Methanol catalytic conversion synthesis method
In the technology of hydrogenation conversion of carbon dioxide to synthesize methanol, using a single layer of graphite/In2O3/MnO2 phase material, in conjunction with the adsorption and decomposition of hydrogen molecules, the problems of slow rate and poor selectivity in the existing technology are solved, and more efficient The catalytic conversion of carbon dioxide into methanol.
Patent Information
- Application Number
- CN202411525926.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-11-26
AI Technical Summary
The existing technologies for hydrogenation of carbon dioxide to convert methanol have a slow rate and poor reaction selectivity, which is difficult to meet the needs of carbon dioxide conversion and utilization.
Using a single-layer graphite/In2O3/MnO2 phase material based on single-layer graphite-supported zinc oxide and manganese oxide, the adsorption and decomposition of hydrogen atoms is coordinated to enhance the adsorption and decomposition of hydrogen gas, and the catalytic conversion of carbon dioxide and hydrogen is improved to synthesize methanol. efficiency.
The methanol generation rate and carbon dioxide conversion rate were significantly improved, so that the methanol generation rate increased from 0.5-0.7 gmethanol·gcat-1·h-1 to ~0.85 gmethanol·gcat-1·h-1, and the carbon dioxide conversion rate was from 17%-20 % increased to ~30%.
Smart Images

Figure CN119015877A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon dioxide waste gas treatment, and in particular to a methanol catalytic conversion synthesis method based on carbon dioxide hydrogenation. Background Art
[0002] Carbon dioxide is one of the main pollutants emitted by industrial production, building operation and human metabolism, and is also the main target of my country's "dual carbon" strategy. Therefore, it is necessary to purify carbon dioxide by means of adsorption capture and underground storage. Compared with the above two methods, converting carbon dioxide into high-value-added chemicals by hydrogenation is a method with greater application value and potential. It can not only harmlessly treat and purify carbon dioxide, but also realize the multiple recycling of carbon dioxide, achieving true "carbon neutrality".
[0003] For example, CN114849715A discloses a method for preparing a catalyst for hydrogenation of carbon dioxide to synthesize methanol; CN109731578A discloses a catalyst for hydrogenation of carbon dioxide and its preparation method and application; CN109499577A discloses a method for preparing and applying a Cu-Ni-based catalyst for reverse water gas reaction; CN118477667A discloses a highly active and highly selective Co-based intermetallic carbide catalyst for hydrogenation of CO2 to produce methanol and its preparation method and application; the catalysts prepared by the above patented methods can all achieve the synthesis treatment of hydrogenation of carbon dioxide to methanol. However, the existing technologies for hydrogenation of carbon dioxide to methanol all have the problems of slow rate and poor reaction selectivity, which makes it difficult to fully meet the demand for carbon dioxide conversion and utilization.
[0004] Therefore, how to provide a methanol catalytic conversion synthesis method that is different from the prior art and can more efficiently realize the synthesis of methanol by hydrogenation of carbon dioxide has become a problem that needs to be considered and solved by those skilled in the art. Summary of the invention
[0005] In view of the above-mentioned deficiencies of the prior art, the technical problem to be solved by the present invention is: how to provide a methanol catalytic conversion synthesis method that is different from the prior art and can more efficiently realize the carbon dioxide hydrogenation conversion synthesis, so as to more efficiently realize the conversion treatment of carbon dioxide.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions: A methanol catalytic conversion synthesis method, characterized in that it comprises the following steps: In the first step, carbon dioxide and hydrogen molecules are adsorbed on the surface of the monolayer graphite / In2O3 / MnO2 phase material to form an adsorbed structure, in which the hydrogen molecules are decomposed into two adsorbed hydrogen atoms; the reaction formula can be characterized as CO2 + C / In2O3 / MnO2→CO2(ad), H2 + C / In2O3 / MnO2→ H2(ad), H2(ad) → 2 * H(ad); In the second step, two adsorbed hydrogen atoms combine with the carbon atom in the adsorbed carbon dioxide to form an O-CH2-O structure; the reaction equation can be represented as CO2(ad) + 2 * H(ad) → O-CH2-O(ad); In the third step, one oxygen atom in the O-CH2-O structure combines with another hydrogen atom to form an O-CH2-OH structure; the reaction formula can be represented as O-CH2-O (ad) + * H(ad) → O-CH2-OH(ad); In the fourth step, the -OH in the above O-CH2-OH structure dissociates and combines with another hydrogen atom to remove the water molecule and obtain the O-CH2 structure; the reaction formula can be represented as O-CH2-OH(ad) + * H(ad) → O-CH2(ad) + H2O; In the fifth step, the carbon and oxygen atoms in the above O-CH2 structure combine with other hydrogen atoms to finally generate methanol molecules; the reaction formula can be represented as O-CH2(ad) + 2 * H → CH3-OH.
[0007] Thus, in the present invention, a single-layer graphite / In2O3 / MnO2 phase material formed by single-layer graphite loaded with zinc oxide and manganese oxide is used as a catalytic conversion synthesis material for synthesizing methanol, and the above reaction can efficiently complete the catalytic conversion synthesis process of synthesizing carbon dioxide and hydrogen into methanol. In this method, firstly, the single-layer graphite phase material can provide a large number of sites for pre-adsorption of carbon dioxide and hydrogen molecules, providing sufficient raw materials for subsequent hydrogenation catalytic reactions; secondly, MnO2 and In2O3 can be used to enhance the process of hydrogen molecule adsorption and decomposition into hydrogen atoms, and the combination of initial / intermediate reactants with hydrogen atoms, respectively, and the two cooperate to enhance the overall hydrogenation catalytic effect.
[0008] Furthermore, in the present invention, a methanol catalytic conversion synthesis material whose main effective component is a single-layer graphite / In2O3 / MnO2 phase material is used to realize the catalytic conversion synthesis treatment of carbon dioxide hydrogenation conversion to synthesize methanol.
[0009] The specific process principle of the catalytic conversion synthesis treatment is as follows: (a) The role of MnO2. Hydrogen adsorption on the surface of monolayer graphite is a weak physical adsorption, and monolayer graphite cannot provide sufficient energy for the decomposition of hydrogen molecules. When MnO2 exists and hydrogen molecules are adsorbed around it, MnO2 has strong oxidizing properties and can attract delocalized π orbital electrons on the surface of monolayer graphite to its surroundings. During the migration of delocalized π orbital electrons, the bonded valence electrons in the hydrogen molecules will be affected by both the instantaneous dipole moment and the strong oxidizing electron attraction of MnO2, which will weaken the HH bond valence electron pairing strength and even destroy it. Then, the valence electrons of hydrogen atoms will also migrate to the surrounding of MnO2 along with the delocalized π orbital electrons on the surface of monolayer graphite, completing the breaking of the HH bond and the adsorption of single hydrogen atoms. In addition, a more fundamental role is that when a single-layer graphite phase is used as a substrate, the above-mentioned process of delocalized π orbital electrons migrating toward the surrounding of MnO2 can be carried out on the entire surface, that is, hydrogen molecules adsorbed at any position will be affected by the surrounding embedded MnO2, and can then be quickly decomposed into single hydrogen atoms for subsequent combination with carbon dioxide and intermediate reactants; (b) The role of In2O3. When carbon dioxide or an intermediate reactant is adsorbed, one or several of its atoms need to be fixed to the catalyst surface site. This binding process requires carbon dioxide or the intermediate reactant to provide its outer active electrons, so it is difficult for carbon dioxide or the intermediate reactant to provide more outer active electrons for bonding with the hydrogen atoms generated by the above decomposition. When In2O3 exists, it is an electronic semiconductor and can provide abundant free electrons to carbon dioxide or the intermediate reactant as outer active electrons to bond with hydrogen atoms, thereby promoting the reaction to the next step. At the same time, a more common role is that the delocalized π bonds on the surface of a single layer of graphite can be used as a channel for the migration of free electrons of In2O3, thereby providing free electrons for the entire surface of carbon dioxide or intermediate reactants for the hydrogenation catalytic process. In addition, since MnO2 and In2O3 are oxidizing and reducing, respectively, the above-mentioned electron migration process on the entire surface can be cyclical and maintain the balance of electrons on the entire surface.
[0010] Therefore, the present invention can effectively improve the conversion efficiency of carbon dioxide and increase the production rate of methanol. The applicant has verified that the present invention can increase the production rate of methanol from 0.5-0.7 g / cm2 in the conventional method. methanol ·g cat -1 ·h -1 Increase to ~ 0.85g methanol ·g cat -1 ·h -1 ; The carbon dioxide conversion rate is increased from 17%-20% in the conventional method to ~ 30%.
[0011] Furthermore, the methanol catalytic conversion synthetic material used in the present invention includes the following phase components in the following mass proportions: 0.01-0.25 parts of pure single-layer graphite phase, 0.01-0.07 parts of metal hydroxide phase (In(OH)3, Mn(OH)2 and MnO(OH)2), 0.05-0.18 parts of metal oxide phase (In2O3, MnO2), and 0.5-0.93 parts of single-layer graphite / In2O3 / MnO2 phase.
[0012] A further optimal mass ratio is: 0.12 parts of pure single-layer graphite phase, 0.02 parts of metal hydroxide phase (In(OH)3, Mn(OH)2 and MnO(OH)2), 0.1 parts of metal oxide phase (In2O3, MnO2), and 0.76 parts of single-layer graphite / In2O3 / MnO2 phase.
[0013] In the above-mentioned synthetic materials for methanol catalytic conversion, the single-layer graphite / In2O3 / MnO2 phase is the main effective component with the largest proportion; at the same time, the pure single-layer graphite phase is used as a place to supplement the adsorption and loading of carbon dioxide and hydrogen molecules, and the metal oxide phase is used to supplement and enhance the catalytic conversion of carbon dioxide hydrogenation. In addition, each component is a common reaction product, and its mixing and doping together can play a certain dynamic conversion supplement effect after the main effective components are converted and consumed (especially the presence of the metal oxide phase), which better ensures the durability of the treatment effect.
[0014] Furthermore, the methanol catalytic conversion synthetic material is prepared by the following steps: Step 1: Prepare a single-layer graphite substrate; weigh 10 g of oxalic acid powder (superior purity, 99.5%) and 0.5 g of layered graphite (100 mesh, 99.99% purity) and mix and grind them, and calcine the mixture to obtain a single-layer graphite polymer (further, the calcination process is: place the mixture in an aluminum crucible, heat it in a muffle furnace at a heating rate of 10 °C / min from room temperature to 200 °C and calcine it for 8 h; then heat it from 200 °C to 400 °C at a heating rate of 40 °C / min and continue calcining for 1 h, and then naturally cool it to room temperature to obtain a single-layer graphite polymer); pour the single-layer graphite polymer into 200 ml of ethanol, and perform ultrasonic dispersion treatment (1 h) obtaining a monolayer graphite dispersion; then vacuum filtering the monolayer graphite dispersion using a polyethersulfone filter membrane and drying it at room temperature, placing the filter membrane and the monolayer graphite loaded thereon in a tablet press for pressing (preferably, the pressing process is to fix the mold at a pressure of 30 MPa for 10 min), then using N, N-dimethylformamide to dissolve the polyethersulfone filter membrane to obtain a monolayer graphite film, and finally drying the monolayer graphite film to obtain a final monolayer graphite substrate (preferably, the drying process is to place it in a drying oven at 50°C for 3 h to obtain a final monolayer graphite substrate); Step 2: Indium trioxide and manganese dioxide are loaded and embedded in a single-layer graphite substrate; prepare and weigh 10 g of the above-mentioned single-layer graphite substrate and dissolve it in 200 ml of deionized water, then add 0.05 mol of indium nitrate tetrahydrate (In(NO3)3·4H2O), 0.05 mol of manganese nitrate hexahydrate (Mn(NO3)2·6H2O) and 100 mol of ammonium hydroxide (NH4OH) / ethanol (C2H5OH) mixed solution (further, the concentration of ammonium hydroxide solution is 25%, the concentration of ethanol solution is 99.5%, and the volume ratio of the two is 1:3) to obtain a mixed solution; the mixed solution is rotary evaporated at (60°C) until all precipitates are obtained, and then rinsed with deionized water for 5 times, and the rinsed precipitates are dried and calcined (preferably, the drying and calcination process is drying at 60°C for 48 h; placing the dried precipitate in an aluminum crucible and calcining it at 800 °C in a muffle furnace for 6 h) to obtain the final single-layer graphite-supported indium trioxide-manganese dioxide composite catalyst.
[0015] The amount of each raw material in the above steps can be adjusted in equal proportions. The chemical reaction characteristics of each step in the above preparation process are as follows: In step 1, the layered graphite is calcined, dispersed, and pressed to obtain a single-layer graphite film. This process is a physical treatment process without chemical reaction, and the reaction formula is C (multi-layer graphite) → C (single-layer graphite film); In step 2, indium nitrate and manganese nitrate react with sodium hydroxide to generate indium hydroxide and manganese hydroxide, respectively, and the chemical reaction formulas are In(NO3)3 + NH4OH → In(OH)3 + NH4NO3, Mn(NO3)2 + NH4OH → Mn(OH)2 + MnO(OH)2+ NH4NO3.
[0016] Indium hydroxide and manganese hydroxide will decompose into corresponding metal oxides under high temperature calcination, and the chemical reaction formula is In(OH)3 → In2O3 + H2O, Mn(OH)2 + O2 → MnO2 + H2O, MnO(OH)2→ MnO2 + H2O.
[0017] The generated indium trioxide and manganese dioxide will be loaded and embedded in the monolayer graphite substrate at high temperature. The reaction formula is: C n +In2O3 + MnO2 → ···C···In2O3···C···MnO2···C···.
[0018] Therefore, the above reaction process can quickly and efficiently obtain a methanol catalytic conversion synthesis material in which the main active ingredient single-layer graphite / In2O3 / MnO2 phase accounts for more than 50%, ensuring the efficient catalytic synthesis effect of carbon dioxide hydrogenation to methanol. At the same time, the other phase components generated are uniformly mixed and doped together, especially the metal oxide phase containing part of In2O3 and MnO2 can play a certain dynamic conversion supplement effect after the main active ingredients are converted and consumed, and the part of the single-layer graphite contained can also improve the adsorption effect; therefore, the catalytic conversion synthesis effect of carbon dioxide hydrogenation to methanol can be better guaranteed.
[0019] Therefore, the present invention has the following characteristics: 1. The rate of converting carbon dioxide into methanol by hydrogenation is increased; 2. The hydrogenation conversion rate of carbon dioxide is increased.
[0020] In summary, the present invention can provide a method for synthesizing methanol by hydrogenation conversion of carbon dioxide, which is different from the prior art and can achieve the conversion treatment of carbon dioxide more efficiently. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the process of hydrogenation of carbon dioxide into methanol on the surface of single-layer graphite / In2O3 / MnO2 phase.
[0022] Figure 2 It is a schematic diagram comparing the methanol conversion rate of the methanol catalytic conversion synthesis material of the present invention and other types of methanol synthesis catalyst materials.
[0023] Figure 3 It is a schematic diagram comparing the methanol conversion rate of the methanol catalytic conversion synthesis material of the present invention and other types of methanol synthesis catalyst materials. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with specific implementation modes.
[0025] Embodiment: A method for synthesizing methanol by catalytic conversion, characterized in that, see Figure 1 , including the following steps: In the first step, carbon dioxide and hydrogen molecules are adsorbed on the surface of the monolayer graphite / In2O3 / MnO2 phase material to form an adsorbed structure, in which the hydrogen molecules are decomposed into two adsorbed hydrogen atoms; the reaction formula can be characterized as CO2 + C / In2O3 / MnO2→CO2(ad), H2 + C / In2O3 / MnO2→ H2(ad), H2(ad) → 2 * H(ad); In the second step, two adsorbed hydrogen atoms combine with the carbon atom in the adsorbed carbon dioxide to form an O-CH2-O structure; the reaction equation can be represented as CO2(ad) + 2* H(ad) → O-CH2-O(ad); In the third step, one oxygen atom in the O-CH2-O structure combines with another hydrogen atom to form an O-CH2-OH structure; the reaction formula can be represented as O-CH2-O (ad) + * H(ad) → O-CH2-OH(ad); In the fourth step, the -OH in the above O-CH2-OH structure dissociates and combines with another hydrogen atom to remove the water molecule and obtain the O-CH2 structure; the reaction formula can be represented as O-CH2-OH(ad) + * H(ad) → O-CH2(ad) + H2O; In the fifth step, the carbon and oxygen atoms in the above O-CH2 structure combine with other hydrogen atoms to finally generate methanol molecules; the reaction formula can be represented as O-CH2(ad) + 2 * H → CH3-OH.
[0026] Thus, in the present invention, a single-layer graphite / In2O3 / MnO2 phase material formed by single-layer graphite loaded with zinc oxide and manganese oxide is used as a catalytic conversion synthesis material for synthesizing methanol, and the above reaction can efficiently complete the catalytic conversion synthesis process of synthesizing carbon dioxide and hydrogen into methanol. In this method, firstly, the single-layer graphite phase material can provide a large number of sites for pre-adsorption of carbon dioxide and hydrogen molecules, providing sufficient raw materials for subsequent hydrogenation catalytic reactions; secondly, MnO2 and In2O3 can be used to enhance the process of hydrogen molecule adsorption and decomposition into hydrogen atoms, and the combination of initial / intermediate reactants with hydrogen atoms, respectively, and the two cooperate to enhance the overall hydrogenation catalytic effect.
[0027] During implementation, in the present invention, a methanol catalytic conversion synthesis material whose main effective component is a single-layer graphite / In2O3 / MnO2 phase material is used to realize the catalytic conversion synthesis treatment of carbon dioxide hydrogenation conversion to synthesize methanol.
[0028] The specific process principle of the catalytic conversion synthesis treatment is as follows: (a) The role of MnO2. Hydrogen adsorption on the surface of monolayer graphite is a weak physical adsorption, and monolayer graphite cannot provide sufficient energy for the decomposition of hydrogen molecules. When MnO2 exists and hydrogen molecules are adsorbed around it, MnO2 has strong oxidizing properties and can attract delocalized π orbital electrons on the surface of monolayer graphite to its surroundings. During the migration of delocalized π orbital electrons, the bonded valence electrons in the hydrogen molecules will be affected by both the instantaneous dipole moment and the strong oxidizing electron attraction of MnO2, which will weaken the HH bond valence electron pairing strength and even destroy it. Then, the valence electrons of hydrogen atoms will also migrate to the surrounding of MnO2 along with the delocalized π orbital electrons on the surface of monolayer graphite, completing the breaking of the HH bond and the adsorption of single hydrogen atoms. In addition, a more fundamental role is that when a single-layer graphite phase is used as a substrate, the above-mentioned process of delocalized π orbital electrons migrating toward the surrounding of MnO2 can be carried out on the entire surface, that is, hydrogen molecules adsorbed at any position will be affected by the surrounding embedded MnO2, and can then be quickly decomposed into single hydrogen atoms for subsequent combination with carbon dioxide and intermediate reactants; (b) The role of In2O3. When carbon dioxide or an intermediate reactant is adsorbed, one or several of its atoms need to be fixed to the catalyst surface site. This binding process requires carbon dioxide or the intermediate reactant to provide its outer active electrons, so it is difficult for carbon dioxide or the intermediate reactant to provide more outer active electrons for bonding with the hydrogen atoms generated by the above decomposition. When In2O3 exists, it is an electronic semiconductor and can provide abundant free electrons to carbon dioxide or the intermediate reactant as outer active electrons to bond with hydrogen atoms, thereby promoting the reaction to the next step. At the same time, a more common role is that the delocalized π bonds on the surface of a single layer of graphite can be used as a channel for the migration of free electrons of In2O3, thereby providing free electrons for the entire surface of carbon dioxide or intermediate reactants for the hydrogenation catalytic process. In addition, since MnO2 and In2O3 are oxidizing and reducing, respectively, the above-mentioned electron migration process on the entire surface can be cyclical and maintain the balance of electrons on the entire surface.
[0029] Therefore, the present invention can effectively improve the conversion efficiency of carbon dioxide and increase the production rate of methanol. The applicant has verified that the present invention can increase the production rate of methanol from 0.5-0.7 g / cm2 in the conventional method. methanol ·g cat -1 ·h -1 Increase to ~ 0.85g methanol ·g cat -1 ·h -1 ; The carbon dioxide conversion rate is increased from 17%-20% in the conventional method to ~ 30%.
[0030] Among them, the methanol catalytic conversion synthetic material used in the present invention includes the following phase components in the following mass proportions: 0.01-0.25 parts of pure single-layer graphite phase, 0.01-0.07 parts of metal hydroxide phase (In(OH)3, Mn(OH)2 and MnO(OH)2), 0.05-0.18 parts of metal oxide phase (In2O3, MnO2), and 0.5-0.93 parts of single-layer graphite / In2O3 / MnO2 phase.
[0031] A further optimal mass ratio is: 0.12 parts of pure single-layer graphite phase, 0.02 parts of metal hydroxide phase (In(OH)3, Mn(OH)2 and MnO(OH)2), 0.1 parts of metal oxide phase (In2O3, MnO2), and 0.76 parts of single-layer graphite / In2O3 / MnO2 phase.
[0032] In the above-mentioned synthetic materials for methanol catalytic conversion, the single-layer graphite / In2O3 / MnO2 phase is the main effective component with the largest proportion; at the same time, the pure single-layer graphite phase is used as a place to supplement the adsorption and loading of carbon dioxide and hydrogen molecules, and the metal oxide phase is used to supplement and enhance the catalytic conversion of carbon dioxide hydrogenation. In addition, each component is a common reaction product, and its mixing and doping together can play a certain dynamic conversion supplement effect after the main effective components are converted and consumed (especially the presence of the metal oxide phase), which better ensures the durability of the treatment effect.
[0033] During implementation, the methanol catalytic conversion synthetic material is prepared by the following steps: Step 1: Prepare a single-layer graphite substrate; weigh 10 g of oxalic acid powder (superior purity, 99.5%) and 0.5 g of layered graphite (100 mesh, 99.99% purity) and mix and grind them; place the mixture in an aluminum crucible, heat the temperature in a muffle furnace from room temperature to 200 °C at a rate of 10 °C / min and calcine for 8 h; then heat the temperature from 200 °C to 400 °C at a rate of 40 °C / min and continue calcining for 1 h, and then naturally cool to room temperature to obtain a single-layer graphite polymer; pour the single-layer graphite polymer into 200 ml of ethanol, and ultrasonically disperse it for 1 h to obtain a single-layer graphite dispersion; then vacuum filter the single-layer graphite dispersion using a polyethersulfone filter membrane and dry it at room temperature; place the filter membrane and the single-layer graphite loaded on it in a tablet press, fix it under a pressure of 30 MPa for 10 min, and then use N, The polyethersulfone filter membrane was dissolved by N-dimethylformamide to obtain a single-layer graphite film, and the single-layer graphite film was dried in a drying oven at 50 °C for 3 h to obtain a final single-layer graphite substrate; Step 2: Indium trioxide and manganese dioxide are loaded and embedded in a single-layer graphite substrate; prepare and weigh 10 g of the above-mentioned single-layer graphite substrate and dissolve it in 200 ml of deionized water, then add 0.05 mol of indium nitrate tetrahydrate (In(NO3)3·4H2O), 0.05 mol of manganese nitrate hexahydrate (Mn(NO3)2·6H2O) and 100 mol of ammonium hydroxide (NH4OH) / ethanol (C2H5OH) mixed solution (further, the concentration of ammonium hydroxide solution is 25%, the concentration of ethanol solution is 99.5%, and the volume ratio of the two is 1:3) to obtain a mixed solution; the mixed solution is rotary evaporated at 60 ° C until all precipitates are obtained, and then rinsed with deionized water for 5 times, and the rinsed precipitates are dried at 60 ° C for 48 h; the dried precipitates are placed in an aluminum crucible and calcined in a muffle furnace at 800 ° C for 6 h, and finally obtain the single-layer graphite-supported indium trioxide-manganese dioxide composite catalyst.
[0034] The amount of each raw material in the above steps can be adjusted in equal proportions. The chemical reaction characteristics of each step in the above preparation process are as follows: In step 1, the layered graphite is calcined, dispersed, and pressed to obtain a single-layer graphite film. This process is a physical treatment process without chemical reaction, and the reaction formula is C (multi-layer graphite) → C (single-layer graphite film); In step 2, indium nitrate and manganese nitrate react with sodium hydroxide to generate indium hydroxide and manganese hydroxide, respectively, and the chemical reaction formulas are In(NO3)3 + NH4OH → In(OH)3 + NH4NO3, Mn(NO3)2 + NH4OH → Mn(OH)2 + MnO(OH)2+ NH4NO3.
[0035] Indium hydroxide and manganese hydroxide will decompose into corresponding metal oxides under high temperature calcination, and the chemical reaction formula is In(OH)3 → In2O3 + H2O, Mn(OH)2 + O2 → MnO2 + H2O, MnO(OH)2→ MnO2 + H2O.
[0036] The generated indium trioxide and manganese dioxide will be loaded and embedded in the monolayer graphite substrate at high temperature. The reaction formula is: C n +In2O3 + MnO2 → ···C···In2O3···C···MnO2···C···.
[0037] Therefore, the above reaction process can quickly and efficiently obtain a methanol catalytic conversion synthesis material in which the main active ingredient single-layer graphite / In2O3 / MnO2 phase accounts for more than 50%, ensuring the efficient catalytic synthesis effect of carbon dioxide hydrogenation to methanol. At the same time, the other phase components generated are uniformly mixed and doped together, especially the metal oxide phase containing part of In2O3 and MnO2 can play a certain dynamic conversion supplement effect after the main active ingredients are converted and consumed, and the part of the single-layer graphite contained can also improve the adsorption effect; therefore, the catalytic conversion synthesis effect of carbon dioxide hydrogenation to methanol can be better guaranteed.
[0038] Therefore, the present invention has the following characteristics: 1. The rate of converting carbon dioxide into methanol by hydrogenation is increased; 2. The hydrogenation conversion rate of carbon dioxide is increased.
[0039] In order to better verify the effect of the present invention, the applicant conducted a comparative experiment, using the methanol catalytic conversion synthetic material obtained by the above specific implementation method as the experimental group, first under the environmental conditions of 200 ℃ / 5 MPa / 0% relative humidity, Pt / In2O3, Pt / In2O3-ZrO2 and 5%Ir / In2O3 were used as control group catalysts, and the molar contents of hydrogen (reaction gas) and nitrogen (carrier gas) were set to 76% and 5% respectively, and the rate of catalytic conversion of carbon dioxide with a molar content of 19% to methanol was compared. The test results are shown in Figure 2 From the experimental results, it can be seen that the methanol generation rate of the above-mentioned control group catalyst is lower than that of single-layer graphite / In2O3 / MnO2, especially the methanol generation rate of single-layer graphite / In2O3 / MnO2 is much higher than that of Pt / In2O3 and 5%Ir / In2O3, indicating that the coexistence of In2O3 and MnO2 can make the surface of single-layer graphite catalyze carbon dioxide to produce a synergistic effect, greatly enhancing the hydrogenation catalytic conversion ability of this type of composite catalyst.
[0040] Then, under the environmental conditions of 200 ℃ / 5 MPa / 0% relative humidity, Pt / In2O3, Pt / In2O3-ZrO2 and 5%Ir / In2O3 were used as control catalysts, and the molar contents of hydrogen (reaction gas) and nitrogen (carrier gas) were set to 76% and 5% respectively, and the conversion rate of carbon dioxide hydrogenation catalytic conversion to methanol with a molar content of 19% was compared. The experimental results are shown in Figure 3 From the experimental results, it can be seen that the carbon dioxide conversion rate of the above-mentioned control group catalyst is lower than that of single-layer graphite / In2O3 / MnO2, especially the carbon dioxide conversion rate of single-layer graphite / In2O3 / MnO2 is much higher than that of Pt / In2O3 and 5%Ir / In2O3, indicating that the coexistence of In2O3 and MnO2 can make the surface of single-layer graphite catalyze carbon dioxide to produce a synergistic effect, greatly enhancing the hydrogenation catalytic conversion ability of this type of composite catalyst.
Claims
1. A methanol catalytic conversion synthesis method, characterized in that: The following steps are involved: In the first step, carbon dioxide and hydrogen molecules are adsorbed on the surface of the monolayer graphite / In2O3 / MnO2 phase material to form an adsorbed structure, in which the hydrogen molecules are decomposed into two adsorbed hydrogen atoms; In the second step, two adsorbed hydrogen atoms combine with the carbon atom in the adsorbed carbon dioxide to form an O-CH2-O structure; In the third step, one oxygen atom in the O-CH2-O structure combines with another hydrogen atom to form an O-CH2-OH structure; In the fourth step, the -OH in the above O-CH2-OH structure dissociates and combines with another hydrogen atom to remove the water molecule to obtain the O-CH2 structure; In the fifth step, the carbon and oxygen atoms in the above O-CH2 structure combine with other hydrogen atoms respectively to finally generate methanol molecules.
2. The methanol catalytic conversion synthesis method according to claim 1, characterized in that: The method adopts a methanol catalytic conversion synthesis material whose main effective component is a single-layer graphite / In2O3 / MnO2 phase material to realize the catalytic conversion synthesis treatment of carbon dioxide hydrogenation conversion to synthesize methanol.
3. The methanol catalytic conversion synthesis method according to claim 2, characterized in that: The methanol catalytic conversion synthetic material used in the present invention includes the following phase components in the following mass proportions: 0.01-0.25 parts of pure single-layer graphite phase, 0.01-0.07 parts of metal hydroxide phase (In(OH)3, Mn(OH)2 and MnO(OH)2), 0.05-0.18 parts of metal oxide phase (In2O3, MnO2), and 0.5-0.93 parts of single-layer graphite / In2O3 / MnO2 phase.
4. The methanol catalytic conversion synthesis method according to claim 3, characterized in that: The physical phase components are: 0.12 parts of pure single-layer graphite phase, 0.02 parts of metal hydroxide phase (In(OH)3, Mn(OH)2 and MnO(OH)2), 0.1 parts of metal oxide phase (In2O3, MnO2), and 0.76 parts of single-layer graphite / In2O3 / MnO2 phase.
5. The methanol catalytic conversion synthesis method according to claim 4, characterized in that: The methanol catalytic conversion synthetic material is prepared by the following steps: Step 1: prepare a single-layer graphite substrate; weigh 10 g of oxalic acid powder and 0.5 g of layered graphite, mix and grind them, and calcine the mixture to obtain a single-layer graphite polymer; pour the single-layer graphite polymer into 200 ml of ethanol, and perform ultrasonic dispersion treatment to obtain a single-layer graphite dispersion; then vacuum filter the single-layer graphite dispersion using a polyethersulfone filter membrane and dry it at room temperature, place the filter membrane and the single-layer graphite loaded on it in a tablet press, and then use N, N-dimethylformamide to dissolve the polyethersulfone filter membrane to obtain a single-layer graphite film, and finally dry the single-layer graphite film to obtain a final single-layer graphite substrate; Step 2: embedding indium trioxide and manganese dioxide loads into a single-layer graphite substrate; preparing and weighing 10 g of the above-mentioned single-layer graphite substrate and dissolving it in 200 ml of deionized water, and then adding 0.05 mol of indium nitrate tetrahydrate, 0.05 mol of manganese nitrate hexahydrate and 100 mol of ammonium hydroxide / ethanol mixed solution to obtain a mixed solution; rotary evaporating the mixed solution until all precipitates are obtained, and then rinsing with deionized water for 5 times, and drying and calcining the rinsed precipitates to obtain the final single-layer graphite-supported indium trioxide-manganese dioxide composite catalyst.
6. The methanol catalytic conversion synthesis method according to claim 5, characterized in that: In step 1, the calcination process is as follows: the mixture is placed in an aluminum crucible, and the temperature is increased from room temperature to 200 °C in a muffle furnace at a heating rate of 10 °C / min and then calcined for 8 h; then the temperature is increased from 200 °C to 400 °C at a heating rate of 40 °C / min and further calcined for 1 h, and then naturally cooled to room temperature to obtain a single-layer graphite polymer.
7. The methanol catalytic conversion synthesis method according to claim 5, characterized in that: In step 1, the ultrasonic dispersion treatment time is 1 h.
8. The methanol catalytic conversion synthesis method according to claim 5, characterized in that: In step 1, the pressing process is to fix the mold at a pressure of 30 MPa for 10 min.
9. The methanol catalytic conversion synthesis method according to claim 5, characterized in that: In step 1, the drying process is to place it in a drying oven at 50° C. for 3 h to obtain the final single-layer graphite substrate.
10. The methanol catalytic conversion synthesis method according to claim 5, characterized in that: In step 2, in the ammonium hydroxide / ethanol mixed solution, the concentration of the ammonium hydroxide solution is 25%, and the concentration of the ethanol solution is 99.5%, and the volume ratio of the two is 1:3; In step 2, the rotary evaporation temperature is 60°C; In step 2, the drying and calcining process is to dry at 60°C for 48 hours; the dried precipitate is placed in an aluminum crucible and calcined at 800°C in a muffle furnace for 6 hours.