Lithium ion battery

By using silicon oxide-based glass filler in the resin components of lithium-ion batteries and adding magnesium or calcium, the problem of deterioration of resin components in the fluorine-containing non-aqueous electrolyte is solved, and the durability and sealing performance are improved, ensuring that the battery is in Stability in fluorine-containing environment.

CN119009065APending Publication Date: 2024-11-22PRIME PLANET ENERGY & SOLUTIONS INC +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410453621.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-04-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In lithium-ion batteries, when a fluorine-containing nonaqueous electrolyte is used, the resin member is prone to deterioration due to the formation of hydrogen fluoride, especially when moisture is mixed, the dissolution of the glass filler leads to a decrease in the durability of the resin member.

Method used

By using glass filler mainly composed of silicon oxide in the resin member and adding a second group element, such as magnesium or calcium, to it, the linear expansion coefficient and elastic modulus are adjusted to make it close to the performance of the shell while suppressing the performance of the shell. The dissolution of the glass filler by hydrogen fluoride maintains the durability of the resin member.

Benefits of technology

Even in the non-aqueous electrolyte containing fluorine, the deterioration rate of the resin member does not accelerate, and the insulation performance and sealing performance are maintained for a long time, and the service life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009065A_ABST
    Figure CN119009065A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium ion battery. The battery is a lithium ion battery having a case, an electrode body and an electrolyte solution housed inside the case, and a resin member fixed to the case and having an inner exposed surface exposed inside the case, the electrolyte solution being a fluorine-containing non-aqueous electrolyte solution, the resin member containing a glass filler, the glass filler is composed of glass mainly composed of silicon oxide and added with a second group element, and the atomic ratio of the second group element to silicon in the component elements of the glass filler is 0.12%-65% (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The disclosed technology relates to lithium-ion batteries. Background Art

[0002] In a lithium-ion battery, an electrode body and an electrolyte are contained inside a shell. A resin member is fixed to a portion of the shell in such a battery for purposes such as the installation of a terminal member. A portion of the resin member is an internal exposed surface exposed inside the shell. As the resin member, a resin member to which a glass filler is added can be used. As such a resin to which a filler is added, for example, a resin described in Patent Document 1 can be used.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-035950 Summary of the invention

[0006] Problems to be solved by the invention

[0007] As the electrolyte in this battery, a fluorine-containing non-aqueous electrolyte is sometimes used. In this case, the resin to which the filler is added sometimes deteriorates. When water is mixed into the non-aqueous electrolyte, the resin to which the filler is added deteriorates. This is because the fluorine in the non-aqueous electrolyte reacts with the mixed water to generate hydrogen fluoride. Hydrogen fluoride dissolves the glass, so the glass filler dissolves and is lost.

[0008] An object of the disclosed technology is to provide a lithium ion battery in which degradation of a resin member is not accelerated even when a non-aqueous electrolyte containing fluorine is used.

[0009] Means for solving problems

[0010] A lithium-ion battery according to one embodiment of the disclosed technology is a battery comprising a shell, an electrode body and an electrolyte contained in the shell, and a resin member, wherein the resin member is fixed to the shell and has an internal exposure surface exposed in the shell, the electrolyte is a fluorine-containing non-aqueous electrolyte, and the resin member contains a glass filler, wherein the glass filler is formed of glass mainly composed of silicon oxide and to which a second group element is added, and the atomic number ratio of the second group element to silicon in the component elements of the glass filler is greater than 0.12% and less than 65%.

[0011] In the lithium-ion battery of the above scheme, the linear expansion coefficient and elastic modulus are adjusted by adding a glass filler to the resin member. Therefore, the linear expansion coefficient and elastic modulus of the resin member can be made close to the linear expansion coefficient and elastic modulus of the shell. On the other hand, if water is mixed into the electrolyte, the hydrogen fluoride generated by the reaction of fluorine in the electrolyte with water will dissolve the glass filler. However, the second group element added to the glass filler inhibits this dissolution. Therefore, even if water is mixed, the characteristics of the resin member are maintained.

[0012] In the lithium ion battery of the above embodiment, at least a portion of the Group II element can be magnesium, and the mass ratio of magnesium to silicon in the component elements of the glass filler is 0.1% to 25%. If magnesium is used as the Group II element, the effect of suppressing the dissolution of the glass filler by hydrogen fluoride is higher.

[0013] In the lithium ion battery of the above embodiment, at least part of the Group II element may be calcium, and the mass ratio of calcium to silicon in the glass filler is 0.17% to 81%. When the Group II element is calcium, it also has the effect of suppressing the dissolution of the glass filler by hydrogen fluoride.

[0014] In the lithium ion battery of any of the above schemes, a terminal member is further provided, the terminal member being connected to the electrode body inside the housing and being provided through the housing and partially exposed outside the housing, and the resin member insulates the housing from the terminal member. In this way, the insulation performance and sealing performance of the resin member between the housing and the terminal member are maintained for a long time.

[0015] Effects of the Invention

[0016] According to the technology disclosed in the present invention, there is provided a lithium ion battery in which degradation of a resin member is not accelerated even when a nonaqueous electrolyte solution containing fluorine is used. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a cross-sectional view of a battery according to an embodiment.

[0018] Figure 2 For the general Figure 1 An enlarged view of a portion of the diagram is shown.

[0019] Figure 3 Graph showing the maximum depth of corrosion of the glass filler due to immersion in the electrolyte.

[0020] Figure 4 It is a graph showing the change in elastic modulus of the resin member due to immersion in the electrolyte solution.

[0021] Figure 5It is a graph showing the relationship between the penetration depth of fluorine due to immersion in the electrolyte and the temperature.

[0022] Description of Reference Numerals

[0023] 1 Battery

[0024] 2 Housing

[0025] 3 Electrode body

[0026] 4 Cabinet

[0027] 5 Cover

[0028] 6 Electrolyte

[0029] 7 Terminal components

[0030] 10 Resin components

[0031] 11 Internal exposed surface DETAILED DESCRIPTION

[0032] This form is as Figure 1 and Figure 2 The battery 1 shown is a product that embodies the disclosed technology. The battery 1 contains an electrode body 3 in a shell 2. The shell 2 is an outer packaging member that forms the appearance of the battery 1. In this form, the shell 2 is made of metal (such as aluminum). The shell 2 is composed of a box body 4 and a cover body 5. The electrode body 3 is a product of stacking positive and negative electrode plates.

[0033] The shell 2 contains not only the electrode body 3 but also the electrolyte 6. The electrolyte 6 not only exists as a liquid electrolyte in the internal space of the shell 2 but also permeates the electrode body 3. The battery 1 also includes a terminal member 7. The terminal member 7 is provided to penetrate the shell 2. The terminal member 7 is partially exposed to the outside of the shell 2. The portion of the terminal member 7 on the inner side of the shell 2 is connected to the electrode body 3. The portion of the terminal member 7 on the outer side of the shell 2 is connected to the external terminal 8. The battery 1 has two terminal members 7 for the positive electrode and the negative electrode and two external terminals 8. The terminal member 7 and the external terminal 8 are made of aluminum or copper.

[0034] A through hole 9 is formed in the cover 5 and penetrates the terminal member 7. The battery 1 further includes a resin member 10. The resin member 10 is fixed to the housing 2. The position where the resin member 10 is fixed in the housing 2 is between the cover 5 and the terminal member 7 at the through hole 9. The functions of the resin member 10 are to separate the internal space of the housing 2 from the external space and to insulate the housing 2 from the terminal member 7. The resin member 10 has an internal exposed surface 11 exposed inside the housing 2.

[0035] The electrolyte solution 6 in the battery 1 of this embodiment will be described. In this embodiment, a non-aqueous electrolyte solution containing fluorine is used as the electrolyte solution 6. The following substances can be mentioned as the solvent and electrolyte in the electrolyte solution 6 of this embodiment.

[0036] Solvent: Polar organic solvents such as ethylene carbonate, propylene carbonate, diethyl carbonate, etc.

[0037] Electrolyte: fluoride-containing salts such as lithium hexafluorophosphate and lithium tetrafluoroborate

[0038] The resin component 10 in the battery 1 of this form is explained. The resin component 10 of this form is a composite material in which a glass filler is mixed with a base resin. The purpose of mixing the glass filler is to adjust the linear expansion coefficient and elastic modulus of the resin component 10. The so-called adjustment of the linear expansion coefficient is to reduce the linear expansion coefficient of the resin component 10. It is to approach the degree of the linear expansion coefficient of metal parts such as the cover body 5 and the terminal component 7. The so-called adjustment of the elastic modulus is to increase the elastic modulus of the resin component 10. All of them contribute to improving the durability of the sealing performance of the resin component 10 in the battery 1.

[0039] The type of resin that can be used as the base resin of the resin member 10 of this embodiment is not particularly limited, but resins with excellent heat resistance and mechanical strength are preferred. For example, polyphenylene sulfide resin (hereinafter referred to as PPS resin), polyphenylene ether resin, modified polyphenylene ether resin, etc. are listed.

[0040] The glass filler of the resin component 10 of this form is a tiny piece formed of glass. The shape is short fiber or granular. The glass used in the glass filler of this form is a product with silicon oxide (silicon dioxide, etc.) as the main body and a second group element (especially magnesium or calcium) added thereto. It is believed that the added second group element becomes an oxidized state in the glass. Sometimes, a small amount of aluminum for improving productivity, titanium and iron for improving acid resistance are also contained in the glass in an oxidized state.

[0041] In this embodiment, the purpose of adding the second group element to the glass filler is to improve the durability of the resin member 10. In this embodiment, as described above, a fluorine-containing salt is used as an electrolyte of the electrolytic solution 6. Therefore, the electrolytic solution 6 contains fluorine in the form of, for example, hexafluorophosphate ions.

[0042] On the other hand, during the manufacturing process of the battery 1, a certain amount of moisture may be mixed into the interior of the housing 2 due to water vapor in the environment. Even during the use of the battery 1, if the airtightness of the housing 2 is loose, moisture may sometimes penetrate from the outside to the inside. Therefore, even if the electrolyte 6 is a non-aqueous solvent-based electrolyte, it cannot necessarily be said that there is no moisture at all.

[0043] As water is mixed into the electrolyte 6, the fluorine in the electrolyte 6 takes hydrogen from the water molecules to generate hydrogen fluoride. The generation of hydrogen fluoride is the main factor that hinders the originally envisioned durability of the resin component 10. The reason is that glass is generally a compound with high chemical stability, but is decomposed by hydrogen fluoride. Therefore, if the hydrogen fluoride generated in the electrolyte 6 contacts the internal exposed surface 11 of the resin component 10, the glass filler in the resin component 10 is attacked by hydrogen fluoride. Since the glass filler is dissolved from the resin component 10, the linear expansion coefficient and elastic modulus of the resin component 10 are close to the linear expansion coefficient and elastic modulus of the original base resin. In this way, the resin component 10 deteriorates earlier than expected.

[0044] However, in this embodiment, the Group II element added to the glass filler prevents the dissolution of the glass caused by hydrogen fluoride. This is because hydrogen fluoride attacks the Group II element preferentially compared to silicon oxide. That is, the Group II element captures hydrogen fluoride and protects silicon oxide from the attack of hydrogen fluoride. The Group II element itself becomes a fluoride by capturing hydrogen fluoride. In addition, water is generated at this time.

[0045] Therefore, the presence of the second group element suppresses the dissolution of the glass caused by hydrogen fluoride. Thus, the originally envisioned durability of the resin member 10 is maintained. Therefore, in the battery 1 of this form, even if moisture intrudes into the housing 2, the durability of the resin member 10 is hardly reduced. Therefore, in this form, the insulation and airtightness between the cover 5 and the terminal member 7 brought about by the resin member 10 are maintained for a long time.

[0046] As for the amount of the second group element in the glass filler, it is preferred that the atomic ratio of the second group element to silicon in the component elements is 0.12% or more and 65% or less. In the case of containing multiple second group elements (such as magnesium and calcium), the amount is the total amount. If the amount of the second group element is insufficient, the effect of improving the durability becomes insufficient. If the amount of the second group element is excessive, there is a disadvantage that the glass productivity is reduced, such as being difficult to form into short fibers.

[0047] When at least a part of the Group II element is magnesium, its blending amount is preferably 0.1% or more and 25% or less, expressed as a mass ratio to silicon. When at least a part of the Group II element is calcium, its blending amount is preferably 0.17% or more and 81% or less, expressed as a mass ratio to silicon.

[0048] The present inventors conducted a test to evaluate the durability of the resin member 10 of this embodiment, and the results are described below. Here, the evaluations used to describe the results are the following two evaluations.

[0049] Depth of corrosion after durability

[0050] Changes in elastic modulus before and after durability

[0051] The following two types of resins to which fillers were added were each prepared into a plate-shaped sample having a thickness of 1 mm and used for these tests.

[0052] (Example)

[0053] Base resin: PPS resin

[0054] Glass filler material: magnesium (1.9% to 25% by mass relative to silicon)

[0055] Shape of glass filler: short fiber (10μmφ×0.3mm long)

[0056] (Comparative Example)

[0057] Base resin: same as above

[0058] Glass filler material: no second group elements

[0059] Shape of glass filler: same as above

[0060] In the test, samples of these resin members were immersed in an electrolyte solution under the following conditions.

[0061] Type of electrolyte solvent: A mixture of ethylene carbonate and diethyl carbonate (mass ratio 1:1)

[0062] Electrolyte type and concentration: Lithium hexafluorophosphate, 1 mol / L

[0063] Water content: 1200ppm (equivalent to 25 years after the battery is used)

[0064] The electrolyte temperature during immersion: 25°C, 65°C, 80°C

[0065] Immersion time: 20 days

[0066] In the evaluation of the corrosion depth after durability, the corrosion condition of the glass filler in the sample after immersion was evaluated. Specifically, in the cross section of the sample, the maximum depth of the surface where the glass filler completely disappeared was evaluated. The surface of the sample is the surface corresponding to the internal exposed surface 11 of the resin member 10. This evaluation was performed by observing the cross section of the sample with a scanning electron microscope. The results are as follows: Figure 3 As shown. Figure 3 In the figure, the maximum corrosion depth after immersion (vertical axis) is shown in comparison between the examples and the comparative examples according to the above three levels of immersion temperature.

[0067] Depend on Figure 3 The following can be explained.

[0068] In general, the higher the immersion temperature, the deeper the corroded area.

[0069] Under all temperature conditions, the corrosion depth of the examples is smaller than that of the comparative examples. In addition, the corrosion depth of the examples immersed at 25°C is zero.

[0070] Thus, by Figure 3 It is found that in the examples containing magnesium, the corrosion of the glass filler is suppressed under all temperature conditions compared to the comparative examples not containing magnesium. This is considered to be because the magnesium added in the examples suppresses the dissolution of the glass by hydrogen fluoride.

[0071] In the evaluation of the change in elastic modulus before and after endurance, the elastic modulus of the sample after immersion was evaluated to what extent it decreased relative to the elastic modulus of the sample before immersion. Therefore, the elastic modulus of the sample before immersion and the sample after immersion were measured, and the reduction rate was calculated. The results are as follows: Figure 4 shown. Figure 4 The vertical axis in the figure is based on the elastic modulus of the sample before immersion, and negative values ​​are used to represent the ratio of the decrease in the elastic modulus of the sample after immersion compared to the reference. Figure 4 The decrease in elastic modulus due to immersion becomes more significant as the thickness goes down. Figure 4 In the embodiment and the comparative example, the results are shown in comparison according to three levels of the temperature during immersion.

[0072] Depend on Figure 4 The following can be explained.

[0073] Generally, there is a tendency that the higher the temperature during immersion, the greater the degree of decrease in elastic modulus due to immersion.

[0074] Under all temperature conditions, the degree of decrease in elastic modulus was smaller in Examples than in Comparative Examples.

[0075] Thus, by Figure 4 It can be seen that in the examples in which magnesium was added, the decrease in elastic modulus due to impregnation was suppressed under all temperature conditions compared to the comparative examples in which magnesium was not added. This is considered to be because the dissolution of glass due to hydrogen fluoride was suppressed by the magnesium added in the examples. That is, it can be seen that in the comparative examples, a large amount of glass filler was lost due to impregnation, while in the examples, the glass filler was maintained to a considerable extent even after impregnation.

[0076] The inventors of the present invention have further conducted tests on the intrusion of fluorine caused by the immersion of the resin component 10 of this form in the electrolyte. As this test, a resin containing the glass fillers of the four components in Table 1 was used as a sample. The shape of the sample is the same as described above. The values ​​in the "mass %" column in Table 1 represent the mass ratio of each element relative to the mass of the entire glass including oxygen, etc. The values ​​in the "mass ratio (%)" column represent the relative mass ratio of each element in the glass. The values ​​in the "atomic ratio (%)" column are the products of converting the mass ratio values ​​into atomic ratios based on the atomic weights of each element.

[0077]

Table 1

[0078]

[0079] Among the four samples in Table 1, sample A contains only calcium as a Group II element but no magnesium. Samples B to D contain both magnesium and calcium as Group II elements. Among them, in sample B, the amount of calcium added is near the upper limit of the above-mentioned preferred range in terms of mass ratio, and the total amount of magnesium and calcium added is near the upper limit of the above-mentioned preferred range in terms of atomic ratio. In sample C, the amount of magnesium added is near the upper limit of the above-mentioned preferred range in terms of mass ratio, and the amount of magnesium added and the amount of calcium added are approximately equal in terms of atomic ratio. In sample D, compared with sample C, the total amount of magnesium added and the amount of calcium added in terms of atomic ratio are approximately equal, but the amount of magnesium added is reduced and the amount of calcium added is increased.

[0080] These four samples were immersed in an electrolyte, and the penetration depth of fluorine in the samples after the immersion was measured. For each type, multiple samples were provided for measurement. As an electrolyte, the same electrolyte as that described in the description of the above test was used. In the measurement of the penetration depth of fluorine, a scanning electron microscope with an X-ray elemental analyzer was used. That is, the cross-section of the sample after immersion was observed with the electron microscope, and the distribution of fluorine was mapped using an X-ray elemental analyzer, and the maximum depth from the surface to the detection of fluorine was measured. It is an indicator different from the above-mentioned "erosion depth", and is generally a value greater than the "erosion depth" under the same conditions.

[0081] Figure 5 The relationship between the measured penetration depth of fluorine and the temperature of the electrolyte during immersion is shown in a graph. Figure 5 The vertical axis is the penetration depth. The deeper it goes, the less penetration there is, and the better the resistance to the electrolyte. Figure 5 In the measurement, the immersion temperature was set at 4 levels: 25°C, 40°C, 60°C, and 80°C. The immersion time was 20 days. Five samples were prepared for each temperature level and each sample type, and the immersion and subsequent measurements were performed, and the maximum penetration depth in each sample was recorded.

[0082] Depend on Figure 5 It can be seen that there is a tendency that the higher the temperature during immersion, the greater the penetration depth of fluorine. In addition, among the four samples, sample A without magnesium tends to have a greater penetration depth than samples B to D containing magnesium. Therefore, it is believed that among the second group elements, magnesium is more effective than other second group elements. However, when there is no second group element at all, fluorine penetrates to Figure 5 Since the depth is outside the range of the vertical axis, it can be said that sample A also suppresses the invasion of fluorine compared with the latter.

[0083] As described in detail above, according to the present embodiment, in the battery 1 containing fluorine in the electrolyte 6, a composite material to which a glass filler to which a second group element is added is used as the resin member 10 to seal the through hole 9 passing through the terminal member 7. Thus, even if water is mixed into the electrolyte 6, the degradation of the resin member 10 caused by it is suppressed. That is, by adding the second group element to the glass filler, the durability of the resin member 10 is improved. In this way, a lithium ion battery 1 is realized in which the degradation of the resin member 10 is not accelerated even when a non-aqueous electrolyte 6 containing fluorine is used.

[0084] The present embodiment and examples are merely illustrative and do not limit the present invention in any way. Therefore, the present invention can be modified and altered in various ways without departing from the main purpose. For example, in the above embodiment, the battery 1 as the object of application of the present invention can be listed as follows: Figure 1 The battery shown is a flat square shape. However, it is not limited to this, and the disclosed technology can also be applied to batteries of other shapes such as cylindrical shapes.

[0085] In addition, in the above-mentioned form, as the applicable part of the present technology, i.e., the resin component 10, a resin component that insulates the terminal component 7 and the cover body 5 can be listed. However, it is not limited to this, and the present technology can also be applied to resin materials in other places in the battery. As resin materials in other places, for example, the sealing resin when the liquid injection port is sealed with a resin material can be listed. In addition, the box body 4 in the shell 2 can be an insulator, so the box body 4 itself can be composed of a resin component to which the present technology is applied. In addition, as a sealing resin between the cylindrical shell and the circular cover in a cylindrical battery, the resin component of the present technology can be used.

[0086] In the above embodiment, the terminal member 7 is connected to the external terminal 8 on the outside of the housing 2. However, the terminal member 7 and the external terminal 8 may be integrally formed. On the inside of the housing 2, the terminal member 7 is not limited to being directly connected to the electrode body 3 at one end, and may be indirectly connected via another current collecting member.

Claims

1. A lithium-ion battery comprising a housing; an electrode body and an electrolyte solution contained in the housing; and a resin member, the resin member being fixed to the housing and having an inner exposed surface exposed in the housing, The electrolyte is a fluorine-containing non-aqueous electrolyte, and the resin component contains a glass filler, which is formed by glass mainly composed of silicon oxide and added with a second group element. The atomic ratio of the second group element to silicon in the component elements of the glass filler is greater than 0.12% and less than 65%.

2. The lithium ion battery according to claim 1, wherein At least a part of the Group 2 elements is magnesium, and a mass ratio of magnesium to silicon in component elements of the glass filler is 0.1% or more and 25% or less.

3. The lithium ion battery according to claim 1, wherein At least a part of the Group 2 elements is calcium, and a mass ratio of calcium to silicon in component elements of the glass filler is 0.17% or more and 81% or less.

4. The lithium ion battery according to any one of claims 1 to 3, comprising a terminal member, wherein the terminal member is connected to the electrode body inside the shell, and is provided through the shell and partially exposed outside the shell, and the resin member insulates the shell from the terminal member.