Current collector, pole piece, battery monomer, battery and electric device
Patent Information
- Application Number
- CN202280094885.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-21
- Publication Date
- 2024-11-22
AI Technical Summary
During the cycle process of existing secondary batteries, the lithium precipitation problem occurs in the middle area of the pole piece due to the expansion of the electrode active material, which affects the cycle performance and service life of the battery.
It adopts a special structure of the current collector, which is thick on both sides and thin in the middle. By setting different pressure densities of the film layers on the first and second parts, the electrolyte holding capacity of the middle area of the pole piece is improved and the lithium precipitation phenomenon is reduced.
It effectively improves the cycle performance and service life of the battery, improves the safety of the battery, and reduces the polarization phenomenon in the middle area of the pole piece.
Smart Images

Figure CN119013804A_ABST
Abstract
Description
Current collectors, pole pieces, battery cells, batteries and electrical devices Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a current collector, a pole piece, a battery cell, a battery, and an electrical device. Background Art
[0002] In recent years, the application scope of secondary batteries has become increasingly extensive. They are widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power plants, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As secondary batteries have achieved great development, higher requirements have been placed on their cycle performance and service life.
[0003] Therefore, how to improve the cycle performance and service life of batteries is a technical problem that needs to be solved urgently.
[0004] Summary of the Invention
[0005] The present application is made in view of the above-mentioned technical problems, and its purpose is to provide a current collector, a pole piece, a battery cell, a battery and an electrical device, wherein the current collector has a special structure, which can effectively improve the wetting of the middle area of the pole piece during the battery cycle, reduce the lithium plating phenomenon of the pole piece, and thus improve the cycle performance and service life of the battery.
[0006] In a first aspect, the present application provides a current collector, comprising: a first part, which is arranged along a first direction, wherein the first direction is the width direction of the current collector or the length direction of the current collector; a second part, which is arranged between two first parts; wherein the first part and the second part are used to support a film layer, the first part has a first thickness, the second part has a second thickness, and the first thickness is greater than the second thickness.
[0007] The current collector provided in the present application has a special structure that is thick on both sides and thin in the middle. Specifically, the current collector has a thicker first part and a thinner second part. When using the current collector to prepare a pole piece, the film layer provided on the first part can be compressed to a higher density, while the film layer provided on the second part can be compressed to a lower density. As a result, the film layer in the middle part of the pole piece can accommodate more electrolyte without changing the thickness of the pole piece, thereby improving the problem of lithium deposition in the middle area of the pole piece caused by the expansion of the electrode active material during the charge and discharge process. This effectively improves the battery cycle performance and service life, and helps improve the safety of the battery.
[0008] In some embodiments, a ratio of a width of the second portion in the first direction to a width of the first portion and the second portion in the first direction is 30%-70%, preferably 40%-60%.
[0009] In an embodiment of the present application, by setting the width of the second part to a proportion of the entire first part and the second part within an appropriate range, the membrane layer arranged on the second part of the current collector can accommodate more electrolyte without increasing the difficulty of the process, thereby further helping to improve the problem of lithium deposition in the middle area of the electrode.
[0010] In some embodiments, the current collector includes: a tab portion, the tab portion is connected to at least one of the first portions in the first direction, and a thickness of the tab portion is less than or equal to a thickness of the first portion.
[0011] In this embodiment, the tab portion is connected to the first portion. When the thickness of the tab portion is equal to the thickness of the first portion, the tab portion and the first portion can be formed at one time, which is conducive to the integrated processing of the pole piece; when the thickness of the tab portion is less than the thickness of the first portion, the thickness of the tab after flattening can be reduced by reducing the thickness of the tab portion, thereby helping to improve the space utilization inside the battery.
[0012] In some embodiments, the first thickness is 10 μm-20 μm, preferably 12 μm-18 μm; the second thickness is 1 μm-20 μm, preferably 6 μm-17 μm.
[0013] In some embodiments, a film layer is disposed on the first portion and the second portion, and a compaction density of the film layer in the first portion is greater than a compaction density of the film layer in the second portion.
[0014] In an embodiment of the present application, by controlling the compaction density of the film layer arranged on the current collector in the first part to be greater than its compaction density in the second part, the film layer arranged in the second part can accommodate more electrolyte than the first part, thereby effectively improving the lithium plating problem in the middle area of the electrode.
[0015] In some embodiments, the current collector is a positive electrode current collector, the film layer is a positive electrode film layer, and the compaction density of the positive electrode film layer in the first part is 2.3 g / cm 3 -2.5g / cm 3 , preferably 2.4 g / cm 3 The compaction density of the positive electrode film layer in the second part is 2.2g / cm 3 -2.4g / cm 3 , preferably 2.35 g / cm 3 .
[0016] In some embodiments, the current collector is a negative electrode current collector, the film layer is a negative electrode film layer, and the compaction density of the negative electrode film layer in the first portion is 1 g / cm 3 -1.65g / cm 3 , preferably 1.5 g / cm 3 The compaction density of the negative electrode film layer in the second part is 0.9g / cm 3 -1.5g / cm 3 , preferably 1.45 g / cm 3 .
[0017] In the embodiments of the present application, the collector with a special structure is used in the positive electrode and / or negative electrode of the battery. By controlling the compaction density of the positive electrode film layer and / or the negative electrode film layer in the first part and the second part within a suitable range, the number of pores in the middle area of the positive electrode sheet and / or the negative electrode sheet can be effectively increased, so that the middle area can accommodate more electrolyte, effectively improving the lithium plating problem of the electrode in the battery.
[0018] In some embodiments, the sum of the thicknesses of the membrane layer and the current collector in the second portion is greater than or equal to the sum of the thicknesses of the membrane layer and the current collector in the first portion.
[0019] In the embodiment of the present application, when the sum of the thickness of the membrane layer and the current collector in the second part is equal to the sum of the thickness of the membrane layer and the current collector in the first part, it means that the electrode has a portion of the membrane layer with equal thickness, that is, the thickness of the entire electrode is uniform. As a result, the spacing between the electrode sheets in the battery is basically equal everywhere, which can avoid battery polarization caused by unequal spacing between the positive electrode sheet and the negative electrode sheet during the battery cycle, thereby helping to improve the battery's lithium plating problem. When the sum of the thickness of the membrane layer and the current collector in the second part is greater than the sum of the thickness of the membrane layer and the current collector in the first part, it means that the distance of ion migration between the positive electrode sheet and the negative electrode sheet at the second part during the battery cycle is smaller, which helps to improve ion dynamics, thereby helping to reduce the polarization phenomenon in the middle part of the electrode sheet, thereby further improving the battery's lithium plating problem.
[0020] In some embodiments, the sum of the thicknesses of the membrane layer and the current collector in the second portion is 1%-3% greater than the sum of the thicknesses of the membrane layer and the current collector in the first portion.
[0021] In some embodiments, the first portion is obtained by thickening the current collector.
[0022] In some embodiments, the second portion is obtained by thinning the current collector.
[0023] In the embodiments of the present application, the current collector with a special structure can be produced through a variety of different processing methods, and the preparation methods are flexible and diverse, which helps to improve the production efficiency of the current collector.
[0024] In a second aspect, a pole piece is provided, comprising the current collector in any embodiment of the first aspect.
[0025] In a third aspect, a battery cell is provided, wherein the battery cell includes the current collector described in any embodiment of the second aspect.
[0026] In a fourth aspect, a battery is provided, comprising the battery cell according to any one of the embodiments of the third aspect.
[0027] In the fifth aspect, an electrical device is provided, characterized in that the electrical device includes at least one of the battery cells described in any embodiment of the third aspect or the batteries described in any embodiment of the fourth aspect, and the battery cells and / or the batteries are used to power the electrical device. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. Those skilled in the art can also derive other drawings based on the drawings without inventive effort. In the drawings, the drawings are not drawn to scale.
[0029] FIG1 is a schematic top view of a current collector according to an embodiment of the present application.
[0030] FIG2 is a schematic cross-sectional view of a current collector according to an embodiment of the present application.
[0031] FIG3 is another schematic cross-sectional view of a current collector according to an embodiment of the present application.
[0032] FIG4 is a schematic structural diagram of a pole piece according to an embodiment of the present application.
[0033] FIG5 is a schematic structural diagram of an electrode assembly according to an embodiment of the present application.
[0034] FIG6 is a photograph of the negative electrode sheet after the cycle of Comparative Example 1 of the present application.
[0035] FIG7 is a photograph of the negative electrode sheet after the cycle of Example 1 of the present application. DETAILED DESCRIPTION
[0036] Below, the embodiments of the negative electrode current collector, the secondary battery containing the negative electrode current collector, the battery module and the electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0037] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0038] In the description of this application, it should be noted that, unless otherwise specified, "multiple" means more than two; the terms "upper", "lower", "left", "right", "inside", "outside", etc., indicating directions or positional relationships, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on this application. In addition, the terms "first", "second", "third", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. "Vertical" is not strictly perpendicular, but is within the allowable error range. "Parallel" is not strictly parallel, but is within the allowable error range.
[0039] The directional words appearing in the following description are all directions shown in the figures, and do not limit the specific structure of this application. In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances.
[0040] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0041] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0042] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0043] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0044] In a battery, the positive electrode sheet, the negative electrode sheet, the electrolyte, and the separator are the basic elements that make up a battery. During the charge and discharge process of the battery, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte conducts active ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet to prevent the positive and negative electrodes of the battery from short-circuiting, while also allowing active ions to pass through. Among them, the positive electrode sheet and the negative electrode sheet are collectively referred to as the electrode sheet, and the electrode sheet generally includes a current collector and a film layer arranged on the current collector, and the film layer includes an electrode active material.
[0045] During battery manufacturing, positive and negative electrode sheets and separators are typically assembled into an electrode assembly. This assembly is then placed in a housing containing the electrode assembly and electrolyte to form a single cell. The electrode assembly can be a wound or laminated structure. A battery comprises at least one single cell.
[0046] Alternatively, the battery may include a lithium ion battery, a sodium ion battery, a magnesium ion battery, or the like.
[0047] This application uses lithium-ion batteries as an example. Lithium-ion batteries are a typical type of secondary battery. Because they rely on chemical reactions in which lithium ions, as active ions, intercalate and disintercalate between the positive and negative electrodes to charge and discharge, they are also called rocking-chair batteries. During charging, lithium ions are released from the positive electrode, moved to the negative electrode, and then intercalated into the positive electrode. During discharge, lithium ions are released from the negative electrode, moved to the positive electrode, and then intercalated into the positive electrode.
[0048] During the electrochemical reactions of lithium-ion batteries, the electrode sheets expand during cycling due to various factors, including structural changes in the electrode active materials during lithium insertion and removal, and side reactions of the active materials. Due to factors such as ion dynamics and battery energy density, the spacing between the positive and negative electrode sheets is very small, often insufficient to accommodate expansion or structural damage to the electrode active materials. Consequently, electrolyte, especially liquid electrolyte, squeezes out between the positive and negative electrode sheets, leaving insufficient electrolyte for ionic conduction between the sheets. This leads to severe battery polarization, and active ions (lithium ions) precipitate on the surface of the negative electrode sheet, a phenomenon known as lithium plating. This significantly impacts the battery's cycle performance and service life, and in severe cases, can even cause safety issues. This is particularly true in wound electrode assemblies, where the electrode sheets are wound into a cylindrical electrode assembly, with the central region of the electrode sheets forming the middle portion of the electrode assembly. Due to structural reasons, the middle portion of a cylindrical electrode assembly is difficult to wet, and the amount of electrolyte storage is limited. During battery cycling, the electrolyte in the middle portion of the electrode assembly is squeezed out, exacerbating the lithium plating problem caused by polarization.
[0049] In view of this, the present application provides a current collector, a pole piece, a battery cell, a battery, and an electrical device. The current collector has a unique structure with thicker sides and thinner middle, which allows the pole piece produced using the current collector to have a relatively uniform thickness while having higher density on both sides and lower density in the middle. As a result, the middle portion of the pole piece can store more electrolyte, improving polarization in the middle region of the pole piece during battery cycling, thereby reducing lithium deposition on the surface of the negative pole piece.
[0050] It should be understood that the "lithium insertion" and "intercalation" processes described in this application refer to the process in which lithium ions are embedded in the positive electrode material and the negative electrode material due to electrochemical reactions, and the "de-lithiumization", "de-lithiumization" and "de-intercalation" processes described in this application refer to the process in which lithium ions are removed from the positive electrode material and the negative electrode material due to electrochemical reactions.
[0051] First, the present application provides a current collector. Figure 1 is a schematic top view of a current collector according to an embodiment of the present application. Figure 2 is a schematic cross-sectional view of a current collector according to an embodiment of the present application.
[0052] As shown in FIG. 1 and FIG. 2 , the current collector 1 includes a first portion 101 and a second portion 102 .
[0053] The first portion 101 is disposed along a first direction k, which is the width direction of the current collector 1 or the length direction of the current collector 1. The second portion 102 is disposed between the two first portions 101. The first portion 101 and the second portion 102 are used to support the film layer. The first portion 101 has a first thickness d1, and the second portion 102 has a second thickness d2, and the first thickness d1 is greater than the second thickness d2.
[0054] It should be understood that the current collector 1 generally has two surfaces opposite to each other along its own thickness direction, and the film layer is provided on any one or both of the two opposite surfaces of the current collector 1. The structure of the current collector 1 shown in Figures 1 and 2 is the structure of the surface of the current collector 1 provided with a film layer. In other words, in the case where the film layer is provided on only one surface of the current collector 1, the surface of the current collector 1 provided with the film layer has the structure shown in Figures 1 and 2. In the case where the film layer is provided on both surfaces of the current collector 1, both surfaces of the current collector 1 have the structure of Figures 1 and 2. The current collector 1 can be a positive electrode current collector or a negative electrode current collector. The pole piece prepared using the current collector 1 can be used to form a wound electrode assembly or a laminated electrode assembly.
[0055] The first portion 101 and the second portion 102 of the current collector 1 form the coating region 10 of the current collector 1 , that is, the portion of the current collector 1 used to carry the film layer.
[0056] In the wound electrode assembly, the first direction k is preferably the width direction of the current collector 1, and the first part 101 is arranged along the first direction k to form two sides of the coating area 10. In the process of preparing the electrode sheet, the electrode active material is usually coated on the current collector, and then a current collector provided with a film layer, i.e., a pole sheet, is formed through steps such as compaction and drying. When the current collector 1 is used to prepare the pole sheet, due to the special structure of the surface of the current collector 1, the film layer obtained by cold pressing and drying has a higher compression density at the first part 101 than at the second part 102. Then, the pole sheet is wound along the second direction j to form a wound electrode assembly. The second direction j is perpendicular to the first direction k. Thus, the second part 102 forms the middle part of the wound electrode assembly after winding.
[0057] It should be understood that compaction refers to the compacted density of the membrane layer.
[0058] In a laminated electrode assembly, the first direction k is preferably the length of the current collector 1. The electrode sheet preparation process is similar to that of a wound electrode assembly. After preparation, the electrode sheets are alternately stacked, with a separator wound in a Z-shaped pattern between them to form the laminated electrode assembly. Thus, after lamination, the second portion 102 forms the middle portion of the laminated electrode assembly.
[0059] In this embodiment, the thickness of the first part 101 of the current collector 1 is greater than the thickness of the second part 102 thereof, so that the film layer arranged on the coating area 10 of the current collector 1 has different compaction. That is, the compaction of the film layer in the first part 101 is greater than the compaction of the film layer in the second part 102, so that the film layer located in the second part 102 can store more electrolyte, especially liquid electrolyte, than the first part 101. As a result, the middle part of the electrode assembly prepared by the current collector 1 has the ability to accommodate more electrolytes than other parts. During the cycle of the battery, although the expansion of the electrode active material will cause part of the electrolyte to be squeezed out, since the middle part of the electrode assembly can accommodate more electrolytes, the middle part still stores enough electrolytes and has better active ion conductivity, thereby improving the polarization phenomenon caused by insufficient electrolytes. By using the current collector 1 with a special structure, the occurrence of lithium plating can be effectively reduced, thereby improving the cycle performance and service life of the battery, and also helping to improve the safety performance of the battery.
[0060] In addition, the current collector 1 provided in the present application is provided in the process of preparing the pole piece, in the process of compaction, for example, in the process of compaction by a roller press, due to the special structure of the surface of the current collector 1, the roller press uses a pressure to roll the current collector and the electrode active material to obtain a pole piece with uniform thickness and different compaction distribution. On the one hand, the thickness of the pole piece obtained by one-time rolling with one pressure is uniform, which helps to make the spacing between the positive pole piece and the negative pole piece equal, whether it is a wound electrode assembly or a laminated electrode assembly, and avoids polarization caused by the large difference in spacing between the positive and negative electrodes of the battery. On the other hand, pole pieces with different compaction distributions can be obtained by rolling with only one pressure once, which makes the processing method and steps of the pole piece simpler, and helps to improve the production efficiency of the pole piece, thereby improving the production efficiency of the battery while improving the cycle performance and service life of the battery.
[0061] Optionally, the ratio of the width of the second portion 102 in the first direction k to the sum of the widths of the first portion 101 and the second portion 102 in the first direction k is 30%-70%, preferably 40%-60%.
[0062] Specifically, as shown in FIG1 , the second portion 102 has a width h in the first direction k, and the sum of the widths of the first portion 101 and the second portion 102 in the first direction k is H. In other words, the coating region 10 has a width H in the first direction k. 30% ≤ h / H ≤ 70%; preferably, 40% ≤ h / H ≤ 60%. h / H can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, or 70%, or any value within the range obtained by combining any two of the above values.
[0063] In this embodiment, by setting the width of the second portion 102 within a suitable range, the membrane layer disposed on the second portion 102 of the current collector can accommodate as much electrolyte as possible without increasing the difficulty of the process.
[0064] FIG3 is another schematic structural diagram of the current collector 1 according to an embodiment of the present application.
[0065] Optionally, as shown in FIG. 2 and FIG. 3 , the current collector 1 includes a tab portion 20 , which is connected to the first portion 101 in the first direction k, and a thickness of the tab portion 20 is less than or equal to a thickness of the first portion 101 .
[0066] Specifically, to facilitate processing, the thickness of the tab portion 20 of the current collector 1 can be less than or equal to the thickness of the first portion 101. For example, referring to FIG3 , when the second portion 102 is prepared by thinning the current collector 1, the thickness of the first portion 101 is equal to the thickness of the substrate used to prepare the current collector 1. In this case, the thickness of the tab portion 20 is equal to the thickness of the first portion 101, that is, the thickness of the tab portion 20 is also equal to the thickness of the substrate, thereby simplifying the processing steps for the tab portion 20 of the current collector 1. For another example, referring to FIG2 , when the second portion 102 is prepared by thickening the first portion 101 of the current collector 1, the thickness of the second portion 102 is equal to the thickness of the substrate used to prepare the current collector 1, thereby also simplifying the processing steps for the tab portion 20. In this case, the thickness of the first portion 101 is greater than the thickness of the substrate, which means that the thickness of the tab portion 20 is less than the thickness of the first portion 101.
[0067] In this embodiment, the tab portion 20 is connected to the first portion 101. When the thickness of the tab portion 20 is equal to that of the first portion 101, the tab portion 20, the first portion 101, and the second portion 102 can be integrally formed, thereby improving the production efficiency of the electrode sheet. When the thickness of the tab portion 20 is less than that of the first portion 101, the thickness of the tab formed after the tab portion 20 is flattened can be reduced, thereby saving space within the battery and improving the space utilization rate within the battery.
[0068] In some other possible implementations, for example, in a laminated electrode assembly, the tab portion 20 of the current collector 1 may also be connected to the second portion 102 on the second reverse direction j.
[0069] Optionally, the first thickness d1 is 10 μm-20 μm, preferably, d1 is 12 μm-18 μm.
[0070] Specifically, d1 can be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, or 20 μm, or its value can be within the range obtained by combining any two of the above values.
[0071] Optionally, the second thickness d2 is 1 μm-20 μm, preferably, d2 is 6 μm-17 μm.
[0072] Specifically, d2 can be 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, or its value can be within the range obtained by combining any two of the above values.
[0073] Optionally, as shown in FIG. 2 , the first portion 101 is obtained by thickening the current collector 1 .
[0074] Specifically, during the preparation of the current collector 1, the first portion 101 can be obtained by thickening both sides of the substrate used to prepare the current collector 1. For example, ultrasonic welding can be performed on both sides of the substrate to obtain the current collector 1 having the first portion 101. For another example, by modifying the mold used to prepare the substrate, the first portion 101 of the current collector 1 can be formed during the grinding process of the substrate, such that the thickness of the tab portion 20 of the current collector 1 is less than the thickness of the first portion 101.
[0075] Optionally, as shown in FIG3 , the second portion 102 is obtained by thinning the current collector 1 .
[0076] Specifically, during the preparation of the current collector 1, the second portion 102 can be obtained by thinning the middle portion of the substrate used to prepare the current collector 1. For example, the current collector 1 having the second portion 102 can be obtained by cutting the middle portion of the substrate. For another example, by changing the grinding tool used to prepare the substrate, the second portion 102 of the current collector 1 can be machined during the grinding process, so that the thickness of the tab portion 20 of the current collector 1 is equal to the thickness of the first portion 101.
[0077] FIG4 is a schematic structural diagram of a pole piece according to an embodiment of the present application.
[0078] As shown in FIG4 , the pole piece 3 includes a current collector 1 and a film layer 30 disposed on the current collector.
[0079] Optionally, a film layer 30 is provided on the first portion 101 and the second portion 102 , and the compaction density of the film layer 30 in the first portion 101 is greater than the compaction density of the film layer 30 in the second portion.
[0080] In this embodiment, by controlling the compaction density of the film layer 30 arranged on the current collector 1 in the first part 101 to be greater than its compaction density in the second part 102, the film layer arranged in the second part can store more electrolyte than the film layer in the first part, thereby effectively reducing the occurrence of polarization on the electrode 3 and reducing lithium plating of the electrode 3 in the battery.
[0081] Optionally, the sum of the thicknesses of the film layer 30 and the current collector 1 in the second portion 102 is greater than or equal to the sum of the thicknesses of the film layer 30 and the current collector 1 in the first portion 101 .
[0082] Continuing with Figure 4 , the film layer 30 has a thickness h1 in the first portion 101 and a thickness h2 in the second portion 102. The current collector 1 has a thickness d1 in the first portion 101 and a thickness d2 in the second portion. In other words, d1 + h1 ≤ d2 + h2. In other words, the thickness of the pole piece 3 in the second portion 102 is greater than or equal to the thickness of the pole piece 3 in the first portion 101.
[0083] Specifically, ideally, the electrode piece 3 obtained by a single rolling process has a uniform thickness, i.e., d1 + h1 = d2 + h2. However, in actual production and processing, this equation is not absolute. Since the current collector is not completely flat and has a special surface structure, the thickness of the electrode piece 3 in the second portion 102 may be slightly greater than that in the first portion 101.
[0084] Optionally, the sum of the thicknesses of the film layer and the current collector in the second portion is 1%-3% greater than the sum of the thicknesses of the film layer and the current collector in the first portion. In other words, the thickness of the pole piece 3 in the second portion 102 is slightly greater than the thickness of the pole piece 3 in the first portion 101, specifically, greater than 1%-3%.
[0085] In this embodiment, when the sum of the thickness of the film layer 3 and the current collector 1 in the second part 102 is equal to the sum of the thickness of the film layer 3 and the current collector 1 in the first part 101, it means that the thickness of the electrode is uniform throughout the entire coating area 10, so that after the electrode is assembled into a battery, the spacing between the positive electrode and the negative electrode in the battery is equal everywhere, effectively avoiding battery polarization caused by the unequal spacing between the positive and negative electrode during the battery cycle, and effectively improving the lithium plating problem of the battery. If there is a certain error in the processing process, when the sum of the thickness of the film layer 3 and the current collector 1 in the second part 102 is greater than the sum of the thickness of the film layer 3 and the current collector 1 in the first part 101, since the thicker part is the second part 102, that is, the middle part of the electrode, most of the electrochemical reactions on the electrode occur in the middle part of the electrode, thereby helping to reduce the active ion migration distance between the positive and negative electrode during the battery cycle, helping to improve ion dynamics, thereby reducing the polarization phenomenon in the middle part of the electrode, and improving the lithium plating problem of the electrode.
[0086] The following describes a specific embodiment in which the current collector 1 is used in a negative electrode sheet and a positive electrode sheet.
[0087] [Negative electrode]
[0088] The negative electrode sheet generally includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0089] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0090] Alternatively, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer substrate (such as a substrate made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0091] Alternatively, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0092] Optionally, the negative electrode film layer further includes a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0093] Optionally, in one embodiment, the negative electrode film layer further includes a conductive agent, which can be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0094] Optionally, the negative electrode film layer further includes other additives, such as a thickener (such as sodium carboxymethyl cellulose (CMC-Na)).
[0095] Optionally, in one embodiment, the current collector 1 is a negative electrode current collector, and the film layer 30 is a negative electrode film layer. The compaction density of the negative electrode film layer in the first portion 101 is 1 g / cm 3 -1.65g / cm 3 , preferably 1.45 g / cm 3 -1.6g / cm 3 , more preferably 1.5 g / cm 3 -1.55g / cm 3 The compaction density of the negative electrode film layer in the second part 102 is 0.9g / cm 3 -1.5g / cm 3 , preferably 1.3 g / cm 3 -1.5g / cm 3 , more preferably 1.35 g / cm 3 -1.45g / cm 3 .
[0096] In some embodiments, the negative electrode sheet can be prepared by forming a negative electrode slurry using the aforementioned components for preparing the negative electrode sheet. For example, the negative electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., N-methylpyrrolidone) to form the negative electrode slurry. The negative electrode slurry is then coated onto the current collector 1. After drying and cold pressing, the negative electrode sheet is obtained.
[0097] [Positive electrode]
[0098] The positive electrode sheet generally includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0099] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0100] Alternatively, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0101] Optionally, the positive electrode active material may adopt the positive electrode active material for batteries known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0102] Optionally, the positive electrode material may further include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0103] Optionally, the positive electrode material layer may further contain a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0104] Optionally, in one embodiment, the current collector 1 is a positive electrode current collector, and the film layer 30 is a positive electrode film layer. The compaction density of the positive electrode film layer in the first portion 101 is 2.3 g / cm 3 -2.5g / cm 3 , preferably 2.4 g / cm 3 The compaction density of the positive electrode film layer in the second part 102 is 2.2g / cm 3 -2.4g / cm 3 , preferably 2.35 g / cm 3 .
[0105] Optionally, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder, the additive and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the current collector 1, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0106] [Electrolytes]
[0107] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0108] Optionally, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0109] Alternatively, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0110] Optionally, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0111] Optionally, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0112] [Isolator]
[0113] Optionally, the battery further includes a separator. The present application has no particular limitation on the type of separator, and any well-known porous structure separator with good chemical and mechanical stability can be selected.
[0114] Optionally, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The separator can be a separator, which can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0115] Alternatively, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly by a winding process or a lamination process. The wound electrode assembly can be cylindrical, square, or any other shape. For example, FIG5 is a schematic diagram of a cylindrical electrode assembly 5 as an example. As shown in FIG5 , the tab portion 21 of the positive electrode sheet is wound to form the positive electrode tab 51 of the electrode assembly 5, and the tab portion 21 of the negative electrode sheet is wound to form the negative electrode tab 52 of the electrode assembly 5. The coating area 10 of the positive and negative electrode sheets and the separator are wound to form the middle portion 53 of the electrode assembly 5.
[0116] An embodiment of the present application further provides a battery cell, which includes the pole piece in any embodiment of the present application.
[0117] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0118] In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the battery cell may be a soft shell, such as a pouch-type soft shell. The soft shell may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0119] The present application has no particular limitation on the shape of the battery cell, which may be cylindrical, square, or any other shape.
[0120] An embodiment of the present application further provides a battery, which includes at least one battery cell according to an embodiment of the present application.
[0121] In some embodiments, multiple battery cells are first assembled into a battery module, which is then installed in a battery housing to form a battery pack. In other production and processing techniques, multiple battery cells can be directly installed in a housing to form a battery pack, eliminating the intermediate battery module stage, thereby reducing the mass of the battery pack and increasing the energy density of the battery. This second production and processing technique can also be referred to as a cell-to-pack packaging technique, where the battery pack is referred to as a battery in this application.
[0122] In addition, the present application also provides an electrical device, comprising at least one of the battery cells or batteries described in any embodiment of the present application. The battery cells or batteries can serve as a power source for the electrical device or as an energy storage unit for the electrical device. Electrical devices may include vehicles, mobile phones, portable devices, laptop computers, ships, spacecraft, electric toys, and power tools, among others. Vehicles may include fuel-powered vehicles, gas-powered vehicles, or new energy vehicles; new energy vehicles may include pure electric vehicles, hybrid vehicles, or extended-range vehicles; spacecraft include aircraft, rockets, space shuttles, and spacecraft; electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys; and power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, among others, but the present application is not limited thereto.
[0123] As an example of an electric device, the electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the electric device's requirements for high power and high energy density of the battery, a battery module or battery can be used as a power source.
[0124] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be lightweight and thin, and may use a battery cell as a power source.
[0125] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0126] Example 1
[0127] (1) Preparation of positive electrode current collector
[0128] On both sides of the aluminum foil with a thickness of 13 μm, the two side areas of the foil are thickened by ultrasonic welding to form the first part 101. Finally, the thickness of the first part 101 is 17 μm, the thickness of the second part 102 is 13 μm, and the width of the second part 102 in the first direction k accounts for 2 / 3 of the width of the coating area 10 in the first direction k, thereby obtaining the positive electrode current collector 1.
[0129] (2) Preparation of positive electrode sheet
[0130] The positive electrode active material lithium iron phosphate, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are dissolved in the solvent N-methylpyrrolidone (NMP) at a mass ratio of 97:0.8:2.2, and the mixture is stirred thoroughly to obtain a positive electrode slurry. The positive electrode slurry is then evenly coated on the coating area 10 of the positive electrode current collector 1, and then dried, cold pressed, and cut to obtain a positive electrode sheet. The density of the first part 101 of the positive electrode sheet is 2.4g / cm 3 The density of the second part 102 is 2.35 g / cm 3 .
[0131] (3) Preparation of negative electrode sheet
[0132] The negative electrode active material graphite, conductive agent acetylene black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) were dissolved in deionized water at a mass ratio of 97:0.4:1.6:1 and mixed thoroughly to produce a negative electrode slurry. The slurry was then evenly coated onto the negative electrode current collector copper foil, followed by drying, cold pressing, and slitting to produce negative electrode sheets.
[0133] (4) Assembly of battery cells
[0134] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order so that the separator is located between the positive electrode sheet and the negative electrode sheet and can isolate the positive electrode sheet from the negative electrode sheet; the stacked components are then wound to obtain an electrode assembly; the electrode assembly is placed in a shell, and after drying, an LiPF6 electrolyte with a mass fraction of 11% is injected; and a battery cell is obtained after processes such as formation and standing.
[0135] Example 2
[0136] (1) Preparation of positive electrode sheet
[0137] The positive electrode active material, lithium iron phosphate, the conductive agent, acetylene black, and the binder, polyvinylidene fluoride (PVDF), were dissolved in the solvent N-methylpyrrolidone (NMP) at a mass ratio of 97:0.8:2.2. The mixture was thoroughly stirred and mixed to obtain a positive electrode slurry. The slurry was then evenly coated onto the positive electrode current collector aluminum foil, followed by drying, cold pressing, and slitting to obtain the positive electrode sheets.
[0138] (2) Preparation of negative electrode current collector
[0139] On both sides of a copper foil with a thickness of 6 μm, the two side areas of the foil are thickened by ultrasonic welding to form a first part 101. Finally, the thickness of the first part 101 is 9 μm, the thickness of the second part 102 is 6 μm, and the width of the second part 102 in the first direction k accounts for 2 / 3 of the width of the coating area 10 in the first direction k, thereby obtaining a negative electrode current collector 1.
[0140] (3) Preparation of negative electrode sheet
[0141] The negative electrode active material graphite, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are dissolved in deionized water at a mass ratio of 97:0.4:1.6:1 and mixed evenly to obtain a negative electrode slurry. The negative electrode slurry is then evenly coated on the coating area 10 of the negative electrode current collector, and then dried, cold pressed, and cut to obtain a negative electrode sheet. The first part 101 of the negative electrode sheet has a density of 1.5 g / cm 3 The density of the second part 102 is 1.45 g / cm 3 .
[0142] (4) Assembly of battery cells
[0143] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order so that the separator is located between the positive electrode sheet and the negative electrode sheet and can isolate the positive electrode sheet from the negative electrode sheet; the stacked components are then wound to obtain an electrode assembly; the electrode assembly is placed in a shell, and after drying, an LiPF6 electrolyte with a mass fraction of 11% is injected; and a battery cell is obtained after processes such as formation and standing.
[0144] Example 3
[0145] Compared with the battery cell of Example 1, Example 3 only changes the negative electrode current collector. The negative electrode current collector in Example 3 is replaced by the common copper foil to the negative electrode current collector 1 same as that in Example 2.
[0146] Example 4
[0147] (1) Preparation of positive electrode current collector
[0148] The positive electrode current collector of Example 4 was prepared using the same preparation method as Example 1 to obtain a positive electrode current collector 1.
[0149] (2) Preparation of positive electrode sheet
[0150] The positive electrode active material Na 0.85 Ni 0.25 Mn 0.75 O2, acetylene black as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder were dissolved in N-methylpyrrolidone (NMP) at a mass ratio of 90:5:5 and thoroughly stirred to obtain a positive electrode slurry. The positive electrode slurry was then evenly coated on the coating area 10 of the positive electrode current collector 1. The positive electrode sheet was then dried, cold pressed, and cut. The density of the first portion 101 of the positive electrode sheet was 2.4 g / cm 3 The second part has a density of 2.35 g / cm 3 .
[0151] (3) Preparation of negative electrode sheet
[0152] The negative electrode active material, hard carbon, the conductive agent, acetylene black, the binder, styrene-butadiene rubber (SBR), and the thickener, sodium carboxymethyl cellulose (CMC), were dissolved in deionized water at a mass ratio of 97:0.4:1.6:1 and mixed thoroughly to produce a negative electrode slurry. The slurry was then evenly coated onto the negative electrode current collector copper foil, followed by drying, cold pressing, and slitting to produce negative electrode sheets.
[0153] (4) Assembly of battery cells
[0154] The battery cell 4 of Example 4 is prepared by the same method as that of Example 1, with the only difference being that an electrolyte containing 11% by mass of NaPF6 is used, which will not be described in detail here.
[0155] Comparative Example 1
[0156] Comparative Example 1 Compared with the battery cell of Example 1, Comparative Example 1 only changes the choice of positive electrode current collector, that is, ordinary aluminum foil is used instead of positive electrode current collector 1. The battery cell of Comparative Example 1 is prepared by the same preparation method as Example 1.
[0157] Comparative Example 2
[0158] The only difference between the battery cells of Comparative Example 2 and Example 4 is that Comparative Example 2 uses ordinary aluminum foil as the positive electrode current collector.
[0159] The product parameters of different embodiments are detailed in Table 1.
[0160] Table 1: Product parameters of comparative examples and different embodiments
[0161]
[0162]
[0163] In Table 1, 101 refers to the first portion of the coating region 10 , and 102 refers to the second portion of the coating region 10 .
[0164] The battery performance test results of the above Examples 1-4 and Comparative Example 1 are detailed in Table 2.
[0165] Table 2: Cycle life test results of comparative examples and different embodiments
[0166] Example Cycle life (cycles) 15527250193623145503Comparative example 14008Comparative example 23996
[0167] Next, a brief introduction to the parameter testing process of the above-mentioned battery is given.
[0168] 1. Battery performance test
[0169] At 25°C, the secondary batteries prepared in each example and comparative example were charged at a constant current rate of 1C to a charge cutoff voltage V1, then charged at a constant voltage rate to a current ≤ 0.05C, allowed to rest for 5 minutes, and then discharged at a constant current rate of 0.33C to a discharge cutoff voltage V2, allowed to rest for 5 minutes. This constitutes one charge-discharge cycle. The batteries were subjected to cyclic charge-discharge testing using this method until the battery capacity decayed to 80%. The number of cycles at this point is the battery's cycle life. The test results are shown in Table 2.
[0170] From the performance comparison between Example 1 and Comparative Example 1, and Example 2 and Comparative Example 1, it can be seen that by using the current collector with a special structure provided by the present application, whether it is applied in the positive electrode or the negative electrode, the cycle performance of the battery can be effectively improved, helping to extend the service life of the battery. Furthermore, from the performance comparison between Example 3 and Example 1, and the performance comparison between Example 3 and Example 2, it can be seen that if the current collector with a special structure is used at the positive and negative electrodes of the battery at the same time, the battery polarization can be further suppressed and the cycle performance of the battery can be improved. From the performance comparison between Example 4 and Comparative Example 2, it can be seen that when the current collector with a special structure is applied to a sodium ion battery, it can also effectively improve the cycle performance of the battery.
[0171] 2. Lithium deposition test
[0172] Under 1C / 1C (charge and discharge conditions), when the battery SOH reached 70%, the battery cells in Example 1 and Comparative Example 1 were disassembled, and photos of the negative electrode plates were obtained, as shown in Figures 6 and 7, respectively. As can be seen from Figures 6 and 7, after the charge and discharge cycles of Example 1 using the electrode provided by the present application, no lithium metal was deposited on the surface of the negative electrode plate, while after the charge and discharge cycles of Comparative Example 1, obvious lithium metal deposition was observed on the negative electrode plate. This fully demonstrates that the electrode provided by the present application can effectively reduce the polarization of the battery during the cycle process, inhibit the lithium deposition phenomenon of the battery, and thus improve the cycle performance and safety performance of the battery.
[0173] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A current collector, wherein: The current collector includes: a first portion, the first portion being arranged along a first direction, the first direction being a width direction of the current collector or a length direction of the current collector; a second part, the second part being arranged between the two first parts; The first part and the second part are used to support a film layer, the first part has a first thickness, the second part has a second thickness, and the first thickness is greater than the second thickness.
2. The current collector according to claim 1, wherein The ratio of the width of the second portion in the first direction to the sum of the widths of the first portion and the second portion in the first direction is 30%-70%, preferably 40%-60%.
3. The current collector according to claim 1 or 2, wherein: The current collector includes: A tab portion is connected to the first portion in the first direction, and a thickness of the tab portion is less than or equal to a thickness of the first portion.
4. The current collector according to any one of claims 1 to 3, wherein The first thickness is 10 μm-20 μm, preferably 12 μm-18 μm; the second thickness is 1 μm-20 μm, preferably 6 μm-17 μm.
5. The current collector according to any one of claims 1 to 4, wherein A film layer is provided on the first part and the second part, and a compaction density of the film layer in the first part is greater than a compaction density of the film layer in the second part. The current collector according to claim 5 , wherein: The current collector is a positive electrode current collector, the film layer is a positive electrode film layer, and the compaction density of the positive electrode film layer in the first part is 1.5 g / cm 3 -2.6g / cm 3 , preferably 2.4 g / cm 3 The compaction density of the positive electrode film layer in the second part is 2.2g / cm 3 -2.45g / cm 3 , preferably 2.35 g / cm 3 .
7. The current collector according to claim 5, wherein: The current collector is a negative electrode current collector, the film layer is a negative electrode film layer, and the compaction density of the negative electrode film layer in the first part is 1g / cm 3 -1.65g / cm 3 , preferably 1.5 g / cm 3 The compaction density of the negative electrode film layer in the second part is 0.9g / cm 3 -1.5g / cm 3 , preferably 1.45 g / cm 3 .
8. The current collector according to claim 5, wherein The sum of the thicknesses of the film layer and the current collector in the second portion is greater than or equal to the sum of the thicknesses of the film layer and the current collector in the first portion.
9. The current collector according to claim 8, wherein The sum of the thicknesses of the film layer and the current collector in the second portion is 1%-3% greater than the sum of the thicknesses of the film layer and the current collector in the first portion.
10. The current collector according to any one of claims 1 to 9, wherein The first portion is obtained by thickening the current collector.
11. The current collector according to any one of claims 1 to 9, wherein The second portion is obtained by thinning the current collector.
12. A pole piece, wherein: The pole piece includes the current collector according to any one of claims 1 to 11.
13. A battery cell, wherein: The battery cell includes the pole piece according to claim 12.
14. A battery, characterized in that: The battery comprises at least one battery cell according to claim 13 .
15. An electrical device, characterized in that: The electrical device comprises at least one of the battery cell according to claim 12 or the battery according to claim 13 , and the battery cell and / or the battery are used to supply power to the electrical device.