Self-excitation microcapsule structure fire extinguishing material
By adding thermal filler and layered shell structure to the microcapsule fire extinguishing materials, the problem of uneven release of fire extinguishing materials caused by uneven temperature at the fire site is solved, and a more efficient and lasting fire extinguishing effect is achieved.
Patent Information
- Application Number
- CN202411120374.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Due to the uneven temperature distribution at the fire site, the fire extinguishing materials in some areas cannot be fully released in time, affecting the fire extinguishing effect.
The self-excited microcapsule structure fire extinguishing material is used. By adding thermal fillers such as graphene, carbon nanotubes and modified alumina to the microcapsules, the thermal conductivity of the microcapsules is improved, and the heat is transferred more evenly, and the release of the capsule core substance is promoted. , and encapsulation stability is enhanced by a layered shell structure.
A more synchronous and efficient fire extinguishing effect is achieved, avoiding the problem of partial microcapsules not being released due to local heating, improving the utilization efficiency and durability of fire extinguishing materials, and ensuring the smooth release of perfluorohexanone.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fire extinguishing materials, and in particular to a self-exciting microcapsule structured fire extinguishing material. Background Art
[0002] The perfluorohexanone fire extinguishing system adopts the principle of chemical fire extinguishing, that is, the fire environment is changed by releasing the fire extinguishing agent to achieve the effect of fire extinguishing. Perfluorohexanone is a colorless, odorless, non-toxic gas. After release, it quickly evaporates into an inert gas. It has the following working principles: 1. Inhibit chain reaction: Perfluorohexanone can inhibit the chain reaction of fire, block the spread of flames, and reduce the fire. 2. Reduce oxygen concentration: After release, perfluorohexanone evaporates into an inert gas, reducing the oxygen concentration at the fire scene so that combustion will no longer continue. 3. Quickly extinguish the fire source: Perfluorohexanone has a fast fire extinguishing speed, which can quickly extinguish the fire source and reduce the losses caused by the fire.
[0003] The flexible fire extinguishing sheet adopts microcapsule technology, and the fire extinguishing medium perfluorohexanone is coated by the capsule shell. When the multiple microcapsule shells in the fire extinguishing sheet are heated to a certain temperature, they rupture and release the fire extinguishing medium perfluorohexanone. Since the fire at different locations on the fire scene is of different sizes, the different locations of the fire extinguishing patch are at different distances from the fire source, resulting in uneven heating of the microcapsule particles at different locations in the fire extinguishing patch, so that the fire extinguishing medium in some areas cannot be fully released in time, affecting the fire extinguishing effect. Therefore, the present application proposes a self-exciting microcapsule structure fire extinguishing material. Therefore, the present application proposes a self-exciting microcapsule structure fire extinguishing material. Summary of the invention
[0004] The purpose of the present invention is to propose a self-exciting microcapsule structured fire extinguishing material to address the problem in the background technology that the fire extinguishing material in some areas cannot be fully released in time due to the uneven temperature distribution at the fire scene.
[0005] The technical solution of the present invention is a self-exciting microcapsule structure fire extinguishing material, comprising the following raw materials in parts by weight:
[0006] Capsule core: 50-60 parts of perfluorohexanone;
[0007] Capsule shell: including a first shell and a second shell, the first shell includes: 16-20 parts of chitosan, 1-2 parts of nano titanium dioxide, 5-7 parts of nano iron oxide, and the second shell includes: 20-30 parts of polyamide resin;
[0008] Thermal conductive filler: 1-3 parts of graphene, 1-3 parts of carbon nanotubes, 2-4 parts of modified alumina.
[0009] Optionally, the preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0010] S1. Solution and dispersion preparation
[0011] Dissolve chitosan in 130-140 parts of acetic acid solution to form solution A;
[0012] Dissolving a polyamide resin in 135-145 parts of an ethanol solution to form a solution B;
[0013] Dispersing nano titanium dioxide and nano iron oxide in 85-90 parts of deionized water to form a nano oxide dispersion C;
[0014] Dispersing graphene and carbon nanotubes in 95-100 parts of deionized water respectively to obtain dispersion D and dispersion E, and then mixing dispersion D and dispersion E evenly to obtain graphene / carbon nanotube mixed dispersion F;
[0015] S2. Emulsification of capsule core
[0016] Add perfluorohexanone to solution A, stir with a high-speed stirrer to fully disperse the perfluorohexanone in solution A to form emulsion droplets, and the uniformly distributed emulsion droplets form emulsion G;
[0017] S3. First shell formation
[0018] Under stirring, the nano-oxide dispersion C is added dropwise to the emulsion G for 40-50 minutes, and then stirred at 50°C-60°C for 2-3 hours to evaporate the solvent, so that the chitosan is cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0019] S4. Second shell formation
[0020] Add solution B dropwise to the emulsion that has formed the first shell layer for 25-35 minutes, stir at 50-60°C and 350-450rpm for 2-3 hours and evaporate the solvent, so that the polyamide resin forms a second shell layer outside the first shell layer, and obtain an emulsion with two shell layers;
[0021] S5. Introduction of thermal conductive filler
[0022] Dispersing the graphene / carbon nanotube mixed dispersion F and modified alumina in 90-95 parts of deionized water to form a thermal conductive filler mixed dispersion H;
[0023] Add the thermal conductive filler mixed dispersion H dropwise into the emulsion of the two shell layers for 40-50 minutes, and stir at 50-60°C and 300-500 rpm for 1-2 hours to evenly distribute the thermal conductive filler on the surface of the microcapsule and in the shell layer;
[0024] S6. Post-processing
[0025] The microcapsules are collected by filtration, washed with deionized water for 3-5 times to remove residual solvent and unreacted substances, and then vacuum dried at 50-60° C. for 15-18 hours to obtain a microcapsule fire extinguishing material.
[0026] Optionally, the specific preparation steps of the modified alumina are as follows:
[0027] Step 1: Add alumina powder to a 3%-7% silane coupling agent ethanol solution, and stir to allow the silane coupling agent molecules to be initially grafted onto the alumina surface;
[0028] Step 2: Add dopamine hydrochloride to the above reaction system and continue stirring to mix and react;
[0029] Step 3: Filter the reaction product and wash it with ethanol to remove unreacted substances;
[0030] Step 4: dispersing the washed product in deionized water, and then adding a silver nitrate solution with a concentration of 0.08-0.12 mol / L dropwise, and allowing the silver ions to react with the functional groups on the surface of the alumina under stirring to form alumina loaded with silver nanoparticles;
[0031] Step 5: Filter the silver nanoparticle-loaded alumina, wash with deionized water, and vacuum dry to obtain modified alumina.
[0032] Optionally, in step 2, the stirring temperature is 55-65° C., and the reaction is carried out at a stirring speed of 280-320 rpm for 1.5-2.5 hours.
[0033] Optionally, the following raw materials are included in parts by weight:
[0034] Capsule core: 52-58 parts of perfluorohexanone;
[0035] Capsule shell: including the first shell and the second shell;
[0036] The first shell layer includes: 17-19 parts of chitosan, 1-2 parts of nano titanium dioxide, and 6-7 parts of nano iron oxide;
[0037] The second shell comprises: 22-28 parts of polyamide resin;
[0038] Thermal conductive filler: 1-2 parts of graphene, 1-2 parts of carbon nanotubes, 3-4 parts of modified alumina.
[0039] Optionally, the following raw materials are included in parts by weight:
[0040] Capsule core: 55 parts of perfluorohexanone;
[0041] Capsule shell: including the first shell and the second shell;
[0042] The first shell layer includes: 18 parts of chitosan, 1.52 parts of nano titanium dioxide, and 6 parts of nano iron oxide;
[0043] The second shell comprises: 25 parts of polyamide resin;
[0044] Thermal conductive filler: 2 parts of graphene, 2 parts of carbon nanotubes, and 3 parts of modified alumina.
[0045] Optionally, in S2, the high-speed stirrer stirs at a rotation speed of 8000-10000 rpm for 20-30 minutes.
[0046] Optionally, in S3, the rotation speed is 350-450 rpm.
[0047] Optionally, the microcapsule fire extinguishing material further includes a connecting layer fixedly connected to the capsule shell and a bottom layer connected to the connecting layer.
[0048] Optionally, the connecting layer is a foam-based double-sided adhesive, and the bottom layer is a non-woven fabric.
[0049] Compared with the prior art, the present invention has at least one of the following beneficial technical effects:
[0050] In the microcapsule fire extinguishing material prepared by the present invention, perfluorohexanone is used as the capsule core fire extinguishing medium, and the fire can be quickly and effectively extinguished. Microencapsulation can effectively encapsulate perfluorohexanone in the capsule core, protect it from leakage or deterioration before storage and use, ensure the stability and effectiveness of the fire extinguishing component, and the layered capsule shell structure provides multiple protections, further enhancing the stability of the encapsulation.
[0051] By adding fillers with good thermal conductivity, such as graphene, carbon nanotubes, and modified alumina, the thermal conductivity of the microcapsules can be improved, so that heat can be transferred more evenly to the inside of the microcapsules, promoting the release of the capsule core material. When the thermal conductivity of the capsule shell is improved, the heat absorbed by one microcapsule can be transferred to the adjacent microcapsules more quickly. This helps to form a more uniform temperature distribution in the fire scene, so that more microcapsules can reach the fire extinguishing trigger temperature at the same time, thereby achieving a more synchronous and efficient fire extinguishing effect. In the case of local heating, the good thermal conductivity capsule shell can quickly diffuse the heat to avoid the situation where only some microcapsules are heated and released while other parts do not respond. This allows the microcapsules as a whole to play a more coordinated fire extinguishing role, and at the same time, the heat absorbed by the microcapsules can be transferred to adjacent microcapsules more quickly, improving the utilization efficiency of the fire extinguishing materials and the comprehensiveness of the fire extinguishing. Uniform heat conduction also helps to control the release rate and total amount of perfluorohexanone, making its release more stable and continuous, and enhancing the durability of fire extinguishing.
[0052] The loading of silver nanoparticles increases the thermal conductivity channels of alumina, further improving its thermal conductivity. When compounded with graphene and carbon nanotubes, a denser thermal conductivity network can be formed, synergistically improving the overall thermal conductivity of the microcapsules. The presence of the polydopamine layer increases the surface activity and roughness of alumina, making it easier to interact with graphene and carbon nanotubes, improving their dispersibility and compatibility in microcapsules. Good dispersibility helps to reduce agglomeration and give full play to the excellent properties of graphene and carbon nanotubes, thereby achieving a synergistic effect. DETAILED DESCRIPTION
[0053] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0054] In the following examples and comparative examples, the specific preparation steps of modified alumina are as follows:
[0055] Step 1: Add 10g of alumina powder to 50mL of 5% KH-570 silane coupling agent ethanol solution, and react at 55°C with a stirring speed of 300rpm for 4 hours to initially graft the silane coupling agent molecules onto the alumina surface;
[0056] Step 2: Add 2 g of dopamine hydrochloride to the above reaction system, and react at 60° C. and 300 rpm for 2 hours;
[0057] Step 3: Filter the reaction product and wash it with ethanol three times to remove unreacted substances;
[0058] Step 4: The washed product was dispersed in 100 mL of deionized water, and then 50 mL of a 0.1 mol / L silver nitrate solution was added dropwise, and the mixture was stirred at 200 rpm for 2 hours to allow the silver ions to react with the functional groups on the surface of the alumina to form alumina loaded with silver nanoparticles;
[0059] Step 5: Filter the silver nanoparticle-loaded alumina, wash it three times with deionized water, and then vacuum dry it at 70° C.-80° C. for 10-12 hours to obtain modified alumina.
[0060] Through this solution, the modified alumina improves its own thermal conductivity through surface modification and loading of silver nanoparticles. When they are present in a microcapsule system as thermal conductive fillers, the modified alumina conducts heat in multiple directions.
[0061] Example 1
[0062] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0063] Capsule core: perfluorohexanone 50g;
[0064] Capsule shell: chitosan 16g, nano titanium dioxide 1g, nano iron oxide 5g, polyamide resin 20g;
[0065] Thermal conductive filler: graphene 1g, carbon nanotube 1g, modified alumina 2g;
[0066] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0067] Dissolve chitosan in 130 g of acetic acid solution to form solution A;
[0068] Dissolve the polyamide resin in 135 g of ethanol solution to form solution B;
[0069] Dispersing nano titanium dioxide and nano iron oxide in 85 g of deionized water to form a nano oxide dispersion C;
[0070] Dispersing graphene and carbon nanotubes in 95 g of deionized water respectively to obtain dispersion D and dispersion E, and then mixing dispersion D and dispersion E to obtain graphene / carbon nanotube mixed dispersion F;
[0071] Perfluorohexanone was added to solution A, and stirred at 8000 rpm for 20 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0072] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 40 minutes, and then stirred at 50°C and 350 rpm for 2 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0073] Solution B is added dropwise to the emulsion that has formed the first shell layer for 25-35 minutes, and the mixture is stirred at 50°C and 350 rpm for 2 hours to evaporate the solvent, so that the polyamide resin forms a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0074] Dispersing graphene / carbon nanotube mixed dispersion F and modified alumina in 90 g of deionized water to form a thermal conductive filler mixed dispersion H; dropping the thermal conductive filler mixed dispersion H into the emulsion of the two-layer shell for 40 minutes, stirring at 50° C. and 300 rpm for 1 hour to evenly distribute the thermal conductive filler on the surface and shell of the microcapsule;
[0075] The microcapsules were collected by filtration, washed three times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 50°C for 15 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided tape, and the other side of the foam substrate double-sided tape was adhered to a torn non-woven fabric to obtain a self-exciting microcapsule structure fire extinguishing material.
[0076] Example 2
[0077] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0078] Capsule core: perfluorohexanone 52g;
[0079] Capsule shell: chitosan 17g, nano titanium dioxide 1.2g, nano iron oxide 5.5g, polyamide resin 22g;
[0080] Thermal conductive filler: graphene 1.5g, carbon nanotubes 1.5g, modified alumina 2.5g;
[0081] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0082] Dissolve chitosan in 132 g of acetic acid solution to form solution A;
[0083] Dissolve the polyamide resin in 137 g of ethanol solution to form solution B;
[0084] Dispersing nano titanium dioxide and nano iron oxide in 86 g of deionized water to form a nano oxide dispersion C;
[0085] Dispersing graphene and carbon nanotubes in 96 g of deionized water respectively to obtain dispersion D and dispersion E, and then mixing dispersion D and dispersion E to obtain graphene / carbon nanotube mixed dispersion F;
[0086] Perfluorohexanone was added to solution A, and stirred at 8500 rpm for 22 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0087] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 42 minutes, and then stirred at 52°C at a speed of 370 rpm for 2.2 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0088] Solution B was added dropwise to the emulsion that had formed the first shell layer for 28 minutes, and the mixture was stirred at 52° C. and 380 rpm for 2.2 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0089] Dispersing graphene / carbon nanotube mixed dispersion F and modified alumina in 91 g of deionized water to form a thermal conductive filler mixed dispersion H; dropping the thermal conductive filler mixed dispersion H into the emulsion of the two-layer shell for 42 minutes, stirring at 52° C. and 350 rpm for 1.2 hours to evenly distribute the thermal conductive filler on the surface and shell of the microcapsule;
[0090] The microcapsules were collected by filtration, washed four times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 52°C for 16 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided adhesive tape, and the other side of the foam substrate double-sided adhesive tape was adhered to a torn non-woven fabric to obtain a self-exciting microcapsule structure fire extinguishing material.
[0091] Example 3
[0092] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0093] Capsule core: perfluorohexanone 55g;
[0094] Capsule shell: chitosan 18g, nano titanium dioxide 1.5g, nano iron oxide 6g, polyamide resin 25g;
[0095] Thermal conductive filler: graphene 2g, carbon nanotubes 2g, modified alumina 3g;
[0096] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0097] Dissolve chitosan in 135 g of acetic acid solution to form solution A;
[0098] Dissolving a polyamide resin in 140 g of an ethanol solution to form a solution B;
[0099] Dispersing nano titanium dioxide and nano iron oxide in 87.5 g of deionized water to form a nano oxide dispersion C;
[0100] Dispersing graphene and carbon nanotubes in 97.5 g of deionized water respectively to obtain dispersions D and E, and then mixing dispersions D and E to obtain graphene / carbon nanotube mixed dispersion F;
[0101] Perfluorohexanone was added to solution A, and stirred at 9000 rpm for 25 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0102] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 45 minutes, and then stirred at 55°C at a speed of 400 rpm for 2.5 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0103] Solution B was added dropwise to the emulsion that had formed the first shell layer for 30 minutes, and the mixture was stirred at 55°C and 400 rpm for 2.5 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0104] Dispersing the graphene / carbon nanotube mixed dispersion F and modified alumina in 92.5 g of deionized water to form a thermal conductive filler mixed dispersion H; dropping the thermal conductive filler mixed dispersion H into the emulsion of the two-layer shell for 45 minutes, stirring at 55° C. and 400 rpm for 1.5 hours to evenly distribute the thermal conductive filler on the surface and shell of the microcapsule;
[0105] The microcapsules were collected by filtration, washed four times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 55°C for 16.5 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided adhesive tape, and the other side of the foam substrate double-sided adhesive tape was adhered to a torn non-woven fabric to obtain a self-excited microcapsule structure fire extinguishing material.
[0106] Example 4
[0107] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0108] Capsule core: perfluorohexanone 58g;
[0109] Capsule shell: chitosan 19g, nano titanium dioxide 1.8g, nano iron oxide 6.5g, polyamide resin 27.5g;
[0110] Thermal conductive filler: graphene 2.5g, carbon nanotubes 2.5g, modified alumina 3.5g;
[0111] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0112] Dissolve chitosan in 137.5 g of acetic acid solution to form solution A;
[0113] Dissolving a polyamide resin in 142 g of an ethanol solution to form a solution B;
[0114] Dispersing nano titanium dioxide and nano iron oxide in 88 g of deionized water to form a nano oxide dispersion C;
[0115] Dispersing graphene and carbon nanotubes in 99 g of deionized water respectively to obtain dispersion D and dispersion E, and then mixing dispersion D and dispersion E to obtain graphene / carbon nanotube mixed dispersion F;
[0116] Perfluorohexanone was added to solution A, and stirred at 9500 rpm for 28 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0117] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 48 minutes, and then stirred at 58°C at a speed of 425 rpm for 2.8 hours to evaporate the solvent and cross-link and solidify the chitosan on the surface of the emulsion droplets to form the first shell layer;
[0118] Solution B was added dropwise to the emulsion that had formed the first shell layer for 32 minutes, and the mixture was stirred at 58°C and 420 rpm for 2.8 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0119] Dispersing graphene / carbon nanotube mixed dispersion F and modified alumina in 94 g of deionized water to form a thermal conductive filler mixed dispersion H; dropping the thermal conductive filler mixed dispersion H into the emulsion of the two-layer shell for 48 minutes, stirring at 58° C. and 480 rpm for 1.8 hours to evenly distribute the thermal conductive filler on the surface and shell of the microcapsule;
[0120] The microcapsules were collected by filtration, washed four times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 58°C for 17 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided tape, and the other side of the foam substrate double-sided tape was adhered to a torn non-woven fabric to obtain a self-exciting microcapsule structure fire extinguishing material.
[0121] Example 5
[0122] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0123] Capsule core: perfluorohexanone 60g;
[0124] Capsule shell: chitosan 20g, nano titanium dioxide 2g, nano iron oxide 7g, polyamide resin 30g;
[0125] Thermal conductive filler: graphene 3g, carbon nanotubes 3g, modified alumina 4g;
[0126] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0127] Dissolve chitosan in 140 g of acetic acid solution to form solution A;
[0128] Dissolve the polyamide resin in 145 g of ethanol solution to form solution B;
[0129] Dispersing nano titanium dioxide and nano iron oxide in 90 g of deionized water to form a nano oxide dispersion C;
[0130] Dispersing graphene and carbon nanotubes in 100 g of deionized water respectively to obtain dispersion D and dispersion E, and then mixing dispersion D and dispersion E to obtain graphene / carbon nanotube mixed dispersion F;
[0131] Perfluorohexanone was added to solution A, and stirred at a speed of 10000 rpm for 30 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0132] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 50 minutes, and then stirred at 60°C and 450 rpm for 3 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0133] Solution B was added dropwise to the emulsion that had formed the first shell layer for 35 minutes, and the mixture was stirred at 60°C and 450 rpm for 3 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0134] Dispersing the graphene / carbon nanotube mixed dispersion F and modified alumina in 95 g of deionized water to form a thermal conductive filler mixed dispersion H; dropping the thermal conductive filler mixed dispersion H into the emulsion of the two-layer shell for 50 minutes, stirring at 60° C. and 500 rpm for 2 hours to evenly distribute the thermal conductive filler on the surface and shell of the microcapsule;
[0135] The microcapsules were collected by filtration, washed with deionized water for 5 times to remove residual solvent and unreacted substances, and then vacuum dried at 60°C for 18 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided adhesive tape, and the other side of the foam substrate double-sided adhesive tape was adhered to a torn non-woven fabric to obtain a self-exciting microcapsule structure fire extinguishing material.
[0136] Comparative Example 1
[0137] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0138] Capsule core: perfluorohexanone 55g;
[0139] Capsule shell: chitosan 18g, nano titanium dioxide 1.5g, nano iron oxide 6g, polyamide resin 25g;
[0140] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0141] Dissolve chitosan in 135 g of acetic acid solution to form solution A;
[0142] Dissolving a polyamide resin in 140 g of an ethanol solution to form a solution B;
[0143] Dispersing nano titanium dioxide and nano iron oxide in 87.5 g of deionized water to form a nano oxide dispersion C;
[0144] Perfluorohexanone was added to solution A, and stirred at 9000 rpm for 25 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0145] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 45 minutes, and then stirred at 55°C at a speed of 400 rpm for 2.5 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0146] Solution B was added dropwise to the emulsion that had formed the first shell layer for 30 minutes, and the mixture was stirred at 55°C and 400 rpm for 2.5 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0147] The microcapsules were collected by filtration, washed four times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 55°C for 16.5 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided adhesive tape, and the other side of the foam substrate double-sided adhesive tape was adhered to a torn non-woven fabric to obtain a self-excited microcapsule structure fire extinguishing material.
[0148] Comparative Example 2
[0149] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0150] Capsule core: perfluorohexanone 55g;
[0151] Capsule shell: chitosan 18g, nano titanium dioxide 1.5g, nano iron oxide 6g, polyamide resin 25g;
[0152] Thermal conductive filler: graphene 7g;
[0153] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0154] Dissolve chitosan in 135 g of acetic acid solution to form solution A;
[0155] Dissolving a polyamide resin in 140 g of an ethanol solution to form a solution B;
[0156] Dispersing nano titanium dioxide and nano iron oxide in 87.5 g of deionized water to form a nano oxide dispersion C;
[0157] Dispersing graphene in 97.5 g of deionized water to obtain dispersion F;
[0158] Perfluorohexanone was added to solution A, and stirred at 9000 rpm for 25 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0159] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 45 minutes, and then stirred at 55°C at a speed of 400 rpm for 2.5 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0160] Solution B was added dropwise to the emulsion that had formed the first shell layer for 30 minutes, and the mixture was stirred at 55°C and 400 rpm for 2.5 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0161] Dispersing the dispersion F in 92.5 g of deionized water to form a thermally conductive filler mixed dispersion H; dropping the thermally conductive filler mixed dispersion H into the emulsion of the two-layer shell for 45 minutes, stirring at 55° C. and 400 rpm for 1.5 hours to evenly distribute the thermally conductive filler on the surface of the microcapsule and in the shell layer;
[0162] The microcapsules were collected by filtration, washed four times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 55°C for 16.5 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided adhesive tape, and the other side of the foam substrate double-sided adhesive tape was adhered to a torn non-woven fabric to obtain a self-excited microcapsule structure fire extinguishing material.
[0163] Comparative Example 3
[0164] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0165] Capsule core: perfluorohexanone 55g;
[0166] Capsule shell: chitosan 18g, nano titanium dioxide 1.5g, nano iron oxide 6g, polyamide resin 25g;
[0167] Thermal conductive filler: carbon nanotubes 7g;
[0168] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0169] Dissolve chitosan in 135 g of acetic acid solution to form solution A;
[0170] Dissolving a polyamide resin in 140 g of an ethanol solution to form a solution B;
[0171] Dispersing nano titanium dioxide and nano iron oxide in 87.5 g of deionized water to form a nano oxide dispersion C;
[0172] The carbon nanotubes were dispersed in 97.5 g of deionized water to obtain dispersion F;
[0173] Perfluorohexanone was added to solution A, and stirred at 9000 rpm for 25 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0174] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 45 minutes, and then stirred at 55°C at a speed of 400 rpm for 2.5 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0175] Solution B was added dropwise to the emulsion that had formed the first shell layer for 30 minutes, and the mixture was stirred at 55°C and 400 rpm for 2.5 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0176] Dispersing the dispersion F in 92.5 g of deionized water to form a thermally conductive filler mixed dispersion H; dropping the thermally conductive filler mixed dispersion H into the emulsion of the two-layer shell for 45 minutes, stirring at 55° C. and 400 rpm for 1.5 hours to evenly distribute the thermally conductive filler on the surface of the microcapsule and in the shell layer;
[0177] The microcapsules were collected by filtration, washed four times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 55°C for 16.5 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided adhesive tape, and the other side of the foam substrate double-sided adhesive tape was adhered to a torn non-woven fabric to obtain a self-excited microcapsule structure fire extinguishing material.
[0178] Comparative Example 4
[0179] The self-exciting microcapsule structure fire extinguishing material comprises the following raw materials in parts by weight:
[0180] Capsule core: perfluorohexanone 55g;
[0181] Capsule shell: chitosan 18g, nano titanium dioxide 1.5g, nano iron oxide 6g, polyamide resin 25g;
[0182] Thermal conductive filler: modified alumina 7g;
[0183] The preparation method of the microcapsule fire extinguishing material comprises the following steps:
[0184] Dissolve chitosan in 135 g of acetic acid solution to form solution A;
[0185] Dissolving a polyamide resin in 140 g of an ethanol solution to form a solution B;
[0186] Dispersing nano titanium dioxide and nano iron oxide in 87.5 g of deionized water to form a nano oxide dispersion C;
[0187] Perfluorohexanone was added to solution A, and stirred at 9000 rpm for 25 minutes using a high-speed stirrer to form emulsion droplets, and the uniformly distributed emulsion droplets formed emulsion G;
[0188] Under stirring, the nano-oxide dispersion C was added dropwise to the emulsion G for 45 minutes, and then stirred at 55°C at a speed of 400 rpm for 2.5 hours to evaporate the solvent, so that the chitosan was cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer;
[0189] Solution B was added dropwise to the emulsion that had formed the first shell layer for 30 minutes, and the mixture was stirred at 55°C and 400 rpm for 2.5 hours to evaporate the solvent, so that the polyamide resin formed a second shell layer outside the first shell layer, thereby obtaining an emulsion with two shell layers;
[0190] The modified alumina was dispersed in 92.5 g of deionized water to form a thermal conductive filler mixed dispersion H; the thermal conductive filler mixed dispersion H was added dropwise to the emulsion of the two-layer shell for 45 minutes, and stirred at 55° C. and 400 rpm for 1.5 hours to make the thermal conductive filler evenly distributed on the surface of the microcapsule and in the shell layer;
[0191] The microcapsules were collected by filtration, washed four times with deionized water to remove residual solvents and unreacted substances, and then vacuum dried at 55°C for 16.5 hours to obtain a microcapsule fire extinguishing material. The microcapsule fire extinguishing material was adhered to a foam substrate double-sided adhesive tape, and the other side of the foam substrate double-sided adhesive tape was adhered to a torn non-woven fabric to obtain a self-excited microcapsule structure fire extinguishing material.
[0192] Comparative Example 5
[0193] The only difference between this comparative example and Example 3 is that alumina is used instead of modified alumina.
[0194] In order to verify the technical effect of the present application, the self-exciting microcapsule structure fire extinguishing materials prepared in Examples 1-5 and Comparative Examples 1-5 were tested:
[0195] Specific methods for testing fire extinguishing performance:
[0196] Experimental Materials:
[0197] 1. Ten stainless steel boxes of the same size (1m×1m×1m), with one side of the box open.
[0198] 2. Perfluorohexanone fire extinguishing patches prepared in Examples 1-5 and Comparative Examples 1-5
[0199] 3. Fuel barrel (inner diameter 50cm, depth 5cm)
[0200] 4. Diesel
[0201] 5. Ignition gun
[0202] 6. Timer
[0203] Experimental steps:
[0204] 1. Place ten stainless steel boxes in a safe and ventilated experimental area.
[0205] 2. The perfluorohexanone fire extinguishing materials prepared in Examples 1-5 and Comparative Examples 1-5 with a length and width of 80 cm*80 cm are respectively pasted on the middle positions of the top inner walls of ten boxes to ensure that the fire extinguishing stickers are flat and fit.
[0206] 3. Place a fuel barrel in the middle of the bottom inner wall of the box and add 500mL of diesel into the fuel barrel.
[0207] 4. Use the ignition gun to ignite the diesel and start burning.
[0208] 5. Start the timer at the same time to record the fire extinguishing time during the burning process.
[0209] 6. Observe and record the extinguishing time of the fire extinguishing material. The extinguishing time is recorded from the time after ignition to the time after extinguishing the fire. Calculate the release of the fire extinguishing material. Since the edge of the fire extinguishing material is farther away from the fire source than the middle position, the heat received by the middle position is different from that received by the edge of the fire extinguishing material. The release of the fire extinguishing material at different positions is simulated under the condition of uneven temperature in the fire scene. The appearance release of the fire extinguishing material after extinguishing the fire is observed under a microscope. The originally plump fire extinguishing sticker becomes shrunken, indicating that the perfluorohexanone inside it has been completely released. The shrunken area ratio of the fire extinguishing material is recorded. The shrunken area ratio = (shrunken area / area of the fire extinguishing material before extinguishing the fire) * 100% to understand the release degree.
[0210] The specific results are shown in Table 1.
[0211] Table 1 Test results of microcapsule materials prepared in Examples 1-5 and Comparative Examples 1-5.
[0212] Test items Fire extinguishing time(s) Shrunken area ratio (%) Example 1 9.7 94.6 Example 2 9.2 95.8 Example 3 8.7 96.7 Example 4 8.8 96.6 Example 5 8.8 96.3 Comparative Example 1 26.5 54.8 Comparative Example 2 22.7 72.5 Comparative Example 3 23.1 68.3 Comparative Example 4 23.5 62.7 Comparative Example 5 16.3 78.2
[0213] It can be seen from the above table data that the self-exciting microcapsule structure fire extinguishing material prepared by the present invention can quickly extinguish fires. At the same time, the shrinkage area of the self-exciting microcapsule structure fire extinguishing material prepared in this embodiment accounts for a large proportion, and it can be concluded that the microcapsules in the fire extinguishing material are released more fully, indicating that the addition of the thermal conductive filler prepared by the present invention into the capsule shell of the fire extinguishing material can promptly and quickly extinguish the fire, and can be beneficial to the heat conduction between the microcapsules, can cope with fires with uneven temperature distribution, and improve the reliability of the fire extinguishing effect. Since the edge position of the fire extinguishing material is farther away from the fire source than the middle position, the heating degree of the middle position is different from that of the edge position of the fire extinguishing material. In this embodiment 1-5, most of the microcapsules can still be released, proving that the addition of the thermal conductive filler proves that the heat can be quickly conducted in the fire extinguishing material. Even if the uneven temperature of the fire scene causes uneven heating of different positions of the fire extinguishing material, it can still ensure that the fire extinguishing medium at the low temperature is fully released, which improves the reliability of the fire extinguishing material and avoids the local release of the fire extinguishing medium after the fire extinguishing material is heated.
[0214] In the microcapsule fire extinguishing material prepared by the present invention, perfluorohexanone is used as the capsule core fire extinguishing medium, and the fire can be quickly and effectively extinguished. Microencapsulation can effectively encapsulate perfluorohexanone in the capsule core, protect it from leakage or deterioration before storage and use, ensure the stability and effectiveness of the fire extinguishing component, and the layered capsule shell structure provides multiple protections, further enhancing the stability of the encapsulation.
[0215] By adding fillers with good thermal conductivity, such as graphene, carbon nanotubes, and modified alumina, the thermal conductivity of the microcapsules can be improved, so that heat can be transferred more evenly to the inside of the microcapsules, promoting the release of the capsule core material. When the thermal conductivity of the capsule shell is improved, the heat absorbed by one microcapsule can be transferred to the adjacent microcapsules more quickly. This helps to form a more uniform temperature distribution in the fire scene, allowing more microcapsules to reach the fire extinguishing trigger temperature at the same time, thereby achieving a more synchronous and efficient fire extinguishing effect. In the case of local heating, the good thermal conductivity of the capsule shell can quickly diffuse the heat, avoiding the situation where only part of the microcapsules are heated and released while other parts do not respond. This enables the microcapsules as a whole to play a more coordinated fire extinguishing role, improve the utilization efficiency of fire extinguishing materials and the comprehensiveness of fire extinguishing. Uniform heat conduction also helps to control the release rate and total amount of perfluorohexanone, making its release more stable and continuous, and enhancing the durability of fire extinguishing.
[0216] The addition of modified alumina not only enhances the thermal conductivity, but also improves the mechanical strength and stability of the microcapsules. In addition, the grafting of KH570 silane coupling agent can improve the interface compatibility between alumina and graphene and carbon nanotubes, reduce the interface thermal resistance, and improve the thermal conduction efficiency.
[0217] The loading of silver nanoparticles increases the thermal conductivity channels of alumina, further improving its thermal conductivity. When compounded with graphene and carbon nanotubes, a denser thermal conductivity network can be formed, synergistically improving the overall thermal conductivity of the microcapsules.
[0218] The presence of the polydopamine layer increases the surface activity and roughness of alumina, making it easier to interact with graphene and carbon nanotubes, and improving their dispersibility and compatibility in microcapsules. Good dispersibility helps reduce agglomeration and give full play to the excellent properties of graphene and carbon nanotubes, thus playing a synergistic role.
[0219] The functional groups on the surface of modified alumina can interact with the amide groups in the polyamide resin to enhance the interfacial bonding between the two. This enhanced interfacial bonding helps to improve the mechanical properties and stability of the microcapsules, and may also improve the crystallization behavior of the polyamide resin, further improving the performance of the microcapsules. A better synergistic effect between modified alumina, graphene and carbon nanotubes is achieved, and the comprehensive performance of the microcapsules is improved.
[0220] It is worth noting that carbon nanotubes have extremely high axial thermal conductivity and can efficiently transfer heat in one-dimensional direction. Graphene has excellent thermal conductivity in the planar direction, while modified alumina improves its own thermal conductivity through surface modification and loading of silver nanoparticles. When they are present in the microcapsule system as thermal conductive fillers together: a complementary thermal conductive network is formed: the one-dimensional thermal conductivity of carbon nanotubes, the planar thermal conductivity of graphene, and the multi-dimensional thermal conductivity of modified alumina complement each other to form a denser and more comprehensive thermal conductive network, so that heat can be transferred more quickly and evenly in the microcapsule system. The synergistic effect of the three increases the heat conduction pathway, reduces thermal resistance, and thus improves the overall thermal conductivity efficiency. Synergistically strengthen the capsule shell structure: while improving thermal conductivity, they interact with capsule shell materials such as chitosan and polyamide resin to enhance the structural stability of the capsule shell, which helps to maintain the integrity and performance stability of the microcapsules. The synergistic effect of modified alumina, carbon nanotubes and graphene significantly improves the performance and response efficiency of microcapsule fire extinguishing materials by building a more complete thermal conductive network and strengthening the capsule shell structure.
[0221] When microcapsule fire extinguishing materials are used in places where electronic equipment is densely populated, graphene and carbon nanotubes have certain electromagnetic shielding properties and will have a certain regulating effect on the surrounding electromagnetic environment. Its electromagnetic shielding effect may help reduce the secondary damage of fire to electronic equipment.
[0222] The above specific embodiments are only several optional embodiments of the present invention. Based on the technical solutions of the present invention and the relevant inspirations of the above embodiments, those skilled in the art can make various alternative improvements and combinations to the above specific embodiments.
Claims
1. A self-exciting microcapsule structure fire extinguishing material, characterized in that: It includes the following raw materials in parts by weight: Capsule core: 50-60 parts of perfluorohexanone; Capsule shell: including a first shell and a second shell, the first shell includes: 16-20 parts of chitosan, 1-2 parts of nano titanium dioxide, 5-7 parts of nano iron oxide, and the second shell includes: 20-30 parts of polyamide resin; Thermal conductive filler: 1-3 parts of graphene, 1-3 parts of carbon nanotubes, 2-4 parts of modified alumina.
2. The self-exciting microcapsule structure fire extinguishing material according to claim 1, characterized in that: The preparation method of the microcapsule fire extinguishing material comprises the following steps: S1. Solution and dispersion preparation Dissolve chitosan in 130-140 parts of acetic acid solution to form solution A; Dissolving a polyamide resin in 135-145 parts of an ethanol solution to form a solution B; Dispersing nano titanium dioxide and nano iron oxide in 85-90 parts of deionized water to form a nano oxide dispersion C; Dispersing graphene and carbon nanotubes in 95-100 parts of deionized water respectively to obtain dispersion D and dispersion E, and then mixing dispersion D and dispersion E evenly to obtain graphene / carbon nanotube mixed dispersion F; S2. Emulsification of capsule core Add perfluorohexanone to solution A, stir with a high-speed stirrer to fully disperse the perfluorohexanone in solution A to form emulsion droplets, and the uniformly distributed emulsion droplets form emulsion G; S3. First shell formation Under stirring, the nano-oxide dispersion C is added dropwise to the emulsion G for 40-50 minutes, and then stirred at 50°C-60°C for 2-3 hours to evaporate the solvent, so that the chitosan is cross-linked and solidified on the surface of the emulsion droplets to form the first shell layer; S4. Second shell formation Add solution B dropwise to the emulsion that has formed the first shell layer for 25-35 minutes, stir at 50-60°C and 350-450rpm for 2-3 hours and evaporate the solvent, so that the polyamide resin forms a second shell layer outside the first shell layer, and obtain an emulsion with two shell layers; S5. Introduction of thermal conductive filler Dispersing the graphene / carbon nanotube mixed dispersion F and modified alumina in 90-95 parts of deionized water to form a thermal conductive filler mixed dispersion H; Add the thermal conductive filler mixed dispersion H dropwise into the emulsion of the two shell layers for 40-50 minutes, and stir at 50-60°C and 300-500 rpm for 1-2 hours to evenly distribute the thermal conductive filler on the surface of the microcapsule and in the shell layer; S6. Post-processing The microcapsules are collected by filtration, washed with deionized water for 3-5 times to remove residual solvent and unreacted substances, and then vacuum dried at 50-60° C. for 15-18 hours to obtain a microcapsule fire extinguishing material.
3. The self-exciting microcapsule structure fire extinguishing material according to claim 2, characterized in that: The specific preparation steps of the modified alumina are as follows: Step 1: Add alumina powder to a 3%-7% silane coupling agent ethanol solution, and stir to allow the silane coupling agent molecules to be initially grafted onto the alumina surface; Step 2: Add dopamine hydrochloride to the above reaction system and continue stirring to mix and react; Step 3: Filter the reaction product and wash it with ethanol to remove unreacted substances; Step 4: dispersing the washed product in deionized water, and then adding a silver nitrate solution with a concentration of 0.08-0.12 mol / L dropwise, and allowing the silver ions to react with the functional groups on the surface of the alumina under stirring to form alumina loaded with silver nanoparticles; Step 5: Filter the silver nanoparticle-loaded alumina, wash with deionized water, and vacuum dry to obtain modified alumina.
4. The self-exciting microcapsule structure fire extinguishing material according to claim 3, characterized in that: In the step 2, the stirring temperature is 55-65° C., and the reaction is carried out at a stirring speed of 280-320 rpm for 1.5-2.5 hours.
5. The self-exciting microcapsule structure fire extinguishing material according to claim 1, characterized in that: It includes the following raw materials in parts by weight: Capsule core: 52-58 parts of perfluorohexanone; Capsule shell: including the first shell and the second shell; The first shell layer includes: 17-19 parts of chitosan, 1-2 parts of nano titanium dioxide, and 6-7 parts of nano iron oxide; The second shell comprises: 22-28 parts of polyamide resin; Thermal conductive filler: 1-2 parts of graphene, 1-2 parts of carbon nanotubes, 3-4 parts of modified alumina.
6. The self-exciting microcapsule structure fire extinguishing material according to claim 1, characterized in that: It includes the following raw materials in parts by weight: Capsule core: 55 parts of perfluorohexanone; Capsule shell: including the first shell and the second shell; The first shell layer includes: 18 parts of chitosan, 1.52 parts of nano titanium dioxide, and 6 parts of nano iron oxide; The second shell comprises: 25 parts of polyamide resin; Thermal conductive filler: 2 parts of graphene, 2 parts of carbon nanotubes, and 3 parts of modified alumina.
7. The self-exciting microcapsule structure fire extinguishing material according to claim 2, characterized in that: In S2, the high-speed stirrer stirs at a rotation speed of 8000-10000 rpm for 20-30 minutes.
8. The self-exciting microcapsule structure fire extinguishing material according to claim 2, characterized in that: In S3, the rotation speed is 350-450 rpm.
9. The self-exciting microcapsule structure fire extinguishing material according to claim 1, characterized in that: The microcapsule fire extinguishing material further comprises a connecting layer fixedly connected to the capsule shell and a bottom layer connected to the connecting layer.
10. The self-exciting microcapsule structure fire extinguishing material according to claim 9, characterized in that: The connecting layer is a double-sided adhesive with a foam substrate, and the bottom layer is a non-woven fabric.
Citation Information
Patent Citations
Heat conducting gap filling material and preparing method thereof
CN105621960A
Core-shell-structured silver-based heat-conductive rubber composite material and preparation method thereof
CN109265762A
Perfluorohexanone microcapsule fire extinguishing material and preparation method thereof
CN114748830A
Preparation method of mixture containing fire extinguishing microcapsules
CN118253064A
Polymer nanocomposite material, method for producing the same, electronic component apparatus and method for manufacturing the component apparatus
JP2008063449A