Method for manufacturing grazing incidence optical element and optical element obtained thereby

By using optical components of glass layers and carbon fiber reinforced materials, the complex and expensive production process of grazing incident optical components in the prior art is solved, and optical component manufacturing with high precision, low cost and high angle resolution is achieved.

CN119013588APending Publication Date: 2024-11-22INST NAT DI ASTROFISICA INAF +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380020123.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-03
Filing Date
2023-02-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The production process of existing grazing incident optical components is complex, expensive and difficult to manage, especially due to the need for high-precision and low-roughness substrates and mandrels, resulting in poor optical properties of the modular structure and complex metal deposition process.

Method used

Using optical components composed of glass layer and carbon fiber reinforced material shell, the mandrel is turned by diamond, wound the carbon fiber layer and deposited the CFRP shell, combining the characteristics of low thermal expansion coefficient and high stiffness, avoiding polishing steps and complex metal deposition The process enables high-precision and low-cost manufacturing.

Benefits of technology

Achieve high angle resolution, reduce production time and cost, simplify management complexity, and avoid surface irregularities due to the low roughness of the glass layer and the isotropic distribution of carbon fibers, creating high rigidity and thermal stability optical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013588A_ABST
    Figure CN119013588A_ABST
Patent Text Reader

Abstract

A method for manufacturing a grazing incidence optical element (1), comprising the steps of: providing a mandrel (11) having a surface (12) with a contour complementary to a contour of an optical surface (5) of the optical element (1) to be manufactured; adhering at least one glass sheet (31, 32) to the mandrel (11) to define the optical surface (5); a carbon fiber reinforcement material is deposited on the outer surfaces (51, 52) of the glass sheets (31, 32) to form a housing (3) that is securely connected to the glass sheets (31, 32).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This patent application claims the priority of Italian Patent Application No. 102022000001904, filed on February 3, 2022, the entire disclosure of which is incorporated herein by reference. Technical Field

[0003] The present invention relates to a method for producing a grazing incidence optical element. Background Art

[0004] As is known, grazing incidence optics comprise optical surfaces, which are usually surfaces of revolution (such as paraboloids, hyperboloids or ellipsoids), sometimes combined together to obtain a double reflection system.

[0005] Typically, grazing incidence optics are used for X-ray optics because X-rays can be reflected efficiently only at angles of incidence relative to the normal to the reflecting surface close to 90° (e.g., at angles of incidence greater than 88°), unlike what happens for visible light.

[0006] Grazing incidence optical elements with a modular structure are known, in which the optical surface consists of a plurality of discrete modules, for example having a substantially rectangular or hexagonal shape, usually made of glass. Obviously, this discreteness makes the optical properties (such as angular resolution) worse, and requires the integration of multiple modules, which makes the production process long, expensive and difficult to manage.

[0007] Grazing incidence optics are also known, which comprise a structure consisting of a metal or glass shell or of a monolithic glass-ceramic material, for example in nickel replicated from a mandrel by electroforming, and a continuous optical surface formed by a reflective coating, for example gold. However, to manufacture such optics, substrates (or mandrels, if replication techniques are used) with high dimensional accuracy and very low roughness are required, since metal deposition involves replicating the roughness of the substrate or mandrel on the optical surface of the reflective cover. These requirements make the production process very expensive relative to monolithic grazing incidence optics.

[0008] The object of the present invention is to provide an optical element allowing to overcome the above-mentioned problems. Summary of the invention

[0009] The above object is achieved by a method according to claim 1 .

[0010] The invention also relates to an optical element according to claim 13 and a mirror according to claim 16 . BRIEF DESCRIPTION OF THE DRAWINGS

[0011] For a better understanding of the present invention, preferred embodiments are described below by way of non-limiting examples and with reference to the accompanying drawings, in which:

[0012] Figure 1 is a perspective view of an optical element according to the present invention;

[0013] Figure 2 Based on including Figure 1 A stereoscopic view of a mirror of the present invention having multiple optical elements;

[0014] Figures 3 to 6 Schematic diagram showing the process for making Figure 1 The consecutive steps of the method for producing an optical element; and

[0015] Figure 7 A plant for carrying out the steps of the manufacturing method according to the invention is schematically shown. DETAILED DESCRIPTION

[0016] Reference Figure 1 , denoted by 1 is a grazing incidence optical element according to the present invention. The optical element 1 comprises a glass layer 2 and a shell 3 of a reinforcing material, wherein the reinforcing material comprises a plurality of carbon fiber layers deposited on the glass layer 2.

[0017] The optical element 1 may be configured as ( Figure 2 ) A module of a mirror 4 made by integrating multiple optical elements 1 that are nested in each other.

[0018] The glass layer 2 has a thickness of less than 100 μm, preferably 50 μm or less, and is composed of one or more thin sheets, having a flexibility comparable to that of a paper sheet. For example, SCHOTT ECO glass can be used for this purpose. The use of one or more sheets depends on the geometry of the optical surface 5 of the optical element 1, as described in detail below. The glass layer 2 inherently has a negligible roughness of less than 0.5 nm.

[0019] In the following, without loss of generality, an optical element 1 for a type I Wolter telescope is considered to have an optical surface 5 consisting of a first portion 6, which is an A-axis parabola, and a second portion 7, which is a hyperbola coaxial with the parabola and connected thereto along a plane orthogonal to the axis A. Such a telescope has a focal plane 8, which is reached by an incident ray after a double reflection. In particular, the incident ray is reflected from the inner surface of the first portion 6 and subsequently from the inner surface of the second portion 7, the second portion 7 being interposed between the first portion 6 and the focal plane 8.

[0020] The method for producing the optical element 1 comprises several steps which will be described in detail below.

[0021] first( Figure 3 ), a core shaft 11 having a side surface 12 is provided, and the contour of the side surface 12 is complementary to the contour of the optical surface 5 of the optical element 1.

[0022] Thus, the mandrel 11 is a B-axis solid and the side surface 12 of the mandrel 11 includes a first surface 21 which is a B-axis parabola and a second surface 22 which is a hyperboloid coaxial with the parabola and matches it along a plane orthogonal to the axis B.

[0023] The mandrel 11 is machined by diamond turning, i.e. the mandrel 11 is turned with a diamond tool, so that the side surface 12 is exactly equal to the desired shape of the optical surface 5. Thus, the first surface 21 and the second surface 22 of the mandrel 11 correspond respectively to the first portion 6 and the second portion 7 of the optical surface 5. It should be noted that in the method presented, the application of a polishing step is not essential.

[0024] The mandrel 11 internally comprises a plurality of suction conduits connected at one end thereof to respective suction holes 23 arranged along at least one generatrix of the mandrel 11 and at the opposite end thereof to a rotary connector 24 for connection to a vacuum source (not shown).

[0025] Afterwards ( Figure 4 ), in the example described regarding the optical element 1 for a type I Walter telescope, the first glass piece 31 is adhered to the first surface 21 of the mandrel 11, and the second glass piece 32 is adhered to the second surface 22 of the mandrel 11.

[0026] In particular, each glass sheet 31, 32 is wound on a corresponding surface 21, 22 of the mandrel 11 and is held in place by suction thanks to the holes 23. Thus, the glass sheets 31, 32 adhere to the side surface 12 of the mandrel 11 and replicate its shape. After winding around the mandrel 11:

[0027] - the first glass sheet 31 and the second glass sheet 32 ​​match each other along a plane orthogonal to the axis A, in particular along respective adjacent circular edges connected to each other via the first adhesive strip 41 ; and

[0028] The first glass sheet 31 and the second glass sheet 32 ​​each have respective opposite matching edges along a generatrix of the mandrel 11 , which are connected together by a second adhesive tape 42 .

[0029] Afterwards ( Figure 5 ), carbon fiber reinforced material is deposited on the outer surfaces 51, 52 of the glass sheets 31, 32 to form the shell 3.

[0030] In particular, the reinforcement material is carbon fiber reinforced polymer, also known as CFRP, which has low density, high stiffness and low coefficient of thermal expansion, which properties are necessary for manufacturing the housing 3 .

[0031] However, carbon fibers have anisotropic properties, which involve changes in elastic modulus and thermal expansion coefficient when the orientation of the layers is changed.

[0032] Therefore, according to a preferred embodiment of the present invention, a filament winding process ( Figure 7 ) to produce the shell 3 in CFRP, in which unidirectional carbon fibers (ie in filament form) are impregnated with resin and wound around glass sheets 31, 32 to form a distribution that is as isotropic as possible.

[0033] Preferably, carbon fibers with a standard elastic modulus are used. Such fibers unwound from at least one reel 61 pass through an impregnation tank 62 to be impregnated with resin. Conveniently, the fibers are impregnated with resin using system, where epoxy LY5052 and epoxy hardener 5052. During the filament winding process, the fibers and resin are coupled and wound onto the glass sheets 31, 32 by a deposition head 63 which is programmed to deposit CFRP filaments forming successive layers until a predetermined thickness is reached. In order to give the shell 3 isotropic properties, the filaments of one layer are deposited in a different direction than the filaments of the successive layers.

[0034] After the CFRP is deposited, the resin is cured. In particular, the curing is performed at room temperature to avoid the difference in thermal expansion between the CFRP and the glass sheets 31 , 32 .

[0035] Afterwards ( Figure 6 ), the optical element 1 is separated from the mandrel 11 by cooling the mandrel itself.

[0036] Finally, the optical element 1 may undergo a step of internal optical coating designed to optimize the reflectivity of the mirror at the desired energy or wavelength. The optical coating may be manufactured by different techniques such as vacuum evaporation, deposition by sputtering process, deposition by chemical reduction of thin films. The optical coating may consist of one or more metallic or non-metallic thin films.

[0037] The advantages of the present invention are apparent when examining the properties of the optical element 1 .

[0038] In particular, the optical element 1 is monolithic. This results in improved optical properties, such as angular resolution, and reduced time, cost and management complexity in the manufacture of the optical element 1 compared to optical elements with discrete optical surfaces.

[0039] The profile of the glass layer 2 has a high dimensional accuracy, since it is complementary to the profile of the mandrel 11, which can be manufactured by high-precision machining (e.g. diamond turning). Unlike optical elements with metal structures (e.g. nickel) and gold optical surfaces, the roughness of the side surface 12 of the mandrel 11 (which is inherently generated by diamond turning the mandrel 11) is not relevant to the purpose of the optical element 1, since the roughness of the glass layer 2 of the optical element 1 is negligible and, due to the hardness of the glass, the micro-roughness of the mandrel is not transferred to the glass by elastic deformation or by inelastic deformation.

[0040] The properties of CFRP make it suitable for the housing 3 of the optical element 1 .

[0041] A filament winding method in which resin and unidirectional carbon fibers are used, avoiding the use of a woven carbon fiber structure, allows preventing the surface irregularities of the carbon fibers from being reproduced on the optical surface 5 (print-through effect).

[0042] As an alternative to the filament winding process, a fiber placement process can be used, whereby the fibers are robotically deposited in the form of prepreg tapes unwound from a reel, or by manual deposition of the fibers in the form of prepregs.

[0043] The characteristics of the production process allow the manufacture of optical elements with high rigidity, thermal and mechanical stability, diameters up to 1 m and angular resolutions less than 5 arc seconds1.

[0044] Since no polishing operation is required, the manufacturing time and cost of the optical element 1 are reduced.

[0045] Finally, it is obvious that modifications and variations may be made to the optical element 1 without departing from the scope of protection defined in the claims.

[0046] For example, the glass layer 2 may have a geometric shape defined by a cone or a polynomial.

Claims

1. A method for manufacturing a grazing incidence optical element (1), comprising the following steps: - providing a mandrel (11) having a surface (12) having a profile complementary to the profile of an optical surface (5) of an optical element (1) to be manufactured; - adhering at least one glass sheet (31, 32) to said mandrel (11) so as to define said optical surface (5); - depositing carbon fiber reinforcement material on the outer surfaces (51, 52) of the glass sheets (31, 32) to form a shell (3) firmly connected to the glass sheets (31, 32).

2. The method according to claim 1, wherein: The mandrel (11) is processed by diamond turning.

3. The method according to claim 1 or 2, wherein: The glass sheets (31, 32) have a thickness of less than 100 μm.

4. A method according to any one of the preceding claims, wherein: The reinforcing material is CFRP (Carbon Fiber Reinforced Polymer).

5. A method according to any one of the preceding claims, wherein: The step of adhering the at least one glass sheet (31, 32) to the mandrel (11) comprises the steps of wrapping the glass sheet (31, 32) around the mandrel (11) and holding the glass sheet (31, 32) in place by creating a vacuum between the mandrel (11) and the at least one glass sheet (31, 32).

6. A method according to any one of the preceding claims, wherein: The step of adhering the at least one glass sheet (31, 32) to the mandrel (11) comprises the step of applying adhesive tape (41, 42) along opposite, mutually matching edges of the glass sheets (31, 32).

7. A method according to any one of the preceding claims, wherein: The mandrel (11) comprises at least two portions (21, 22) of different geometric shapes matched along a plane orthogonal to an axis (B) of the mandrel (11), and the optical surface (5) is defined by at least two glass sheets (31, 32) arranged on the respective portions (21, 22) of the mandrel (11).

8. The method according to claim 7, wherein: The glass sheets (31, 32) are joined together by adhesive tapes (41, 42) applied to respective adjacent edges of the glass sheets (31, 32) matching along a plane orthogonal to the axis (B) of the mandrel (11).

9. A method according to any one of the preceding claims, wherein: The reinforcement material is deposited in the form of filaments.

10. The method according to claim 9, wherein: The filaments are impregnated with resin prior to deposition.

11. A method according to claim 10, comprising the step of curing at ambient temperature.

12. Method according to any of the preceding claims, comprising the step of cooling the mandrel (11) in order to separate the optical element (1) from the mandrel (11).

13. An optical element comprising at least one glass sheet (31, 32) and a shell (3) of carbon fiber reinforced material firmly connected to the outer surface (51, 52) of the glass sheet (31, 32).

14. The optical element according to claim 11, wherein: The glass sheets (31, 32) have a thickness of less than 100 μm.

15. The optical element according to claim 11 or 12, wherein: The reinforcing material is CFRP (Carbon Fiber Reinforced Polymer).

16. A mirror for a telescope, comprising a plurality of optical elements (1) according to any one of claims 13 to 15, wherein the plurality of optical elements (1) are coaxial and nested with each other.