Rapid preparation method of transition metal boride

CN119013229APending Publication Date: 2024-11-22KUNMING UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380008983.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing preparation methods of transition metal borides are complicated, take a long time, have a great impact on the environment, and have problems with changes in chemical composition and impurity contamination.

Method used

Using the DC arc method, the tungsten rod, boron powder and metal oxide mixture are placed in the electric arc furnace as the anode and cathode, and the transition metal boride is quickly prepared through the arc combustion reaction, and the arc discharge parameters such as current, time and atmosphere are controlled to achieve Simple, low-cost and environmentally friendly preparation process.

Benefits of technology

The rapid and pure preparation of transition metal borides is achieved, the process flow is simplified, the environmental impact is reduced, and the preparation efficiency and product purity are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013229A_ABST
    Figure CN119013229A_ABST
Patent Text Reader

Abstract

The invention relates to a rapid preparation method of transition metal boride, and the preparation method comprises the following steps: taking a tungsten rod as a cathode, taking a mixture of boron powder and metal oxide which are pressed into blocks as an anode, and putting the block mixture and the tungsten rod into an electric arc furnace; and the electric arc furnace is vacuumized, then buffer gas is filled, the electric arc furnace is controlled to start an electric arc, the electric arc furnace is controlled to close the electric arc after the blocky mixture is ignited, and the blocky mixture is subjected to continuous combustion reaction to obtain the transition metal boride. The transition metal boride is prepared by adopting a direct-current arc plasma method which has the advantages of simplicity in operation, low cost, environment friendliness, controllable reaction atmosphere and the like, the preparation process is simple, the preparation process is quick, and the environment is not influenced.
Need to check novelty before this filing date? Find Prior Art

Description

A rapid preparation method for transition metal borides Technical Field

[0001] The invention relates to a rapid preparation method of transition metal boride, and belongs to the field of preparing nano materials using a direct current arc method. Background Art

[0002] In recent years, transition metal borides (TMBs) have attracted significant interest due to their unique mechanical and electrical properties. These compounds, characterized by their high bulk modulus, high hardness, ultrahigh melting point, good thermal stability, strong oxidation resistance, and excellent electrical transmission properties, have been widely used in scramjet and rocket propulsion, hypersonic flight, atmospheric reentry, hard coatings for electromechanical systems, armor, and cutting tools. For example, titanium diboride (TMB) is an emerging engineering ceramic material, characterized by high hardness, high elastic modulus, high melting point, excellent wear resistance, and excellent thermal and electrical conductivity. Baharvandi et al. synthesized B4C-TiB2 composite ceramics using B4C and TiB2 as raw materials by pressureless sintering at 2050 / 2150°C. The addition of TiB2 reduced porosity and inhibited grain growth. At the same TiB2 content, higher synthesis temperatures resulted in improved density.

[0003] Common methods for preparing transition metal borides include reducing a mixture of boron halide and metal halide with hydrogen, reducing a mixture of boron trioxide and metal oxide with carbon, and reducing metal oxides with electrolytic molten salt and elemental boron. Although these methods have been widely used to prepare metal borides, they present some challenges. For example, reducing a mixture of boron halide and metal halide with hydrogen, where the mixture is pyrolyzed on a metal wire in hydrogen, can produce small amounts of very pure metal borides. Reducing a mixture of boron trioxide and metal oxide with carbon can produce larger quantities of metal borides. However, due to the varying volatility of the various oxides at high temperatures, chemical composition changes can occur, and the product is likely to be contaminated by intermediate boron, boron carbide, and carbon. The electrolytic molten salt method can produce many metal borides, some of which have reached industrial production levels. However, the current efficiency is low, several boride phases may be generated, and the product is difficult to separate purely from the molten salt; in addition, the preparation time of the above methods is very long, and some require additional treatment of impurities generated during the preparation process.

[0004] Therefore, the existing technology still needs to be improved and developed.

[0005] Summary of the Invention

[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of this application is to provide a rapid preparation method for transition metal borides, aiming to solve the technical problems of the existing transition metal boride preparation process being complex and having a great impact on the environment.

[0007] The technical solution of the rapid preparation method of a transition metal boride of the present invention is as follows:

[0008] Providing a tungsten rod and a mixture of boron powder and metal oxide, and placing the mixture in a block and the tungsten rod as an anode and a cathode, respectively, in an electric arc furnace;

[0009] [Corrected 07.04.2023 according to Rule 91] The electric arc furnace is evacuated, and then a buffer gas is filled in and the electric arc furnace is controlled to start an arc. After the bulk mixture is ignited, the electric arc furnace is controlled to turn off the arc, and the bulk mixture continues to burn and react to produce a transition metal boride.

[0010] In the above implementation, the arc furnace is used to provide a heat source, and one end of the anode is ignited to close the arc. The reaction proceeds in the form of a combustion wave until the entire anode is completely reacted. The arc plasma method, which has the advantages of simple operation, low cost, environmental friendliness, and controllable reaction atmosphere, can quickly prepare the transition metal boride. The preparation process is simple and will not affect the environment.

[0011] Optionally, the buffer gas is argon.

[0012] Optionally, the metal oxide is one of cobalt oxide, ferroferric oxide, nickel oxide, titanium dioxide and vanadium dioxide.

[0013] Optionally, the distance between the block mixture and the tungsten rod in the electric arc furnace is 1 to 3 mm.

[0014] Optionally, the discharge current of the arc is 12 to 50 A, and the discharge time is 1 to 30 s.

[0015] Optionally, the vacuum degree of the electric arc furnace after evacuation is less than or equal to 3Pa.

[0016] Optionally, the gas pressure after the buffer gas is filled is 40 to 80 kPa.

[0017] Optionally, the transition metal boride includes one of nickel boride, cobalt boride, vanadium diboride and titanium diboride.

[0018] It can be understood that the spacing range between the above-mentioned block mixture and the tungsten rod and the gas pressure range in the arc furnace can make the arc more stable; the arc discharge current and discharge time are matched with the above-mentioned spacing range and pressure range, which can make the preparation effect of metal boride better. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG1 is a schematic flow chart of a method for rapidly preparing a transition metal boride according to the present invention.

[0020] FIG2 is a schematic diagram of an electric arc furnace used in the rapid preparation method of transition metal borides of the present invention.

[0021] FIG3 is an X-ray diffraction pattern of nickel boride nanoparticles prepared in Example 1 of the present invention.

[0022] FIG4 is a transmission electron microscope image of nickel boride nanoparticles prepared in Example 1 of the present invention.

[0023] FIG5 is an X-ray diffraction pattern of vanadium diboride nanoparticles prepared in Example 2 of the present invention.

[0024] FIG6 is a transmission electron microscope image of vanadium diboride nanoparticles prepared in Example 2 of the present invention.

[0025] FIG7 is an X-ray diffraction pattern of titanium diboride nanoparticles prepared in Example 3 of the present invention.

[0026] FIG8 is a transmission electron microscope image of titanium diboride nanoparticles prepared in Example 3 of the present invention.

[0027] FIG9 is an X-ray diffraction pattern of cobalt boride nanoparticles prepared in Example 4 of the present invention.

[0028] FIG10 is a transmission electron micrograph of the cobalt boride nanoparticles prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0029] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to the contents described above.

[0030] 1 and 2 , the present invention provides a rapid preparation method for transition metal borides, which includes steps S1 and S2.

[0031] Step S1: providing a tungsten rod and a mixture of boron powder and metal oxide, and placing the mixture in a block and the tungsten rod as an anode and a cathode in an electric arc furnace, respectively.

[0032] [Corrected 07.04.2023 according to Rule 91] Step S2, evacuating the electric arc furnace, then filling it with buffer gas and controlling the electric arc furnace to start the arc, igniting the bulk mixture and then controlling the electric arc furnace to turn off the arc, and the bulk mixture continues to burn and react to produce the transition metal boride.

[0033] In the above implementation, the arc furnace is used to provide a heat source, and one end of the anode is ignited to close the arc. The reaction proceeds in the form of a combustion wave until the entire anode is completely reacted. The arc plasma method, which has the advantages of simple operation, low cost, environmental friendliness, and controllable reaction atmosphere, can quickly prepare the transition metal boride. The preparation process is simple and will not affect the environment.

[0034] Optionally, the buffer gas is argon.

[0035] Optionally, the metal oxide is one of cobalt oxide, ferroferric oxide, nickel oxide, titanium dioxide and vanadium dioxide.

[0036] Optionally, the distance between the block mixture and the tungsten rod in the electric arc furnace is 1 to 3 mm.

[0037] Optionally, the discharge current of the arc is 12 to 50 A, and the discharge time is 1 to 30 s.

[0038] Optionally, the vacuum degree of the electric arc furnace after evacuation is less than or equal to 3Pa.

[0039] Optionally, the gas pressure after the buffer gas is filled is 40 to 80 kPa.

[0040] Optionally, the transition metal boride includes one of nickel boride, cobalt boride, vanadium diboride and titanium diboride.

[0041] It can be understood that the spacing range between the above-mentioned block mixture and the tungsten rod and the gas pressure range in the arc furnace can make the arc more stable; the arc discharge current and discharge time are matched with the above-mentioned spacing range and pressure range, which can make the preparation effect of metal boride better.

[0042] The following is a detailed description of the rapid preparation method of a transition metal boride provided by the present invention in conjunction with specific Examples 1-5.

[0043] Example 1

[0044] (1) Preparation of a discharge anode: Boron powder and nickel oxide in a ratio of 6:1 were placed in a mortar to mix the two substances to obtain a mixture; the mixture was then placed in a hydraulic press to press into a block mixture.

[0045] (2) A tungsten rod is used as the cathode and the bulk mixture is used as the anode. The tungsten rod and the bulk mixture are placed in an electric arc furnace with a spacing of 1 mm between the two electrodes. After the electric arc furnace is evacuated to a vacuum degree of 3 Pa, the DC arc discharge current is set to 12 A. After filling with 70 kPa of argon gas, the arc is started and the discharge time is set to 1 s. The reactants collected on the inner wall of the reaction chamber are nickel boride particles.

[0046] Example 2

[0047] (1) Preparation of a discharge anode: a mixture of boron powder and vanadium dioxide in a ratio of 8:1 was placed in a mortar to mix the two substances to obtain a mixture; the mixture was then placed in a hydraulic press to press into a block mixture.

[0048] (2) A tungsten rod is used as the cathode and the bulk mixture is used as the anode. The tungsten rod and the bulk mixture are placed in an electric arc furnace with a spacing of 2 mm between the two electrodes. After the electric arc furnace is evacuated to a vacuum degree of 2 Pa, the DC arc discharge current is set to 20 A. After filling with 80 kPa of argon gas, the arc is started and the discharge time is set to 10 s. The reactants collected on the inner wall of the reaction chamber are vanadium diboride particles.

[0049] Example 3

[0050] (1) Preparation of a discharge anode: a mixture of boron powder and titanium dioxide in a ratio of 4:1 was placed in a mortar to mix the two substances to obtain a mixture; the mixture was then placed in a hydraulic press to press into a block mixture.

[0051] (2) A tungsten rod is used as the cathode and the bulk mixture is used as the anode. The tungsten rod and the bulk mixture are placed in an electric arc furnace with a spacing of 3 mm between the two electrodes. After the electric arc furnace is evacuated to a vacuum degree of 3 Pa, the DC arc discharge current is set to 50 A. After filling with 40 kPa of argon gas, the arc is started and the discharge time is set to 5 s. The reactants collected on the inner wall of the reaction chamber are titanium boride particles.

[0052] Example 4

[0053] (1) Preparation of a discharge anode: a mixture of boron powder and cobalt trioxide in a ratio of 10:1 was placed in a mortar to mix the two substances to obtain a mixture; the mixture was then placed in a hydraulic press to press into a block mixture.

[0054] (2) A tungsten rod is used as the cathode and the bulk mixture is used as the anode. The tungsten rod and the bulk mixture are placed in an electric arc furnace with a spacing of 1 mm between the two electrodes. After the electric arc furnace is evacuated to a vacuum degree of 3 Pa, the DC arc discharge current is set to 12 A. After filling with 70 kPa of argon gas, the arc is started and the discharge time is set to 30 s. The reactants collected on the inner wall of the reaction chamber are cobalt boride particles.

[0055] Example 5

[0056] (1) Preparation of a discharge anode: a mixture of boron powder and ferroferric oxide in a ratio of 10:1 was placed in a mortar to mix the two substances to obtain a mixture; the mixture was then placed in a hydraulic press to press into a block mixture.

[0057] (2) A tungsten rod is used as the cathode and the bulk mixture is used as the anode. The tungsten rod and the bulk mixture are placed in an electric arc furnace with a spacing of 1 mm between the two electrodes. After the electric arc furnace is evacuated to a vacuum degree of 3 Pa, the DC arc discharge current is set to 12 A. After filling with 70 kPa of argon gas, the arc is started and the discharge time is set to 5 s. The reactants collected on the inner wall of the reaction chamber are iron boride particles.

[0058] Furthermore, the transition metal boride prepared in Example 1 was analyzed. Figure 3 is an X-ray diffraction pattern of the nickel boride particles prepared in Example 1. The test results show that the diffraction peaks of the product are basically consistent with the standard spectrum below, that is, high-purity nickel boride particles were prepared by the DC arc method in Example 1. Furthermore, Figure 4 is a transmission electron microscope image of the nickel boride particles prepared in Example 1. The measured interplanar spacing d of the nickel boride particles is 0.28 nm, which corresponds to the (110) crystal plane of the nickel boride structure, indicating that nickel boride has been successfully prepared.

[0059] Furthermore, the vanadium diboride particles prepared in Example 2 were analyzed. Figure 5 is an X-ray diffraction pattern of the vanadium diboride particles prepared in Example 2. The test results show that the diffraction peaks of the product are basically consistent with the standard spectrum below, that is, high-purity vanadium diboride particles were prepared by the DC arc method in Example 2. Furthermore, Figure 6 is a transmission electron microscope image of the vanadium diboride particles prepared in Example 2. The measured interplanar spacing d of the nickel boride particles is 0.12 nm, which corresponds to the (201) crystal plane of the vanadium diboride structure, indicating that vanadium diboride has been successfully prepared.

[0060] Furthermore, the titanium diboride particles prepared in Example 3 were analyzed. Figure 7 is an X-ray diffraction pattern of the titanium diboride particles prepared in Example 3. The test results show that the diffraction peaks of the product are basically consistent with the standard spectrum below, that is, high-purity titanium diboride particles were prepared by the DC arc method in Example 3. Furthermore, Figure 8 is a transmission electron microscope image of the titanium diboride particles prepared in Example 3. The measured interplanar spacing d of the nickel boride particles is 0.12 nm, which corresponds to the (201) crystal plane of the nickel boride structure, indicating that titanium diboride was successfully prepared.

[0061] [Corrected 07.04.2023 according to Rule 91] Furthermore, the cobalt boride particles prepared in Example 4 were analyzed, wherein FIG9 is an X-ray diffraction pattern of the cobalt boride particles prepared in Example 4. The test results show that the diffraction peaks of the product are basically consistent with the standard spectrum below, that is, high-purity cobalt boride particles were prepared by the DC arc method of Example 4. Furthermore, FIG10 is a transmission electron microscope image of the cobalt boride particles prepared in Example 4, and the measured interplanar spacing d of the nickel boride particles is 0.22 nm, which corresponds to the (111) crystal plane of the nickel boride structure, indicating that cobalt boride was successfully prepared.

[0062] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations and simplifications that deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. A rapid preparation method of transition metal borides, It is characterized in that Includes steps: Providing a tungsten rod and a mixture of boron powder and metal oxide, and placing the tungsten rod and the mixture as a cathode and an anode in an electric arc furnace respectively; The arc furnace is evacuated, and then a buffer gas is filled in and the arc furnace is controlled to start an arc. After the block mixture is ignited, the arc furnace is controlled to close the arc. The block mixture continues to burn and react to obtain transition metal borides.

2. The rapid preparation method of transition metal borides according to claim 1, It is characterized in that The buffer gas is argon.

3. The rapid preparation method of transition metal boride according to claim 1, It is characterized in that The metal oxide is one of cobalt oxide, ferroferric oxide, nickel oxide, titanium dioxide and vanadium dioxide.

4. The rapid preparation method of transition metal borides according to claim 1, It is characterized in that The distance between the block mixture and the tungsten rod in the electric arc furnace is 1 to 3 mm.

5. The rapid preparation method of transition metal boride according to claim 1, It is characterized in that The discharge current of the arc is 12-50A, and the discharge time is 1-30s.

6. The rapid preparation method of transition metal boride according to claim 1, It is characterized in that The vacuum degree of the electric arc furnace after evacuation is less than or equal to 3Pa.

7. The rapid preparation method of transition metal boride according to claim 2, It is characterized in that The argon pressure is 40-80 kPa.

8. The rapid preparation method of transition metal boride according to claim 1, It is characterized in that The transition metal boride includes one of nickel boride, cobalt boride, vanadium diboride and titanium diboride.

Citation Information

Patent Citations

  • Magnetic material and method for preparing same

    CN108140480A

  • Method for preparing refractory metal nano-powder by DC arc plasma

    CN110405221A

  • Improvements in a method of producing metal borides

    GB790938A