phenomenon occurs, which leads to a significant decrease in the positive electrode adhesion and conductivity.

[0010] Therefore, in the present invention, a positive electrode capable of minimizing damage to a positive electrode active material during rolling and minimizing problems caused by a migration phenomenon of a binder is introduced. Summary of the invention

[0011] Technical issues

[0012] One aspect of the present invention provides a positive electrode that can minimize damage to a positive electrode active material and improve input / output characteristics and lifespan characteristics by minimizing problems caused by a migration phenomenon of a binder.

[0013] Another aspect of the present invention provides a secondary battery including the positive electrode.

[0014] Technical Solution

[0015] According to one aspect of the present invention, a positive electrode is provided, which includes: a positive electrode collector, a first positive electrode active material layer arranged on the positive electrode collector and including a first positive electrode active material, and a second positive electrode active material layer arranged on the first positive electrode active material layer; wherein the second positive electrode active material layer includes: a second positive electrode active material; and a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are combined side by side, wherein the carbon nanotube structure is included in the second positive electrode active material layer in an amount of 0.01 wt % to 1.0 wt %.

[0016] According to another aspect of the present invention, a secondary battery including the electrode is provided.

[0017] Beneficial Effects

[0018] With regard to the positive electrode according to the present invention, since the second positive electrode active material layer directly subjected to pressure during rolling includes a carbon nanotube structure in the form of a long rope in which 2 to 5,000 single-walled carbon nanotube units are combined side by side, the carbon nanotube structure can firmly hold the positive electrode active material together while connecting the positive electrode active material, and the carbon nanotube structure can appropriately disperse the pressure during rolling. Therefore, the damage to the positive electrode active material can be minimized. In addition, since the positive electrode has a first positive electrode active material layer and a second positive electrode active material layer sequentially arranged as respective slurries, the above-mentioned migration phenomenon of the binder and the conductive agent can be minimized. Therefore, the input / output characteristics and life characteristics of the battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The following drawings attached to the specification illustrate preferred embodiments of the present invention by way of example, and together with the detailed description of the present invention given below, are used to further understand the technical concept of the present invention, and therefore the present invention should not be interpreted solely by the contents in these drawings.

[0020] Figure 1 These are scanning electron microscope (SEM) images of the multi-walled carbon nanotube unit (A) used in the comparative example of the present invention and the carbon nanotube structure (B, C) used in the examples.

[0021] Figure 2 These are transmission electron microscope (TEM) images of the carbon nanotube structure (A) used in the example of the present invention and the single-walled carbon nanotube unit (B) used in the comparative example.

[0022] Figure 3 is a SEM image of the second positive electrode active material layer of the positive electrode according to Example 1 of the present invention.

[0023] Figure 4 is a TEM image of the positive electrode according to Example 1 of the present invention.

[0024] Figure 5 is a SEM image of the second positive electrode active material layer of the positive electrode according to Comparative Example 3 of the present invention.

[0025] Figure 6 is a SEM image of the second positive electrode active material layer of the positive electrode according to Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0026] It will be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in commonly used dictionaries, and it will be further understood that, based on the principle that the inventor can appropriately define the meanings of words or terms to best interpret the present invention, these words or terms should be interpreted as having meanings consistent with the technical concept of the present invention and the meanings in the context of related technologies.

[0027] The terms used in this specification are only used to describe exemplary embodiments and are not intended to limit the present invention. Unless otherwise indicated, terms in the singular form may include plural forms.

[0028] It will be further understood that the terms “comprises,” “comprising,” or “having” in this specification specify the presence of stated features, numbers, steps, elements, or a combination thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, elements, or a combination thereof.

[0029] In the present specification, "%" means weight % unless otherwise specifically indicated.

[0030] In this specification, the "specific surface area" is measured by the BET method, and specifically, the specific surface area can be calculated from the nitrogen adsorption amount at liquid nitrogen temperature (77K) using BELSORP-mini II manufactured by Bell Japan.

[0031] The average particle size (D 50 ) can be defined as the particle size when the cumulative volume in the particle size distribution curve is 50%. For example, the average particle size D can be measured by using a laser diffraction method. 50 Laser diffraction can usually measure particle sizes from submicron to several millimeters, and can obtain results with high repeatability and high resolution.

[0032] In the present invention, the expression "single-wall carbon nanotube unit" means a tubular unit having a single wall composed of carbon atoms, and the expression "multi-wall carbon nanotube unit" means a tubular unit having multiple walls composed of carbon atoms.

[0033] Hereinafter, the present invention will be described in detail.

[0034] positive electrode

[0035] The positive electrode according to the present invention includes: a positive electrode collector, a first positive electrode active material layer disposed on the positive electrode collector and including a first positive electrode active material, and a second positive electrode active material layer disposed on the first positive electrode active material layer; wherein the second positive electrode active material layer includes: a second positive electrode active material; and a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are combined side by side, wherein the content of the carbon nanotube structure in the second positive electrode active material layer can be 0.01 wt % to 1.0 wt %.

[0036] The positive electrode may include a positive electrode active material layer. The positive electrode may further include a positive electrode current collector, and in this case, the positive electrode active material layer may be provided on one surface or both surfaces of the positive electrode current collector.

[0037] There is no particular limitation on the positive electrode current collector as long as it has conductivity and does not cause adverse chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, alloys thereof, these materials surface-treated with one of carbon, nickel, titanium, silver, etc., or calcined carbon can be used.

[0038] The positive electrode current collector may generally have a thickness of 3 μm to 500 μm, and fine concavoconvexities may be formed on the surface of the positive electrode current collector to improve the adhesion of the positive electrode active material. In addition, the positive electrode current collector may be used in various shapes such as a film, a sheet, a foil, a net, a porous body, a foam body, a non-woven fabric body, etc.

[0039] The positive electrode active material layer may include a first positive electrode active material layer and a second positive electrode active material layer. The first positive electrode active material layer may be disposed on the positive electrode current collector, and specifically, may be in direct contact with the positive electrode current collector.

[0040] Generally, when using carbon nanotubes as a conductive agent, in order to uniformly arrange the carbon nanotubes in the positive electrode active material layer, a carbon nanotube dispersion with a low solid content can be used. However, when using a carbon nanotube dispersion with a low solid content, there is a problem that the adhesion and conductivity of the positive electrode are significantly reduced due to the following phenomenon (migration phenomenon). In this phenomenon, the binder and the conductive agent have a relatively lower density than the positive electrode active material and are prone to move to the upper part (away from the current collector and closer to the surface) of the positive electrode active material layer during the drying of the positive electrode slurry. In contrast, since the positive electrode of the present invention has a first positive electrode active material layer and a second positive electrode active material layer which are sequentially provided as respective slurries, the above-mentioned migration phenomenon of the binder and the conductive agent can be minimized. Therefore, the input / output characteristics and life characteristics of the battery can be improved.

[0041] The first positive electrode active material layer may include a first positive electrode active material.

[0042] The first positive electrode active material may be a positive electrode active material commonly used in the art, but its type is not particularly limited.

[0043] For example, as the first positive electrode active material, a lithium oxide containing lithium and at least one metal such as cobalt, manganese, nickel or aluminum can be used. Specifically, the lithium oxide may include: lithium manganese-based oxides (such as LiMnO2, LiMn2O, etc.); lithium cobalt-based oxides (such as LiCoO2, etc.); lithium nickel-based oxides (such as LiNiO2, etc.); lithium nickel manganese-based oxides (such as LiNi 1- Y1 Mn Y1 O2 (where 0 < Y1 < 1), LiMn 2-Z1 Ni z1 O4 (where 0 < Z1 < 2), etc.); lithium nickel cobalt-based oxides (such as LiNi 1- Y2 Co Y2 O2 (where 0 < Y2 < 1)); lithium manganese cobalt-based oxides (such as LiCo 1-Y3 Mn Y3 O2 (where 0 < Y3 < 1), LiMn 2-Z2 Co z2 O4 (where 0 < Z2 < 2), etc.); lithium nickel cobalt manganese-based oxides (such as Li(Ni P1 Co Q1 Mn R1 )O2 (where 0 < P1 < 1, 0 < Q1 < 1, 0 < R1 < 1, and P1 + Q1 + R1 = 1) or Li(Ni P2 Co Q2 Mn R2)O4 (where 0 < P2 < 2, 0 < Q2 < 2, 0 < R2 < 2, and P2 + Q2 + R2 = 2, etc.); or lithium nickel cobalt manganese - transition metal (M) oxide (e.g., Li(Ni P3 Co Q3 Mn R3 M 1 S )O2 (where M 1 is selected from the group consisting of aluminum (Al), copper (Cu), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), zirconium (Zr), zinc (Zn), tantalum (Ta), niobium (Nb), magnesium (Mg), boron (B), tungsten (W), and molybdenum (Mo), and P3, Q3, R3, and S are atomic fractions of each independent element, where 0 < P3 < 1, 0 < Q3 < 1, 0 < R3 < 1, 0 < S < 1, and P3 + Q3 + R3 + S = 1), etc.), and may include any one of them or a mixture of two or more of them.

[0044] The first positive electrode active material may be included in the first positive electrode active material layer in an amount of 70% to 99.5% by weight, for example, 80% to 99% by weight. When the amount of the first positive electrode active material satisfies the above range, excellent energy density, positive electrode adhesion, and conductivity can be achieved.

[0045] The first positive electrode active material layer may further include a first conductive agent.

[0046] The first conductive agent may include at least one selected from the group consisting of a carbon nanotube structure, a multi - walled carbon nanotube unit, and carbon black. The carbon nanotube structure will be described in detail later.

[0047] The first conductive agent may be included in the positive electrode active material layer in an amount of 0.01% to 2.0% by weight, particularly 0.01% to 1.5% by weight, and more particularly 0.05% to 1.0% by weight. When the amount of the first conductive agent satisfies the above range, by using only a small amount of the first conductive agent, the adhesion and conductivity of the positive electrode can be significantly improved, and a battery with excellent input / output characteristics and life characteristics can be obtained.

[0048] The thickness of the first positive electrode active material layer may be 1 μm to 100 μm, particularly 5 μm to 90 μm, and more particularly 10 μm to 80 μm. When the thickness satisfies the above range, the above - mentioned migration phenomenon of the binder and the conductive agent can be minimized. Therefore, the adhesion and conductivity of the positive electrode can be significantly improved, and the input / output characteristics and life characteristics of the battery can be improved.

[0049] The second positive electrode active material layer may be disposed on the first positive electrode active material layer. Specifically, the second positive electrode active material layer may be spaced apart from the current collector, while the first positive electrode active material layer is disposed therebetween.

[0050] The second positive electrode active material layer may include a second positive electrode active material.

[0051] The second positive electrode active material may be a positive electrode active material commonly used in the art, but there is no particular limitation on its type.

[0052] For example, as the second positive electrode active material, a lithium oxide containing lithium and at least one metal such as cobalt, manganese, nickel or aluminum may be used. Specifically, the lithium oxide may include: lithium manganese-based oxides (such as LiMnO2, LiMn2O, etc.); lithium cobalt-based oxides (such as LiCoO2, etc.); lithium nickel-based oxides (such as LiNiO2, etc.); lithium nickel manganese-based oxides (such as LiNi 1- Y1 Mn Y1 O2 (where 0 < Y1 < 1), LiMn 2-Z1 Ni z1 O4 (where 0 < Z1 < 2), etc.); lithium nickel cobalt-based oxides (such as LiNi 1- Y2 Co Y2 O2 (where 0 < Y2 < 1)); lithium manganese cobalt-based oxides (such as LiCo 1-Y3 Mn Y3 O2 (where 0 < Y3 < 1), LiMn 2-Z2 Co z2 O4 (where 0 < Z2 < 2), etc.); lithium nickel cobalt manganese-based oxides (such as Li(Ni P1 Co Q1 Mn R1 )O2 (where 0 < P1 < 1, 0 < Q1 < 1, 0 < R1 < 1, and P1 + Q1 + R1 = 1) or Li(Ni P2 Co Q2 Mn R2 )O4 (where 0 < P2 < 2, 0 < Q2 < 2, 0 < R2 < 2, and P2 + Q2 + R2 = 2), etc.); or lithium nickel cobalt manganese-transition metal (M) oxides (such as Li(Ni P3 Co Q3 Mn R3 M 1 S )O2 (where M 1Selected from the group consisting of aluminum (Al), copper (Cu), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), zirconium (Zr), zinc (Zn), tantalum (Ta), niobium (Nb), magnesium (Mg), boron (B), tungsten (W), and molybdenum (Mo), and P3, Q3, R3, and S are atomic fractions of each independent element, where 0 < P3 < 1, 0 < Q3 < 1, 0 < R3 < 1, 0 < S < 1, and P3 + Q3 + R3 + S = 1), etc.), and may include any one of them or a mixture of two or more of them.

[0053] The second positive electrode active material may be included in the second positive electrode active material layer in an amount of 70 wt% to 99.5 wt%, for example, 80 wt% to 99 wt%. When the amount of the second positive electrode active material satisfies the above range, excellent energy density, positive electrode adhesion, and conductivity can be achieved.

[0054] The second positive electrode active material layer may further include a carbon nanotube structure.

[0055] The carbon nanotube structure may include a plurality of single-walled carbon nanotube units. Specifically, the carbon nanotube structure may be a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are bonded to each other. More specifically, considering the durability and conductive network of the positive electrode, the carbon nanotube structure is most preferably a carbon nanotube structure in which 2 to 4,500, preferably 50 to 4,000, and more preferably 1,000 to 4,000 single-walled carbon nanotube units are bonded to each other.

[0056] The single-walled carbon nanotube units may be arranged side by side and bonded in the carbon nanotube structure (a flexible cylindrical structure in which the units are bonded such that the long axes of the units are parallel to each other) to form the carbon nanotube structure. The carbon nanotube structures are interconnected in the positive electrode to form a network structure.

[0057] In a conventional positive electrode including carbon nanotubes, a positive electrode active material layer is prepared by dispersing a bundle type or entangled type carbon nanotube (a form in which single-walled carbon nanotube units or multi-walled carbon nanotube units are attached or entangled to each other) in a dispersion medium to prepare a conductive agent dispersion, and then using the conductive agent dispersion. In this case, since the carbon nanotubes are completely dispersed in the conventional conductive agent dispersion, the carbon nanotubes exist as a conductive agent dispersion in which single-chain carbon nanotube units are dispersed. With respect to conventional conductive agent dispersions, since the carbon nanotube units are easily cut by excessive dispersion processes, the carbon nanotube units have a length shorter than the initial length (e.g., 3 μm or shorter) or have a shape that may be easily cut. Therefore, since these units cannot smoothly play a buffering role that suppresses damage (e.g., breakage) to the positive electrode active material during the rolling process during the preparation of the battery, damage to the positive electrode active material is likely to occur. In addition, since the single-walled carbon nanotube unit has a small diameter and is easily broken, it is difficult to ensure the space between the positive electrode active materials, and therefore, the porosity of the positive electrode active material layer is inevitably low. Therefore, the lithium ion diffusion rate is reduced. In addition, with respect to the multi-walled carbon nanotube unit, the structural defects are high due to the mechanism of node growth (these units are not smooth and linear, but nodes exist due to defects generated during the growth process). Therefore, the multi-walled carbon nanotube unit is more easily cut in the dispersion process (see Figure 2 A), and the short-cut multi-walled carbon nanotube units can be easily aggregated by π-π stacking caused by the carbon surface of the unit. Therefore, it is more difficult to make the multi-walled carbon nanotube units more uniformly dispersed in the positive electrode slurry.

[0058] Alternatively, regarding the carbon nanotube structure included in the second positive electrode active material layer of the present invention, since the carbon nanotube structure is a structure in which 2 to 5,000 single-walled carbon nanotube units maintaining relatively high crystallinity without structural defects are arranged side by side and bonded together (see Figure 1 B and C and Figure 2A) in the form of a rope, even if the volume of the positive electrode active material changes, the single-walled carbon nanotube unit will not be cut, and its length can be maintained smoothly, so that the conductivity of the positive electrode can be maintained even during the continuous charge / discharge process of the battery. In addition, since the high conductivity of the single-walled carbon nanotube unit with high crystallinity leads to an increase in the conductivity of the positive electrode, the resistance of the positive electrode can be reduced and the input / output characteristics and life characteristics of the battery can be significantly improved. In addition, since the carbon nanotube structure in the second positive electrode active material layer that directly bears the pressure during rolling is interconnected and has a network structure, damage to the second positive electrode active material (for example, breakage phenomenon such as cracks) can be suppressed. In addition, even if cracks are generated in the second positive electrode active material, since the carbon nanotube structure can connect the second positive electrode active material while passing through the cracks, the conductive network can be maintained. In addition, since the carbon nanotube structure is not easily damaged and can maintain its long shape, the conductive network can be enhanced throughout the second positive electrode active material layer. In addition, by suppressing the peeling of the second positive electrode active material, the positive electrode adhesion can be significantly improved.

[0059] In the carbon nanotube structure, the average diameter of the single-walled carbon nanotube unit can be 0.5nm to 5nm, for example, 1nm to 5nm. When this average diameter is met, the conductivity of the positive electrode can reach the maximum even with a very small amount of conductive agent. When the prepared positive electrode is observed by TEM, the average diameter corresponds to the average value of the diameters of the first 100 single-walled carbon nanotube units with larger diameters and the last 100 single-walled carbon nanotube units with smaller diameters.

[0060] In the carbon nanotube structure, the average length of the single-walled carbon nanotube unit can be 1 μm to 100 μm, for example, 5 μm to 50 μm. When this average length is met, since a long conductive path for conductive connection between the positive electrode active materials can be formed and a unique network structure can be formed, the conductivity of the positive electrode can be maximized even with a very small amount of conductive agent. When the prepared positive electrode is observed by TEM, the average length corresponds to the average of the lengths of the first 100 single-walled carbon nanotube units with longer lengths and the last 100 single-walled carbon nanotube units with shorter lengths.

[0061] The specific surface area of ​​a single-walled carbon nanotube unit can be 500m 2 / g to 1,000m 2 / g, for example 600m 2 / g to 800m 2 / g. When the specific surface area satisfies the above range, since the conductive path in the positive electrode can be smoothly ensured by the wide specific surface area, the conductivity of the positive electrode can be maximized even with a very small amount of conductive agent. The specific surface area of ​​the single-walled carbon nanotube unit can be specifically calculated by the nitrogen adsorption at liquid nitrogen temperature (77K) using Bell Japan's BELSORP-mini II.

[0062] The average diameter of the carbon nanotube structure can be 2nm to 200nm, particularly 5nm to 150nm, and more particularly 50nm to 120nm. When the average diameter meets the above range, since it effectively forms a conductive network structure and is conducive to connecting active materials, excellent conductivity can be achieved. When the prepared positive electrode is observed by SEM, the average diameter corresponds to the average value of the diameters of the first 100 carbon nanotube structures with larger diameters and the last 100 carbon nanotube structures with smaller diameters.

[0063] The average length of the carbon nanotube structure can be 1 μm to 500 μm, particularly 5 μm to 100 μm, and more particularly 10 μm to 70 μm. When the average length meets the above range, since it effectively forms a conductive network structure and is conducive to connecting the positive electrode active material, excellent conductivity can be achieved. When the prepared positive electrode is observed by SEM, the average length corresponds to the average value of the lengths of the first 100 carbon nanotube structures with longer lengths and the last 100 carbon nanotube structures with shorter lengths.

[0064] The carbon nanotube structure can be included in the second positive electrode active material layer in an amount of 0.01 wt % to 1.0 wt %, can be specifically included in an amount of 0.01 wt % to 0.5 wt %, and can be more specifically included in an amount of 0.01 wt % to 0.2 wt %. When the amount of the carbon nanotube structure meets the above range, since the conductive path in the second positive electrode active material layer can be ensured, the life characteristics of the battery can be improved while the positive electrode resistance is kept at a low level. When preparing a conductive agent dispersion, the carbon nanotubes are fully dispersed (as a conventional dispersion method, in which the carbon nanotubes are dispersed so that the single-chain carbon nanotube units are separated from each other as much as possible), and the carbon nanotube structure will not be generated, or even if the carbon nanotube structure is inadvertently generated, only a very small amount (e.g., 0.0005 wt %) of the carbon nanotube structure will be generated. That is, the above-mentioned amount range may never be reached in the usual way. Since the carbon nanotube structure is in a form in which 2 to 5,000 single-walled carbon nanotube units are arranged side by side and combined, even if the volume of the positive electrode active material changes, the carbon nanotube structure will not be cut and its length can be smoothly maintained. Therefore, due to the high conductivity of the carbon nanotube structure, the conductive network in the second positive electrode active material layer can be maintained and the conductivity of the second positive electrode active material layer can be smoothly ensured. Therefore, even if the amount of the carbon nanotube structure in the second positive electrode active material layer is small, the input / output characteristics and life characteristics of the battery can be excellent.

[0065] In some cases, the single-walled carbon nanotube units can be surface treated by oxidation or nitridation to improve affinity with the dispersion.

[0066] The exposed area of ​​the surface of the second positive electrode active material not covered by the carbon nanotube structure may be in the range of 50% to 99.99% of the entire surface of the second positive electrode active material, and may be specifically in the range of 50% to 99.9%. That is, this means that the carbon nanotube structure is not formed as a layer on the second positive electrode active material, but only connects the second positive electrode active material.

[0067] The thickness of the second positive electrode active material layer may be 1 μm to 100 μm, particularly 5 μm to 90 μm, and more particularly 10 μm to 80 μm. When the thickness satisfies the above range, the above migration phenomenon of the binder and the conductive agent can be minimized. Therefore, the adhesion and conductivity of the positive electrode can be significantly improved, and the input / output characteristics and life characteristics of the battery can be improved.

[0068] The thickness of the second positive electrode active material layer may be greater than or equal to the thickness of the first positive electrode active material layer. The thickness ratio of the first positive electrode active material layer to the second positive electrode active material layer may be 10:90 to 50:50, particularly 20:80 to 50:50, and more particularly 25:75 to 50:50. In the case where the ratio does not meet the above range, the effect of suppressing the above migration phenomenon of the binder and the conductive agent is reduced, and the effect of improving the diffusion resistance by increasing the porosity of the second positive electrode active material layer is reduced. Since when the thickness of the first positive electrode active material layer is outside the above range and is too small, the effect of suppressing the above migration phenomenon of the binder and the conductive agent is reduced, and the effect of improving the positive electrode adhesion and improving the interface resistance becomes negligible.

[0069] There is an interface between the first positive electrode active material layer and the second positive electrode active material layer. This can be confirmed by the cross section of the prepared positive electrode. In contrast, if the positive electrode active material layer is formed in a single layer structure rather than a multilayer structure (by coating only once using a single positive electrode slurry), no interface is observed.

[0070] The first positive electrode active material layer and the second positive electrode active material layer may each further include a binder, and the binder of the first positive electrode active material layer and the binder of the second positive electrode active material layer may be the same or different from each other. The binder is used to ensure the adhesion between the positive electrode active materials and the adhesion of the positive electrode active material to the collector, wherein the common binder used in the art can be used, and there is no particular restriction on its type. The binder may include, for example: polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, carboxymethyl cellulose (carboxymethyl cellulose: CMC), styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and any one of them or a mixture of two or more thereof may be used.

[0071] The binder may be included in the first electrode active material layer (or the second positive electrode active material layer) in an amount of 10 wt % or less, for example, 0.1 wt % to 5 wt %. When the amount of the binder satisfies the above range, excellent positive electrode adhesion can be achieved while minimizing the increase in positive electrode resistance.

[0072] Method for preparing positive electrode

[0073] Next, a method for producing the positive electrode of the present invention will be described.

[0074] The preparation method of the positive electrode of the present invention may include the following steps: preparing a first positive electrode slurry and a second positive electrode slurry; forming a first positive electrode active material layer on a positive electrode current collector using the first positive electrode slurry; and forming a second positive electrode active material layer on the first positive electrode active material layer using the second positive electrode slurry; wherein the first positive electrode slurry includes a first positive electrode active material, and the second positive electrode slurry includes a second positive electrode active material and a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are combined side by side; wherein the carbon nanotube structure may be contained in the second positive electrode active material layer in an amount of 0.01 wt % to 1.0 wt %. The first positive electrode active material, the second positive electrode active material, and the carbon nanotube structure are the same as those of the first positive electrode active material, the second positive electrode active material, and the carbon nanotube structure of the above-mentioned embodiment.

[0075] (1) Preparation of the first positive electrode slurry and the second positive electrode slurry

[0076] The method for preparing the first positive electrode slurry may be the same as the conventional method for preparing the positive electrode slurry. For example, after preparing a mixture including the first positive electrode active material, the first conductive agent (the same as the first conductive agent of the above embodiment) and the solvent (which may further include a binder), the mixture is stirred to prepare the first positive electrode slurry.

[0077] However, in the case where the first positive electrode slurry includes a carbon nanotube structure, a carbon nanotube structure dispersion described later may be prepared.

[0078] The solvent may include, for example: an amide-based polar organic solvent such as dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc) and N-methylpyrrolidone (NMP); an alcohol such as methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol or octanol; a glycol such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,5-pentanediol or hexanediol ; Polyhydroxy alcohol, such as glycerol, trimethylolpropane, pentaerythritol or sorbitol; Ethylene glycol ether, such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether or tetraethylene glycol monobutyl ether; Ketone, such as acetone, methyl ethyl ketone, methyl propyl ketone or cyclopentanone; Esters, such as ethyl acetate, γ-butyrolactone and ε-propiolactone, and any one of them or a mixture of two or more thereof can be used, but the present invention is not limited thereto. The solvent may be the same as or different from the dispersion medium used in the pre-dispersion, and the solvent may preferably be N-methylpyrrolidone (NMP, N-methylpyrrolidone).

[0079] After preparing a mixture including the second positive electrode active material, the carbon nanotube structure dispersion, and a solvent, a second positive electrode slurry may be prepared by stirring the mixture.

[0080] The carbon nanotube structure dispersion can be prepared as follows.

[0081] The preparation of the carbon nanotube structure dispersion may include the following steps: preparing a mixed solution including a dispersion medium, a dispersant, and bundle-type single-walled carbon nanotubes (bonded bodies or aggregates of single-walled carbon nanotube units) (S1-1); and dispersing the bundle-type single-walled carbon nanotubes by applying a shear force to the mixed solution, thereby forming a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are bonded side by side (S1-2).

[0082] In step S1-1, a mixed solution can be prepared by adding bundled single-walled carbon nanotubes and a dispersant to a dispersion medium. The bundled single-walled carbon nanotubes exist in the form of bundles combining the above-mentioned single-walled carbon nanotube units, wherein the bundled carbon nanotubes generally include 2 or more, substantially 500 or more, for example, 5,000 or more single-walled carbon nanotube units.

[0083] The specific surface area of ​​bundled single-walled carbon nanotubes can be 500m 2 / g to 1,000m 2 / g, for example 600m2 / g to 800m 2 When the specific surface area satisfies the above range, since a conductive path in the second positive electrode active material layer can be smoothly ensured by a wide specific surface area, the conductivity of the second positive electrode active material layer can be maximized even with a very small amount of the conductive agent.

[0084] The bundled single-walled carbon nanotubes may be included in the mixed solution in an amount of 0.1 wt % to 1.0 wt %, for example, 0.2 wt % to 0.5 wt %. When the amount of the bundled single-walled carbon nanotubes satisfies the above range, since the bundled single-walled carbon nanotubes are dispersed at an appropriate level, a carbon nanotube structure may be formed at an appropriate level, and dispersion stability may be improved.

[0085] The dispersion medium may include, for example: an amide-based polar organic solvent such as dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc) and N-methylpyrrolidone (NMP); an alcohol such as methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol or octanol; a glycol such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,5-pentanediol or hexanediol. Alcohol; polyhydric alcohol, such as glycerol, trimethylolpropane, pentaerythritol or sorbitol; glycol ether, such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether or tetraethylene glycol monobutyl ether; ketone, such as acetone, methyl ethyl ketone, methyl propyl ketone or cyclopentanone; ester, such as ethyl acetate, γ-butyrolactone and ε-propiolactone, and any one of them or a mixture of two or more thereof can be used, but the present invention is not limited thereto. Specifically, the dispersion medium can be N-methylpyrrolidone (NMP).

[0086] The dispersant may include at least one selected from hydrogenated nitrile rubber, polyvinylidene fluoride, and carboxymethyl cellulose, and specifically may be polyvinylidene fluoride or hydrogenated nitrile rubber.

[0087] In the conductive agent dispersion, the weight ratio of the bundle-type carbon nanotubes to the dispersant may be in the range of 1:0.1 to 1:7, for example, 1:1 to 1:6. When the weight ratio satisfies the above range, since the bundle-type single-walled carbon nanotubes are dispersed at an appropriate level, the carbon nanotube structure may be formed at an appropriate level, and the dispersion stability may be improved.

[0088] The solid content in the mixed solution can be in the range of 0.1 wt % to 20 wt %, for example, 1 wt % to 10 wt %. When the solid content satisfies the above range, since the bundle-type single-walled carbon nanotubes are dispersed at an appropriate level, the carbon nanotube structure can be formed at an appropriate level, and the dispersion stability can be improved. In addition, the second positive electrode slurry (slurry for preparing the second positive electrode active material layer) can have a viscosity and elasticity suitable for the formation of the second positive electrode active material layer, and also helps to increase the solid content of the second positive electrode slurry.

[0089] In step S1-2, the process of dispersing the bundle-type carbon nanotubes in the mixed solution can be performed by using a mixing device such as a homogenizer, a bead mill, a ball mill, a basket mill, a grinder, a universal stirrer, a transparent mixer, a pin mill, a TK mixer, or an ultrasonic treatment (sonification) device. Among them, the beads mill method is preferred because this method can accurately control the diameter of the carbon nanotube structure, can achieve uniform distribution of the carbon nanotube structure, and can have cost advantages.

[0090] The bead milling method may be as follows: The mixed solution may be put into a container containing beads, and the container may be rotated to disperse the bundle-type single-walled carbon nanotubes.

[0091] In this case, the conditions for performing the bead milling method are as follows.

[0092] The average diameter of the beads may be 0.5 mm to 1.5 mm, for example 0.5 mm to 1.0 mm. When the average diameter satisfies the above range, the diameter of the carbon nanotube structure can be appropriately regulated without destroying the carbon nanotube structure during the dispersion process, and a dispersion solution with a uniform composition can be prepared.

[0093] The rotation speed of the container may be in the range of 500RPM to 10,000RPM, for example, 2,000RPM to 6,000RPM. When the rotation speed satisfies the above range, the diameter of the carbon nanotube structure can be properly regulated without destroying the carbon nanotube structure during the dispersion process, and a dispersion solution with a uniform composition can be prepared.

[0094] The time for performing bead milling can be in the range of 0.5 hours to 2 hours, particularly 0.5 hours to 1.5 hours, and more particularly 0.8 hours to 1 hour. When the time satisfies the above range, the diameter of the carbon nanotube structure can be appropriately regulated without destroying the carbon nanotube structure during the dispersion process, and a dispersed solution with a uniform composition can be prepared. The execution time of bead milling refers to the total time of using bead milling, so, for example, if bead milling is performed several times, the execution time refers to the total time required for performing several bead millings.

[0095] The above-mentioned bead milling conditions are for dispersing the bundle-type single-walled carbon nanotubes at an appropriate level, and specifically exclude the case where the bundle-type single-walled carbon nanotubes are completely dispersed into single-chain single-walled carbon nanotubes. That is, the above-mentioned bead milling conditions are for forming a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are combined side by side in a conductive agent dispersion prepared by appropriately dispersing the bundle-type single-walled carbon nanotubes. This can be achieved only when the composition of the mixed solution and the conditions of the dispersion process (e.g., bead milling process) are strictly regulated.

[0096] The carbon nanotube structure dispersion can be formed by the above method.

[0097] If necessary, a binder may be further included in the positive electrode slurry (the first positive electrode slurry and the second positive electrode slurry). In this case, the binder of the above-described embodiment may be used as the binder.

[0098] (2) forming a first positive electrode active material layer on the positive electrode current collector using the first positive electrode slurry and forming a second positive electrode active material layer on the first positive electrode active material layer using the second positive electrode slurry

[0099] Next, the first positive electrode active material layer is formed by using the first positive electrode slurry prepared as described above. Specifically, the first positive electrode active material layer can be prepared by coating the first positive electrode slurry on the positive electrode collector and drying the coated positive electrode collector, or can be prepared by casting the first positive electrode slurry on a separate carrier and then laminating the film separated from the carrier on the positive electrode collector. If necessary, the first positive electrode active material layer can be formed by the above method, and then the rolling process can be further performed. In this case, considering the physical properties of the finally prepared positive electrode, drying and rolling can be performed under appropriate conditions, and there is no particular restriction.

[0100] Afterwards, a second positive electrode active material layer is formed by using the second positive electrode slurry prepared as described above. Specifically, the second positive electrode active material layer can be prepared by coating the second positive electrode slurry on the first positive electrode active material layer and drying the second positive electrode slurry, or can be prepared by casting the second positive electrode slurry on a separate carrier and then laminating the film separated from the carrier on the first positive electrode active material layer. If necessary, the second positive electrode active material layer can be formed by the above method, and then a rolling process can be further performed. In this case, taking into account the physical properties of the finally prepared positive electrode, drying and rolling can be performed under appropriate conditions without particular restrictions.

[0101] Secondary battery

[0102] A secondary battery according to another embodiment of the present invention may include a negative electrode, a positive electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode may be the positive electrode of the above embodiment.

[0103] The negative electrode may include a negative electrode current collector and a negative electrode active material layer provided on one surface or both surfaces of the negative electrode current collector.

[0104] The negative electrode current collector is not particularly limited as long as it has conductivity and does not cause adverse chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, carbonized carbon, aluminum or stainless steel surface-treated with one of nickel, titanium, silver or the like can be used as the negative electrode current collector. Specifically, transition metals such as copper and nickel that can well absorb carbon can be used as the current collector.

[0105] The negative electrode active material layer may include a negative electrode active material, a negative electrode conductive agent, and a negative electrode binder.

[0106] The negative electrode active material may be a negative electrode active material commonly used in the art, but is not particularly limited. For example, the negative electrode active material may include graphite-based active material particles or silicon-based active material particles. At least one selected from the group consisting of artificial graphite, natural graphite, graphitized carbon fiber, and graphitized mesocarbon microbeads can be used as the graphite-based active material particles, and particularly when artificial graphite is used, the rate performance can be improved. At least one selected from the group consisting of silicon (Si), SiO x (0 < x < 2), Si-C composite, and Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, transition metals, Group 13 elements, Group 14 elements, rare earth elements, and combinations thereof) can be used as the silicon-based active material particles, and particularly when Si or SiO x (0 < x < 2) is used, a high capacity of the battery can be obtained.

[0107] The negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylate, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and materials in which hydrogen is replaced by lithium (Li), sodium (Na) or calcium (Ca), or the negative electrode binder may include various copolymers thereof.

[0108] There is no particular limitation on the negative electrode conductive agent as long as it has conductivity without causing adverse chemical changes in the battery, and, for example, the following conductive materials can be used: graphite, such as natural graphite and artificial graphite; carbon black, such as acetylene black, Ketjen black, channel black, furnace black, furnace black, lamp black, or thermal black; conductive fibers, such as carbon fibers or metal fibers; conductive tubes, such as carbon nanotubes; metal powders, such as carbon fluoride powders, aluminum powders, and nickel powders; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.

[0109] The separator separates the negative electrode and the positive electrode and provides a mobile path for lithium ions, wherein any separator can be used as a separator without particular limitation, as long as it is generally used for secondary batteries, and in particular, a separator having high moisture retention capacity for electrolytes and low resistance to the transmission of electrolyte ions can be used. Specifically, a porous polymer film can be used, for example, a porous polymer film made of polyolefin-based polymers such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers, or a laminated structure having two or more layers thereof can be used as a separator. In addition, conventional porous nonwoven fabrics can be used, for example, nonwoven fabrics formed by high melting point glass fibers or polyethylene terephthalate fibers. In addition, a coated separator including a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a separator having a monolayer or multilayer structure can be selectively used.

[0110] The electrolyte may include an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten-type inorganic electrolyte that may be used in the preparation of a lithium secondary battery, but the present invention is not limited thereto.

[0111] Specifically, the electrolyte may include a nonaqueous organic solvent and a metal salt.

[0112] As the non-aqueous organic solvent, for example, aprotic solvents such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran (franc), 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate can be used.

[0113] Especially, in carbonate-based organic solvents, because ethylene carbonate and propylene carbonate as cyclic carbonate dissociate lithium salts well due to high dielectric constant as high viscosity organic solvent, cyclic carbonate can be preferably used.Because when above-mentioned cyclic carbonate is mixed with low viscosity, straight-chain carbonate of low dielectric constant such as dimethyl carbonate and diethyl carbonate and used in appropriate ratio, electrolyte with high conductivity can be prepared, so cyclic carbonate can be more preferably used.

[0114] As the metal salt, a lithium salt may be used, and the lithium salt is a material that is easily soluble in a non-aqueous organic solvent, wherein, as an anion of the lithium salt, for example, at least one selected from the group consisting of: F - , Cl - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C -CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - .

[0115] In order to improve the life characteristics of the battery, inhibit the reduction of the battery capacity, and improve the discharge capacity of the battery, in addition to the electrolyte components, at least one additive can be further added to the electrolyte, for example, a halogenated alkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum chloride.

[0116] According to another embodiment of the present invention, a battery module including the secondary battery as a unit cell and a battery pack including the battery module are provided. Since the battery module and the battery pack include secondary batteries having high capacity, high rate performance, and high cycle characteristics, the battery module and the battery pack can be used as a power source for medium and large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0117] Hereinafter, the present invention will be described in detail according to specific examples and comparative examples.

[0118] Preparation Example 1: Preparation of Carbon Black Dispersion

[0119] The specific surface area is 240m 2 / g of carbon black (in the form of secondary particles consisting of primary particles with an average diameter of 25nm) and hydrogenated nitrile rubber (weight average molecular weight: 260,000g / mol) were mixed in N-methylpyrrolidone (NMP) as a solvent to prepare a mixture with a solid content of 16.5wt%.

[0120] By stirring the mixture by a bead mill method, carbon black was dispersed in the solvent, and thus a carbon black dispersion was prepared. In this case, the diameter of the beads was 1 mm, the rotation speed of the stirring container containing the beads was 3,000 RPM, and stirring was performed for 60 minutes.

[0121] In the carbon black dispersion, the amount of carbon black was 15 wt % and the amount of hydrogenated nitrile rubber was 1.5 wt %.

[0122] Preparation Example 2: Preparation of Carbon Nanotube Structure Dispersion

[0123] Bundle-type single-walled carbon nanotubes (specific surface area 650 m2) consisting of single-walled carbon nanotube units with an average diameter of 1.5 nm and an average length of 5 μm or more 2 / g) and polyvinylidene fluoride (PVdF, KF9700, weight average molecular weight: 880,000 g / mol) were mixed in N-methylpyrrolidone (NMP) as a solvent to prepare a mixture having a solid content of 2.4 wt%.

[0124] The bundle-type single-walled carbon nanotubes were dispersed in the solvent by stirring the mixture by a bead mill method, and thus a carbon nanotube structure dispersion was prepared. In this case, the diameter of the beads was 1 mm, the rotation speed of the stirring container containing the beads was 3,000 RPM, and stirring was performed for 60 minutes. The carbon nanotube structure dispersion includes a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are connected side by side (see Figure 2 A).

[0125] In the carbon nanotube structure dispersion, the amount of the carbon nanotube structure was 0.4 wt %, and the amount of the polyvinylidene fluoride was 2.0 wt %.

[0126] Preparation Example 3: Preparation of Carbon Nanotube Structure Dispersion

[0127] A carbon nanotube structure dispersion was prepared in the same manner as in Preparation Example 2, except that the polyvinylidene fluoride in Preparation Example 2 was replaced with hydrogenated nitrile rubber (weight average molecular weight: 260,000 g / mol).

[0128] Preparation Example 4: Preparation of single-walled carbon nanotube unit dispersion

[0129] Bundle-type single-walled carbon nanotubes (specific surface area 650 m2) consisting of single-walled carbon nanotube units with an average diameter of 1.5 nm and an average length of 5 μm or more 2 / g) and hydrogenated nitrile rubber (weight average molecular weight: 260,000 g / mol) were mixed in N-methylpyrrolidone (NMP) as a solvent to prepare a mixture with a solid content of 4.4 wt% (0.4 wt% of bundle-type single-walled carbon nanotubes, 4 wt% of hydrogenated nitrile rubber).

[0130] By stirring the mixture by a bead mill method, the bundle-type single-walled carbon nanotubes were dispersed in the solvent, and thus a conductive agent dispersion was prepared. In this case, the diameter of the beads was 1 mm, the rotation speed of the stirring container containing the beads was 3,000 RPM, and stirring for 60 minutes under the above conditions was set as 1 cycle, and a total of 4 cycles were performed (natural cooling was performed for 60 minutes between each cycle). Thus, a single-walled carbon nanotube unit dispersion was prepared (see Figure 2 B). In the dispersion, since the bundle-type single-walled carbon nanotubes are completely dispersed, the single-walled carbon nanotube units exist only as single chain units, and the above-mentioned carbon nanotube structure is not detected. In addition, in the single-walled carbon nanotube unit dispersion, the amount of the carbon nanotube structure is 0.4% by weight, and the amount of the hydrogenated nitrile rubber is 4.0% by weight.

[0131] Preparation Example 5: Preparation of Multi-walled Carbon Nanotube Unit Dispersion

[0132] Bundle-type multi-walled carbon nanotubes, hydrogenated nitrile rubber (H-NBR) as a dispersant, and N-methylpyrrolidone (NMP) as a dispersion medium were mixed in a weight ratio of 4:0.8:95.2 to form a mixture. The mixture was added to a pin mill in which 80% was filled with beads having a diameter of 0.65 mm, dispersed, and discharged at a discharge rate of 2 kg / min. By performing this process twice, the bundle-type multi-walled carbon nanotubes were completely dispersed to prepare a multi-walled carbon nanotube unit dispersion (see Figure 1 A).

[0133] Examples and Comparative Examples

[0134] Example 1: Preparation of positive electrode

[0135] (1) Formation of the First Positive Electrode Active Material Layer

[0136] The carbon black dispersion of Preparation Example 1, LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and binder (PVDF-HFP, KF9700) were mixed with N-methylpyrrolidone (NMP) to prepare a first positive electrode slurry. The first positive electrode slurry was coated on a 20 μm thick aluminum (Al) film collector, dried at 130°C, and then rolled to form a first positive electrode active material layer.

[0137] 96.35 wt% LiNi 0.6 Co 0.2 Mn 0.2O2 (NCM622), 2.0 wt% of a binder, 0.15 wt% of hydrogenated nitrile rubber, and 1.5 wt% of carbon black were included in the first positive active material layer.

[0138] (2) Formation of the Second Positive Electrode Active Material Layer

[0139] The carbon nanotube structure dispersion of Preparation Example 2, LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and a binder (PVDF-HFP, KF9700) were mixed with N-methylpyrrolidone (NMP) to prepare a second positive electrode slurry. The second positive electrode slurry was coated on the first positive electrode active material layer, dried at 130°C, and then rolled to form a second positive electrode active material layer.

[0140] 98.39 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 1.51 wt% of polyvinylidene fluoride (PVDF), and 0.1 wt% of a carbon nanotube structure were included in the second positive active material layer.

[0141] Example 2: Preparation of positive electrode

[0142] A positive electrode was prepared in the same manner as in Example 1, except that when the second positive electrode active material layer was formed in Example 1, the carbon nanotube structure dispersion of Preparation Example 3 was used instead of the carbon nanotube structure dispersion of Preparation Example 2.

[0143] Example 3: Preparation of positive electrode

[0144] The positive electrode was prepared in the same manner as in Example 1, except that during the formation of the first positive electrode slurry in Example 1, the multi-walled carbon nanotube unit dispersion of Preparation Example 5 was used instead of the carbon black dispersion of Preparation Example 1. 97.16 wt % of LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 2.0 wt% of a binder, 0.14 wt% of hydrogenated nitrile rubber, and 0.7 wt% of a multi-walled carbon nanotube unit were included in the first positive active material layer.

[0145] Example 4: Preparation of positive electrode

[0146] The positive electrode was prepared in the same manner as in Example 1, except that during the formation of the first positive electrode slurry in Example 1, the carbon nanotube structure dispersion of Preparation Example 2 and the multi-walled carbon nanotube unit dispersion of Preparation Example 5 were used instead of the carbon black dispersion of Preparation Example 1. In the prepared first positive electrode active material layer, the weight ratio of the carbon nanotube structure to the multi-walled carbon nanotube was 0.05:0.65. 97.05 wt% of LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 2.13 wt% of a binder, 0.12 wt% of hydrogenated nitrile rubber, 0.05 wt% of a carbon nanotube structure, and 0.65 wt% of a multi-walled carbon nanotube unit were included in the first positive active material layer.

[0147] Example 5: Preparation of positive electrode

[0148] A positive electrode was prepared in the same manner as in Example 1, except that during the formation of the first positive electrode slurry in Example 1, the carbon nanotube structure dispersion of Preparation Example 2 was used instead of the carbon black dispersion of Preparation Example 1.

[0149] 97.75 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 2.15 wt% of polyvinylidene fluoride, and 0.1 wt% of a carbon nanotube structure were included in the first positive active material layer.

[0150] 98.45 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 1.45 wt% of polyvinylidene fluoride (PVDF), and 0.1 wt% of a carbon nanotube structure were included in the second positive active material layer.

[0151] Comparative Example 1: Preparation of positive electrode

[0152] The carbon nanotube structure dispersion of Preparation Example 2, LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and a binder (polyvinylidene fluoride: PVDF, KF9700) were mixed with N-methylpyrrolidone (NMP) to prepare a positive electrode slurry. The positive electrode slurry was coated on a 20 μm thick aluminum (Al) film collector, dried at 130°C, and then rolled to prepare a positive electrode including a positive electrode active material layer.

[0153] 98.1 wt% LiNi 0.6 Co0.2 Mn 0.2 O2 (NCM622), 1.8 wt% of polyvinylidene fluoride, and 0.1 wt% of a carbon nanotube structure were included in the positive electrode active material layer.

[0154] Comparative Example 2: Preparation of positive electrode

[0155] A positive electrode was prepared in the same manner as in Example 1, except that during the formation of the second positive active material layer in Example 1, the single-walled carbon nanotube unit dispersion of Preparation Example 4 was used instead of the carbon nanotube structure dispersion of Preparation Example 2.

[0156] 96.4 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 1.95 wt% of a binder, 0.15 wt% of hydrogenated nitrile rubber, and 1.5 wt% of carbon black were included in the first positive active material layer.

[0157] 98.5 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 0.4 wt% of a binder, 1.0 wt% of hydrogenated nitrile rubber, and 0.1 wt% of a single-walled carbon nanotube unit were included in the second positive active material layer.

[0158] Comparative Example 3: Preparation of positive electrode

[0159] A positive electrode was prepared in the same manner as in Example 1, except that during the formation of the second positive electrode active material layer in Example 1, the multi-walled carbon nanotube unit dispersion of Preparation Example 5 was used instead of the carbon nanotube structure dispersion of Preparation Example 2.

[0160] 96.35 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 2.0 wt% of a binder, 0.15 wt% of hydrogenated nitrile rubber, and 1.5 wt% of carbon black were included in the first positive active material layer.

[0161] 97.84 wt% LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), 1.32 wt% of polyvinylidene fluoride, 0.14 wt% of hydrogenated nitrile rubber, and 0.7 wt% of multi-walled carbon nanotube units were included in the second positive electrode active material layer.

[0162] [Table 1]

[0163]

[0164] In Examples 1 to 5 and Comparative Example 1, the average diameter of the carbon nanotube structure was 100 nm, and the average length thereof was 15.6 μm. In Example 2, the average diameter of the carbon nanotube structure was 10 nm, and the average length thereof was 8.2 μm. In Comparative Example 2, the average diameter of the single-walled carbon nanotube unit was 1.6 nm, and the average length thereof was 1.8 μm.

[0165] In the positive electrodes of Examples 3 and 4 and Comparative Example 3, the average diameter of the multi-walled carbon nanotube units was 10.8 nm, and the average length thereof was 1.3 μm.

[0166] When the prepared positive electrode is observed by TEM, the average diameter and the average length correspond to the average value of the diameters (or lengths) of the first 100 carbon nanotube structures (or multi-walled carbon nanotube units, or single-walled carbon nanotube units) with larger diameters (or lengths) and the last 100 carbon nanotube structures (or multi-walled carbon nanotube units, or single-walled carbon nanotube units) with smaller diameters (or lengths).

[0167] Test Example 1: Observation of the positive electrode

[0168] When the second positive electrode active material layer of Example 1 was observed by SEM, it was confirmed that the rope-like carbon nanotube structure (a form in which 2 to 5,000 single-walled carbon nanotube units are arranged side by side and bonded to each other) together formed a network structure while having a long and thick shape to connect the NCM622 particles to each other (see Figure 3 ). In addition, for the positive electrode of Example 1, it can be understood that there is clearly an interface separating the first positive electrode active material layer and the second positive electrode active material layer (see Figure 4 ).

[0169] In contrast, when the second positive electrode active material layer of Comparative Example 3 was observed by SEM, multi-walled carbon nanotube units having very short lengths were arranged on the surface of the NCM622 particles, but a long and thick structure such as the above-mentioned carbon nanotube structure was not recognized (see Figure 5 ).

[0170] In addition, when the second positive electrode active material layer of Comparative Example 2 was observed by SEM, single-walled carbon nanotube units having a shorter length were arranged in a layer on the surface of the NCM622 particles, but a long and thick structure such as the above-mentioned carbon nanotube structure was not recognized (see Figure 6 ).

[0171] Test Example 2: Evaluation of positive electrode adhesion

[0172] The positive electrode adhesion was measured under dry conditions. Specifically, after the double-sided tape was attached to the slide glass and the positive electrode punched into a size of 20 mm × 180 mm was placed on it, a 2 kg roller was reciprocated 10 times to attach the electrode to the tape, and then the electrode was pulled at a speed of 200 mm / min using a universal testing machine (UTM, TA Instruments) to measure the force of separation from the slide glass. In this case, the measurement angle between the slide glass and the positive electrode was 90 °. The measurement results are listed in Table 2 below.

[0173] Test Example 3: Evaluation of Adhesion Between the First Positive Electrode Active Material Layer and the Second Positive Electrode Active Material Layer

[0174] The shear strength (N / mm) of Examples 1 to 5 and Comparative Examples 2 and 3 was measured by the following method 2 ). The shear strength was measured using SAICAS (Surface and Interfacial Characterization Analysis System) (SAICAS EN-EX (Daipla Wintes, Japan)), and the shear strength was determined based on the force applied to the knife while the positive electrode was cut obliquely in the depth direction with a diamond microknife. The measured data is the shear strength at a position of 1 / 2 of the total thickness of the positive electrode (near the interface between the first positive electrode active material layer and the second positive electrode active material layer and at a depth of about 50 μm), and the results are shown in Table 2 below.

[0175] Test Example 4: Electrical conductivity evaluation

[0176] The resistance of each positive electrode was measured by using a Multi-Probe electrode resistance measurement system (Hioki EE Co., Ltd., RM-2610 model), and the positive electrode resistance was divided into the volume resistance of the positive electrode active material layer (Ω·cm) and the interface resistance between the active material layer and the current collector (Ω·cm 2 ) and measured by using the corresponding system.

[0177] Test Example 5: Evaluation of Capacity Retention and Discharge Capacity Based on C-Rate

[0178] Batteries were prepared by using the positive electrodes of Examples 1 to 5 and Comparative Examples 1 to 3, respectively, as follows.

[0179] Artificial graphite as a negative electrode active material, carbon black as a negative electrode conductive agent, styrene butadiene rubber (SBR) as a negative electrode binder, and carboxymethyl cellulose (CMC) were mixed in distilled water at a weight ratio of 96.1:0.5:2.3:1.1 to prepare a negative electrode slurry. A 20 μm thick negative electrode collector (Cu) was coated with the prepared slurry so that the loading amount was 10 mg / cm2 , and dried. Thereafter, the negative electrode current collector on which the negative electrode slurry was arranged was rolled by a rolling method so that the total thickness of the negative electrode slurry and the negative electrode current collector was 80 μm. Thereafter, the negative electrode slurry and the negative electrode current collector were dried at 110° C. for 6 hours to prepare a negative electrode.

[0180] Afterwards, after preparing a single cell by assembling the above-prepared negative electrode and the above-prepared positive electrode with a 15μm thick polyethylene-based separator arranged therebetween, an electrolyte (ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 1 / 2 (volume ratio)) and lithium hexafluorophosphate (1M LiPF6) are injected into the single cell to prepare a lithium secondary battery.

[0181] 1) Evaluate discharge capacity based on C rate

[0182] The charge C rate was fixed at 0.2C, and the discharge C rate was increased from 0.2C to 2.0C. The 2.0C discharge capacity (%) relative to the 0.2C discharge capacity was measured for each lithium secondary battery. The results are shown in Table 2.

[0183] 2) Evaluation of capacity retention rate (lifetime characteristics)

[0184] Charging and discharging of each lithium secondary battery was performed under the following conditions.

[0185] Each lithium secondary battery was set to charge / discharge at 0.33C / 0.33C in a voltage range of 4.25V to 2.8V at 45°C as one cycle, and a total of 100 cycles were performed. Thereafter, the discharge capacity (capacity retention rate) after 100 cycles was evaluated based on the discharge capacity after 1 cycle being 100%, and is shown in Table 2.

[0186] [Table 2]

[0187]

[0188] The following content corresponds to the original claims in the parent application and is now incorporated herein as part of the specification:

[0189] 1. A positive electrode, comprising: a positive electrode current collector, a first positive electrode active material layer disposed on the positive electrode current collector and comprising a first positive electrode active material, and a second positive electrode active material layer disposed on the first positive electrode active material layer;

[0190] The second positive electrode active material layer comprises:

[0191] a second positive electrode active material; and

[0192] A carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are linked side by side.

[0193] The carbon nanotube structure is included in the second positive electrode active material layer in an amount of 0.01 wt % to 1.0 wt %.

[0194] 2. The positive electrode according to item 1, wherein the carbon nanotube structures are connected to each other in the second positive electrode active material layer to form a network structure.

[0195] 3. The positive electrode according to item 1, wherein in the carbon nanotube structure,

[0196] The single-walled carbon nanotube units are arranged and combined side by side.

[0197] 4. The positive electrode according to item 1, wherein the average length of the carbon nanotube structure is 1 μm to 500 μm.

[0198] 5. The positive electrode according to item 1, wherein the average length of the carbon nanotube structure is 10 μm to 70 μm.

[0199] 6. The positive electrode according to item 1, wherein the average diameter of the carbon nanotube structure is 2 nm to 200 nm.

[0200] 7. The positive electrode according to item 1, wherein the average diameter of the carbon nanotube structure is 50 nm to 120 nm.

[0201] 8. The positive electrode according to item 1, wherein in the carbon nanotube structure, the average diameter of the single-walled carbon nanotube unit is 0.5 nm to 5 nm.

[0202] 9. The positive electrode according to item 1, wherein the carbon nanotube structure is a carbon nanotube structure in which 50 to 4,000 single-walled carbon nanotube units are bonded to each other.

[0203] 10. The positive electrode according to item 1, wherein the first positive electrode active material layer comprises the first positive electrode active material and a first conductive agent, and

[0204] The first conductive agent includes at least one selected from the group consisting of the carbon nanotube structure, a multi-walled carbon nanotube unit, and carbon black.

[0205] 11. The positive electrode according to item 1, wherein the thickness of the first positive electrode active material layer is 1 μm to 100 μm.

[0206] 12. The positive electrode according to item 1, wherein the second positive electrode active material layer has a thickness of 1 μm to 100 μm.

[0207] 13. A secondary battery comprising the positive electrode according to any one of items 1 to 12.

Claims

1. A positive electrode, the positive electrode include: A positive electrode current collector, a first positive electrode active material layer disposed on the positive electrode current collector, and a second positive electrode active material layer disposed on the first positive electrode active material layer; wherein the first positive electrode active material layer comprises a first positive electrode active material; The second positive electrode active material layer comprises: a second positive electrode active material; and A carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are linked side by side. The thickness of the second positive electrode active material layer is greater than or equal to the thickness of the first positive electrode active material layer. 2 . The positive electrode according to claim 1 , wherein the carbon nanotube structures are connected to each other in the second positive electrode active material layer to form a network structure.

3. The positive electrode according to claim 1, in, In the carbon nanotube structure, The single-walled carbon nanotube units are arranged and combined side by side. The positive electrode according to claim 1 , wherein the carbon nanotube structure has an average length of 1 μm to 500 μm. 5 . The positive electrode according to claim 1 , wherein an average length of the carbon nanotube structure is 10 μm to 70 μm. The positive electrode according to claim 1 , wherein the average diameter of the carbon nanotube structure is 2 nm to 200 nm. 7 . The positive electrode according to claim 1 , wherein an average diameter of the carbon nanotube structure is 50 nm to 120 nm.

8. The positive electrode according to claim 1, in, In the carbon nanotube structure, the average diameter of the single-walled carbon nanotube unit is 0.5 nm to 5 nm. 9 . The positive electrode according to claim 1 , wherein the carbon nanotube structure is a carbon nanotube structure in which 50 to 4,000 single-walled carbon nanotube units are bonded to each other.

10. The positive electrode according to claim 1, wherein the first positive electrode active material layer comprises the first positive electrode active material and a first conductive agent, and The first conductive agent includes at least one selected from the group consisting of the carbon nanotube structure, a multi-walled carbon nanotube unit, and carbon black. 11 . The positive electrode according to claim 1 , wherein the first positive electrode active material layer has a thickness of 1 μm to 100 μm. 12 . The positive electrode according to claim 1 , wherein the second positive electrode active material layer has a thickness of 1 μm to 100 μm. 13 . The positive electrode according to claim 1 , wherein a ratio of a thickness of the first positive electrode active material layer to a thickness of the second positive electrode active material layer is in a range of 10:90 to 50:

50. 14 . A secondary battery comprising the positive electrode according to claim 1 .

Citation Information

Patent Citations

  • Discoloration alloy wheel

    KR1020190123144A