Leading edge structures for airfoils and systems and methods for making same

Through cold spray additive manufacturing technology, metal powder is deposited in the leading edge structure of the airfoil to form inner, intermediate and outer layers of complex shapes, solving the problem that the prior art is difficult to create complex aerodynamic shapes, and realizing the Improved strength and wear resistance, suitable for modern aircraft.

CN119018340APending Publication Date: 2024-11-26THE BOEING CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410629593.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively manufacture the leading edge structure of airfoils in complex aerodynamic shapes, especially while maintaining strength and reducing weight, conventional manufacturing techniques are difficult to meet the needs of modern aircraft.

Method used

Cold spray additive manufacturing technology is used to deposit metal powder on the tool surface of the mandrel to form a complex leading edge structure, including inner layer, intermediate layer and outer layer, ensuring the strength and wear resistance of the structure.

Benefits of technology

Efficient protection of the leading edge of the airfoil is achieved, manufacturing capabilities for complex aerodynamic shapes are provided, weight reduction is reduced, while avoiding the problems of material incompatibility and stress deformation in traditional technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018340A_ABST
    Figure CN119018340A_ABST
Patent Text Reader

Abstract

The invention discloses a leading edge structure for an airfoil and a system and method for manufacturing the same. Systems and methods for manufacturing a protective leading edge structure for an airfoil include a system having a mandrel and a cold spray additive manufacturing device. A cold spray additive manufacturing apparatus is configured to deposit a metal powder on a tool surface of the mandrel to form an inner layer, an intermediate layer, and an outer layer of the leading edge structure. The inner layer forms an inner surface of the leading edge structure. The outer layer forms an outer surface of the leading edge structure. The intermediate layer forms a thickness of the leading edge structure. The inner surface of the leading edge structure is configured to be coupled to the airfoil such that the outer surface of the leading edge structure forms a portion of the leading edge of the airfoil and a portion of the aerodynamic surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates generally to aerodynamic structure manufacturing, and more particularly to systems and methods for manufacturing leading edge structures of airfoils, such as rotor blades, using cold spray additive manufacturing. Background Art

[0002] The leading edges of airfoils, such as helicopter rotors, aircraft propellers, turbine rotors, and other rotating parts, are subject to wear, erosion, and / or damage during operation due to the impact of foreign matter in the air. Therefore, covers made of impact- and wear-resistant materials, such as titanium, steel, nickel, and alloys thereof, have been assembled on the airfoils to provide protection to the leading edges. However, as the aerodynamic design and geometry of airfoils have evolved, it has become increasingly challenging to manufacture material covers for the leading edges using conventional manufacturing techniques. Therefore, those skilled in the art continue to conduct research and development in the field of aerodynamic structure manufacturing. Summary of the invention

[0003] Examples of a system for manufacturing a leading edge structure of an airfoil, a method for manufacturing a leading edge structure of an airfoil, a leading edge structure of an airfoil manufactured using the system or according to the method, an airfoil, and a method for manufacturing an airfoil are disclosed. The following is a non-exhaustive list of examples of the subject matter of the present disclosure, which may or may not be claimed.

[0004] In one example, the disclosed system includes a mandrel including a tool surface. The system includes a cold spray additive manufacturing device. The cold spray additive manufacturing device is configured to deposit metal powder on the tool surface of the mandrel to form an inner layer of the leading edge structure. The cold spray additive manufacturing device is configured to deposit the metal powder on the inner layer to form an intermediate layer of the leading edge structure. The cold spray additive manufacturing device is configured to deposit the metal powder on the intermediate layer to form an outer layer of the leading edge structure. The inner layer forms an inner surface of the leading edge structure. The outer layer forms an outer surface of the leading edge structure opposite to the inner surface and a thickness of the leading edge structure between the inner surface and the outer surface. The intermediate layer forms a thickness of the leading edge structure between the inner surface and the outer surface. The inner surface of the leading edge structure is configured to be coupled to the airfoil so that the outer surface of the leading edge structure forms a portion of the leading edge of the airfoil and a portion of the aerodynamic surface.

[0005] In one example, the disclosed method includes the following steps: (1) cold spraying the metal powder on the tool surface of the mandrel to form an inner layer of the leading edge structure; (2) cold spraying the metal powder on the inner layer to form multiple intermediate layers of the leading edge structure; and (3) cold spraying the metal powder on the intermediate layer to form an outer layer of the leading edge structure. The inner layer forms an inner surface of the leading edge structure. The outer layer forms an outer surface of the leading edge structure opposite the inner surface. The intermediate layer forms the thickness of the leading edge structure between the inner surface and the outer surface. The inner surface of the leading edge structure is configured to be coupled to the airfoil so that the outer surface of the leading edge structure forms a portion of the leading edge and a portion of the aerodynamic surface of the airfoil.

[0006] In one example, a leading edge structure is disclosed that includes an inner surface configured to be coupled to the airfoil. The leading edge structure includes an outer surface that is opposite the inner surface and is configured to form a portion of a leading edge and a portion of an aerodynamic surface of the airfoil. The leading edge structure is manufactured by depositing niobium powder on a tool surface of a mandrel using a cold spray additive manufacturing process.

[0007] In one example, a disclosed airfoil includes a composite body. The composite body includes a tip and a root opposite the tip. The composite body includes a leading edge, the leading edge including a leading edge first portion extending from the root toward the tip. The composite body includes a trailing edge opposite the leading edge and extending from the root to the tip. The airfoil also includes a leading edge structure coupled to the leading edge of the composite body and forming a leading edge second portion of the leading edge extending from the leading edge first portion to the tip. The leading edge structure is manufactured by depositing niobium powder on a tool surface of a mandrel using a cold spray additive manufacturing process.

[0008] In one example, the disclosed method includes the following steps: (1) manufacturing a composite body including a tip, a root opposite the tip, a leading edge including a leading edge first portion extending from the root toward the tip, and a trailing edge opposite the leading edge and extending from the root to the tip; (2) manufacturing a leading edge structure by depositing niobium powder on a tool surface of a mandrel using a cold spray additive manufacturing process; and (3) coupling the leading edge structure to the leading edge of the composite body to form a leading edge second portion extending from the leading edge first portion to the tip.

[0009] Other examples of the systems, methods, leading edge structures, and airfoils disclosed herein will become apparent from the following detailed description, the accompanying drawings, and the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 is a schematic perspective view of an example of a rotor;

[0011] Figure 2 is a schematic cross-sectional view of a portion of an example of a rotor blade;

[0012] Figure 3 is a schematic plan view of an example of a rotor blade having a leading edge structure;

[0013] Figure 4 is a schematic exploded plan view of an example of a rotor blade and leading edge structure;

[0014] Figure 5 is a schematic perspective view of an example of a leading edge structure;

[0015] Figure 6 is a schematic front view of an example of a leading edge structure;

[0016] Figure 7 is a schematic plan view of an example of a leading edge structure;

[0017] Figure 8 is a schematic diagram of an example of a manufacturing environment for manufacturing a leading edge structure using a cold spray process;

[0018] Fig. 9 is a schematic diagram of an example of using a cold spray process to manufacture a leading edge structure;

[0019] Fig.10 is a schematic block diagram of an example of a manufacturing environment, an airfoil, and a leading edge structure;

[0020] Fig.11 is a flow chart of an example of a method for manufacturing a leading edge structure using a cold spray process;

[0021] Fig.12 is a flow chart of an example of a method for manufacturing an airfoil having a leading edge structure;

[0022] Fig.13 is a flowchart of an example of an aircraft manufacturing and service method; and

[0023] Fig.14 is a schematic block diagram of an example of an aircraft. DETAILED DESCRIPTION

[0024] Reference Figures 1 to 12, by way of example, the present disclosure relates to a system 100 and a method 1000 for manufacturing a leading edge structure 102 of an airfoil 104. More specifically, the system 100 and the method 1000 relate to manufacturing the leading edge structure 102 using a cold spray additive manufacturing process that utilizes a single component build material and a single build-up mandrel. By way of example, the present disclosure also relates to a leading edge structure 102 of an airfoil 104 manufactured using the system 100 and / or according to the method 1000. By way of example, the present disclosure also relates to an airfoil 104 that includes a leading edge structure 102 that forms a portion of a leading edge of the airfoil 104. By way of example, the present disclosure additionally relates to a method 2000 for manufacturing an airfoil 104.

[0025] In the example shown herein, airfoil 104 includes or takes the form of a rotor blade of a helicopter or other rotorcraft. However, in other examples, airfoil 104 may include or take the form of an aircraft propeller, a turbine rotor blade, a fan rotor blade, and other rotating airfoils.

[0026] The present disclosure recognizes that in the process of striving to improve the operating efficiency of modern aircraft, it is desirable to reduce weight while maintaining the strength of component parts. By using composite materials (including, for example, fiber-reinforced polymer composites), weight reduction of components (such as rotor blades, propeller blades, fan blades, etc.) has been achieved without reducing their strength. In addition, the use of composite materials also enables efficient aerodynamic designs with complex surface geometries, which cannot be achieved using traditional materials. However, composite blades may need to be enhanced at their leading edges to provide sufficient strength to protect the blades from erosion and foreign matter damage. As the aerodynamic geometry of composite blades becomes more complex, conventional techniques (such as electroforming and thermomechanical forming) for providing leading edge protection for rotor blades, propeller blades, fan blades and other airfoil blades become increasingly challenging. In addition, conventional materials and techniques for manufacturing and attaching leading edge protection may not be sufficient to meet the needs of modern aircraft. The present disclosure solves the above-identified problems regarding leading edge protection of blades and other airfoils by using a unique cold spray additive manufacturing technique to manufacture a leading edge structure 102.

[0027] Figure 1 An example of a rotor 110 of a rotorcraft is schematically shown. Rotor 110 includes a plurality of rotor blades 106, also referred to in the singular as rotor blades 106. Rotor blades 106 are airfoil members 104 ( Fig.10). Each of rotor blades 106 includes leading edge 108, trailing edge 112, tip 114, root 116, upper aerodynamic surface 160, and lower aerodynamic surface 162. Rotor blade 106 is coupled to hub 166 at root 116. Rotor mast 168 is coupled to hub 166 and rotates rotor blade 106 in the direction of directional arrow 170. Each of rotor blades 106 is made of composite material 172 ( Fig.10 ) (such as fiber reinforced polymer (FRP)). Each of rotor blades 106 includes a leading edge structure 102. Leading edge structure 102 is coupled (e.g., bonded or adhered) to rotor blade 106 to form a single structural unit and thereby protects at least a portion of a leading edge 108 of rotor blade 106 from impact and erosion, wear, and / or damage.

[0028] In one or more examples, the leading edge structure 102 is coupled to and protects an outboard end or outboard portion of a leading edge 108 of a rotor blade 106. In one or more examples, the leading edge structure 102 is coupled to and protects an outboard portion and a middle portion of a leading edge 108 of a rotor blade 106. In one or more examples, the leading edge structure 102 is coupled to and protects an outboard portion, a middle portion, and an inboard portion of a leading edge 108 of a rotor blade 106.

[0029] Generally speaking, leading edge structure 102 carries a portion of the loads applied to airfoil 104 (e.g., rotor blade 106) during operation. Leading edge structure 102 also has a degree of strain capacity to allow for conformance with the underlying airfoil structure and any adhesive bondline between airfoil 104 and leading edge structure 102. Thus, "strength" when used to describe leading edge structure 102 refers to resistance to impact, erosion, and wear, as well as the ability to carry aerodynamic loads.

[0030] In one or more examples, a single instance or segment of leading edge structure 102 (e.g., one leading edge structure segment) is coupled to rotor blade 106 or airfoil 104 to protect a desired portion of leading edge 108 between root 116 and tip 114. In one or more examples, multiple instances or segments of leading edge structure 102 (e.g., a series of leading edge structure segments) are coupled to rotor blade 106 or airfoil 104 along the span direction to protect a desired portion of leading edge 108 between root 116 and tip 114. In one or more examples, one or more leading edge structure segments may be manufactured using different manufacturing processes, may be manufactured using different materials, and / or may have a size and shape determined by the airfoil operating environment, materials, coverage, and thickness.

[0031] Figure 2 The rotor blades 106 ( Figure 1 ) in one of the following examples. Figure 2 The rotor blade 106 shown is an airfoil 104 ( Fig.10 ). Rotor blade 106 includes aerodynamic surfaces 152, such as upper aerodynamic surface 160 (e.g., suction side or low pressure side) and lower aerodynamic surface 162 (e.g., pressure side or high pressure side). Rotor blade 106 includes composite body 174, which is composed of composite material 172 ( Fig.10 ) (such as a fiber reinforced polymer composite material) and has, for example, an airfoil shape (eg, an airfoil body). Leading edge structure 102 is coupled to support surface 164 of composite body 174 of rotor blade 106 .

[0032] Figure 2 An example of a leading edge structure 102 having an approximately constant thickness 176 in the chord direction is shown. The present disclosure recognizes that it is more common for airfoil and blade designs to have a thickness that tapers in the chord direction. Additionally, manufacturing a leading edge structure 102 that includes a complex portion with tapered thickness is an advantage of using a cold spray process. Furthermore, Figure 2 The example shown has no additional layer errors superimposed.

[0033] In one or more examples, support surface 164 comprises a structural substrate or otherwise provides or serves as an underlying support and attachment surface for leading edge structure 102. For example, support surface 164 forms a portion of an outer mold line (OML) of rotor blade 106 made of composite material 172. Support surface 164 is set back (e.g., offset) from aerodynamic surface 152 of rotor blade 106 such that a recess is formed to receive leading edge structure 102. The recess or offset of support surface 164 from aerodynamic surface 152 of rotor blade 106 is equal to a thickness 176 of leading edge structure 102 and any adhesive used to bond leading edge structure 102 to rotor blade 106. Thus, with leading edge structure 102 coupled to support surface 164 of rotor blade 106, leading edge structure 102 forms a portion of leading edge 108 of rotor blade 106 and a portion of aerodynamic surface 152 of rotor blade 106.

[0034] In one or more examples, for example, leading edge structure 102 is bonded to underlying blade structure (support surface 164) using a structural adhesive that satisfies the interfacial stress and strain environment. In one or more examples, leading edge structure 102 is bonded to rotor blade 106 prior to curing of composite material 172, and rotor blade 106 is cured with leading edge structure 102 in place. In one or more examples, rotor blade 106 is cured and then leading edge structure 102 is bonded to rotor blade 106.

[0035] In one or more examples, the leading edge structure 102 includes an inner surface 124, an outer surface 126 opposite the inner surface 124, and a thickness 176 between the inner surface 124 and the outer surface 126. The inner surface 124 forms the internal geometry of the leading edge structure 102. The inner surface 124 of the leading edge structure 102 is configured (e.g., sized, shaped, etc.) to complement or substantially match the profile of the support surface 164, so that the inner surface 124 and the support surface 164 are in close fitting contact with the leading edge structure 102 coupled to the rotor blade 106. In one or more examples, the inner surface 124 is adhesively bonded to the support surface 164. With the leading edge structure 102 coupled to the rotor blade 106, the outer surface 126 forms a portion of the leading edge 108 of the rotor blade 106 and a portion of the aerodynamic surface 152 of the rotor blade 106. For example, leading edge structure 102 is manufactured using cold spray additive manufacturing with an appropriate value for thickness 176 such that outer surface 126 of leading edge structure 102 has a profile that extends continuously from aerodynamic surface 152 of rotor blade 106 .

[0036] In one or more examples, the leading edge structure 102 includes a head portion 178, an upper portion 180, and a lower portion 182. The head portion 178 forms a leading edge vertex of the leading edge structure 102 and is configured to be positioned along the leading edge 108 of the rotor blade 106. The upper portion 180 extends from the head portion 178 toward the trailing edge 112 of the rotor blade 106. The lower portion 182 extends from the head portion 178 opposite the upper portion 180 toward the trailing edge 112 of the rotor blade 106. The outer surface 126 of the head portion 178 of the leading edge structure 102 is configured to form a portion of the leading edge 108 of the rotor blade 106. The outer surface 126 of the upper portion 180 is configured to form a portion of the upper aerodynamic surface 160 of the rotor blade 106. The outer surface 126 of the lower portion 182 is configured to form a portion of the lower aerodynamic surface 162 of the rotor blade 106.

[0037] In one or more examples, the thickness 176 of the leading edge structure 102 is constant in the chord-wise direction and / or the span-wise direction. In one or more examples, the thickness 176 of the leading edge structure 102 varies in the chord-wise direction and / or the span-wise direction.

[0038] In one or more examples, the thickness 176 of the leading edge structure 102 includes a tapered thickness distribution in one or more directions. The tapered thickness distribution is based on a designed chord and / or span variation, which is optimized for erosive wear based on impact angle, impact velocity, and erosive agent concentration. In addition, the thickness variation can be optimized or balanced for weight, weight distribution, structural life, and adhesive layer life. The tapered thickness distribution of the leading edge structure 102 can vary. In one or more examples, the area of ​​the thickness 176 from the structural leading edge 194 of the leading edge structure 102 to the structural trailing edge 196 of the leading edge structure 102 has a ratio greater than five times (5X), such as ten times (10X) or more. For example, the thickness 176 of the front end of the head portion 178 or the upper portion 180 and / or the lower portion 182 may be greater than five times the thickness 176 of the rear end of the upper portion 180 and / or the lower portion 182. For example, the thickness 176 at the head portion 178 or the front end of the upper portion 180 and / or the lower portion 182 is about 0.1 inches, and the thickness 176 at the rear end of the upper portion 180 and / or the lower portion 182 is about 0.01 inches.

[0039] Figure 3 and Figure 4 An example of a rotor blade 106 and a leading edge structure 102 is schematically illustrated. Figure 3 Leading edge structure 102 is depicted coupled to rotor blade 106 . Figure 4 Leading edge structure 102 is depicted separated from rotor blade 106. Figure 3 As shown, after attachment of leading edge structure 102 (e.g., with leading edge structure 102 attached), leading edge 108 of rotor blade 106 includes leading edge first portion 128 and leading edge second portion 130. Leading edge first portion 128 extends from near (e.g., at or near) root 116 of rotor blade 106 toward tip 114. Leading edge second portion 130 extends from leading edge first portion 128 to near (e.g., at or near) tip 114. Leading edge first portion 128 is formed by aerodynamic surface 152 of composite body 174 of rotor blade 106. Leading edge second portion 130 is formed by aerodynamic surface 152 of metal body 198 of leading edge structure 102. Leading edge first portion 128 and leading edge second portion 130 form or are positioned along an outer mold line of rotor blade 106. As shown in FIG. Figure 4As shown, in one or more examples, rotor blade 106 is manufactured such that leading edge 108 includes or is formed by leading edge first portion 128 and leading edge setback portion 184. In other words, prior to attachment of leading edge structure 102 (e.g., in a case where leading edge structure 102 is not attached), leading edge 108 of rotor blade 106 includes leading edge first portion 128 and leading edge setback portion 184. Leading edge first portion 128 forms or is located along an outer mold line of rotor blade 106. Leading edge setback portion 184 is formed by support surface 164 of rotor blade 106. Leading edge setback portion 184 is offset from the outer mold line of rotor blade 106 and leading edge first portion 128.

[0040] Figures 5 to 7 An example of a leading edge structure 102 is schematically shown. In one or more examples, the leading edge structure 102 includes a metal body 198 ( Fig.10 ) and has an airfoil shape. Generally speaking, the airfoil shape of metal body 198 of leading edge structure 102 complementarily matches the airfoil shape of a portion of composite body 174 of rotor blade 106 .

[0041] The metal body 198 of the leading edge structure 102 includes a structure first end 186, a structure second end 188, a structure upper surface 190 (e.g., an upper airfoil surface), a structure lower surface 192 (e.g., a lower airfoil surface), a structure leading edge 194, and a structure trailing edge 196. The structure first end 186 is configured to be located at the rotor blade 106 ( Figure 3 ) near the tip 114 of the rotor blade 106 ( Figure 3 ). Structural second end 188 is opposite structural first end 186 along the longitudinal axis of leading edge structure 102 and is configured to be spaced apart from tip 114 of rotor blade 106 toward root 116 of rotor blade 106. Structural leading edge 194 is configured to form a portion of leading edge 108 of rotor blade 106, such as leading edge second portion 130 ( Figure 3 For example, structural leading edge 194 is formed by a portion of outer surface 126 of head portion 178 of metal body 198 of leading edge structure 102. Structural trailing edge 196 is opposite structural leading edge 194 in the chordwise direction and is configured to abut a portion of composite body 174 of rotor blade 106 such that structural upper surface 190 forms a continuous aerodynamic surface contour with upper aerodynamic surface 160 of rotor blade 106 and structural lower surface 192 is contiguous with rotor blade 106 ( Figure 2) forms a continuous aerodynamic surface contour. The structural upper surface 190 is formed by a portion of the outer surface 126 of the upper portion 180 of the metal body 198 of the leading edge structure 102. The structural lower surface 192 is formed by a portion of the outer surface 126 of the lower portion 182 of the metal body 198 of the leading edge structure 102.

[0042] In various examples, the aerodynamic geometry of the leading edge structure 102 depends on one or more factors, such as, but not limited to, the type of airfoil or blade to which the leading edge structure 102 is to be attached, the type of machine (e.g., rotorcraft, aircraft, fan, etc.) for which the leading edge structure 102 will be used, and / or the operating conditions under which the leading edge structure 102 will be used. In one or more examples, the metal body 198 of the leading edge structure 102, such as manufactured using a cold spray process, has a complex aerodynamic shape and / or a complex shape of the structure leading edge 194. In one or more examples, the chord dimension (e.g., chord width) of the leading edge structure 102 at the second end 188 of the structure is greater than the chord dimension (e.g., chord width) of the leading edge structure 102 at the first end 186 of the structure (e.g., twice as large). In one or more examples, the leading edge structure 102 has a taper in the chord direction. In one or more examples, the leading edge structure 102 has a dihedral shape or is configured for use with a dihedral blade or airfoil having a positive (e.g., upward) slope. In one or more examples, the leading edge structure 102 has an anhedral shape or is configured for use with an anhedral blade having an airfoil with a negative (e.g., downward) slope. In one or more examples, the leading edge structure 102 includes a profile that transitions between different geometries. In one or more examples, the leading edge structure 102 includes a nonlinear twist about the spanwise direction. In one or more examples, the thickness 176 of the leading edge structure 102 varies to form a taper from a thicker portion at the head portion 178 or along the leading edge 194 of the structure to a thinner portion, along the upper portion 180 and / or the lower portion 182 toward the trailing edge 196 of the structure. In one or more examples, the metal body 198 of the leading edge structure 102 includes an inlet or peripheral cutout 200.

[0043] In one or more examples, the leading edge structure 102 manufactured using the system 100 and / or according to the method 1000 includes any desired geometry with various levels of complexity. In one or more examples, the leading edge structure 102 includes a length (e.g., a span from the first end 186 of the structure to the second end 188 of the structure) and a width (e.g., a chord distance from the leading edge 194 of the structure to the trailing edge 196 of the structure) ratio from about 5:1 to about 20:1 (such as about 12:1). In one or more examples, the leading edge structure 102 includes a swept tip, for example, the leading edge 194 of the leading edge structure 102 and / or the trailing edge 196 of the structure are not in a straight line. In one or more examples, the leading edge structure 102 includes one of a dihedral angle and an anhedral angle, for example, a flap direction returning upward and downward along the z-axis or along the airfoil 104, respectively. In one or more examples, the leading edge structure 102 accommodates an airfoil profile transition, wherein the airfoil shape along the chord changes in length, for example, from thicker to thinner. In one or more examples, the leading edge structure 102 includes a chord-to-chord taper, where the distance along the chord direction from the structure leading edge 194 to the structure trailing edge 196 varies with length and / or the airfoil profile scales from larger to smaller. In one or more examples, the leading edge structure 102 includes a nonlinear twist where the chord angle rotation varies over the length. In one or more examples, the leading edge structure 102 includes a thickness taper profile, where the chord thickness changes from the structure leading edge 194 to the structure trailing edge 196 and / or the spanwise thickness changes from the inner end (e.g., the structure first end 186) to the outer end (e.g., the structure second end 188). In one or more examples, the leading edge structure 102 includes a plurality of cutout features, such as the cutout 200 ( Figure 6 ). In one or more examples, the leading edge structure 102 is manufactured to include a desired airfoil profile and other geometric tolerances. In one or more examples, the leading edge structure 102 includes a desired surface finish, for example, a smooth surface finish at the inner molded surface for bonding that generally avoids excessive deposition and / or surface effects. In one or more examples, the leading edge structure 102 includes other features, such as a "step-down" or depression of the airfoil profile intended to enter under the adjacent leading edge portion.

[0044] In one or more examples, the airfoil 104, such as the rotor blade 106, has a very small upper and lower airfoil radius at the transition of its profile. Therefore, in one or more examples, the inner radius of the head portion 178 of the leading edge structure 102 formed by the inner surface 124 is different from the outer radius of the head portion 178 of the leading edge structure 102 formed by the outer surface 126. In one or more examples, the inner radius is smaller than the outer radius.

[0045] Figure 8An example of the system 100 and a manufacturing environment 202 within which the system 100 operates to manufacture the leading edge structure 102 is schematically illustrated. Fig. 9 An example of a leading edge structure 102 fabricated by a cold spray process using the system 100 is schematically illustrated. In general, the system 100 includes a mandrel 118 and a cold spray additive manufacturing apparatus 120, which may also be referred to herein as a cold spray apparatus 120. The cold spray apparatus 120 is configured to perform a cold spray process or cold spray deposition.

[0046] As used herein, "cold spray process" or "cold spray deposition" refers to a solid-state process that generally involves fluidizing a fine (micron) metal powder in a gas (such as helium or other inert gas) stream, followed by spraying the resulting powder and gas mixture directly through a nozzle at sonic speeds, thereby causing the accelerated metal powder to impact the build surface with sufficient force to establish an interfacial bond between the deposited powdered metal material and the build surface. Such processes are referred to as "cold" techniques because the gas / powder stream has a relatively low temperature when it strikes the substrate. In the present disclosure, the substrate is the mandrel 118.

[0047] The cold spray device 120 is configured to perform a suitable cold spray process, wherein the cold spray device 120 uses a fluid to accelerate the metal powder 132 at a very high speed toward the tool surface 122 of the mandrel 118. The fluid is typically a gas fluid, such as nitrogen or helium. When the particles of the metal powder 132 impact the tool surface 122 of the mandrel 118, the particles of the metal powder 132 are locally plastically deformed so that the metal powder 132 can be bonded to the tool surface 122 of the mandrel 118. In this way, the tool surface 122 of the mandrel 118 defines the shape of the inner surface 124 of the metal body 198 of the leading edge structure 102. After the particles of the metal powder 132 build a layer on the mandrel 118 (e.g., the inner layer 136 of the metal body 198), new particles of the metal powder 132 are deformed on the surface of the inner layer 136, they impact and bond to the inner layer 136, and then new particles of the metal powder 132 are deformed on the surface of the previously built layer, they impact and bond to the previously built layer, thereby subsequently forming multiple intermediate layers 224 built on the previous layers and increasing the thickness 176 of the metal body 198 of the leading edge structure 102 until an outer layer 138 is formed, which forms the outer surface 126 of the leading edge structure 102.

[0048] In one or more examples, a cold spray process that promotes plastic deformation is performed by accelerating particles of metal powder 132 to a velocity in the range of about 300 m / s to about 1500 m / s. This is achieved by accelerating a fluid to a velocity that is generally higher than the velocity desired for particles of metal powder 132 and then allowing particles of metal powder 132 to be dragged in the fluid stream. The temperature of the fluid in the cold spray device 120 for propelling particles of metal powder 132 is generally maintained between about 20 degrees Celsius (68 degrees Fahrenheit) and about 1,000 degrees Celsius (1,832 degrees Fahrenheit). The temperature is selected to ensure that the metal powder material used remains solid so as to allow for proper deformation and bonding. As desired for the cold spray process, the temperature and / or velocity may be adjusted to increase or decrease the gas velocity, for example, to achieve a sufficiently high velocity for propelling the powder material at a velocity capable of forming a very dense deposit, or to achieve a sufficiently low velocity for propelling the powder material at a velocity capable of forming a less dense deposit. Although most gases or fluids have the potential to adequately accelerate metal powder particles, typical gases used in cold spray processes include inert and semi-inert gases, such as nitrogen and helium, although one skilled in the art may use alternative fluids to accelerate particles. In one or more examples, the velocity of the metal powder 132 may be affected by the density of the gas selected during the cold spray process.

[0049] like Figure 8 As shown, in one or more examples, the cold spray device 120 includes a gas source 210, a gas heater 212, a powder metering device 214, a nozzle 216, and a motion control device 208 for depositing the metal powder 132 on the tool surface 122 of the mandrel 118 to form the metal body 198 of the leading edge structure 102, as shown in FIG. Fig. 9 In one or more examples, the cold spray device 120 is configured to form the metal body 198 of the leading edge structure 102 on the tool surface 122 in a layer-by-layer manner, as described above.

[0050] In one or more examples, a pressurized gas stream is supplied from a gas source 210 to a gas heater 212 and then to a nozzle 216. The gas stream includes a gas 222, such as nitrogen, helium, other inert gases, and combinations thereof. The gas stream is supplied from the gas source 210 at a suitable pressure (e.g., from about 300 psi to about 1,000 psi, such as between about 400 psi and about 500 psi, such as about 450 psi). The gas heater 212 heats the gas stream to a suitable temperature (e.g., from about 500°F (260°C) to about 1900°F (1038°C)) using any of a variety of conventional heating techniques, and then supplies the resulting heated gas stream to the nozzle 216 at a suitable pressure and temperature. In one or more examples, the metal powder 132 is supplied from a powder metering device 214 and combined with the gas stream from the gas source 210 and supplied to the nozzle 216. The selection of the particle size of the metal powder 132 affects (e.g., increases) deformation, which in turn can lead to better adhesion. A suitable powder feed rate (e.g., about 1 g / min to about 20 g / min) of the metal powder 132 into the gas stream is used. The powder feed rate can be used to increase or decrease the thickness of the deposit, as well as to tailor the microstructure and mechanical properties of the deposit as desired. In one or more examples, the nozzle 216 is a conventional converging / diverging nozzle to accommodate the mixing of the gas 222 and the metal powder 132. In one or more examples, a heated first gas stream is introduced into the nozzle 216 at a first inlet, and a metal powder 132 driven by a second gas stream is introduced into the nozzle 216 at a second inlet, wherein the metal powder 132 can be mixed, accelerated, and heated by the gas 222. The size of the resulting deposit of the metal powder 132 can vary. In one or more examples, the deposit has a thickness of about 1.0 mm to about 2.0 mm. In one or more examples, the cold spray device 120 uses a motion control device 208 (such as a robotic arm) under computer control to apply multiple layers of deposits to the leading edge structure 102 ( Fig. 9 ) is accumulated into a near net shape, thereby controlling the placement and orientation of the deposit of metal powder 132. In addition, the nozzle traverse speed controls the layer thickness of each pass, for example, in each pass, a lower traverse speed results in an increase in the deposited layer thickness, and an increase in the traverse speed results in a decrease in the deposited layer thickness. Generally, the net total thickness is controlled by the number of passes. As an example, 0.003 inches to 0.01 inches per pass is suitable, with a net thickness of between about 0.01 inches to about 0.1 inches.

[0051] In one or more examples, the mandrel 118 is supported by a positioning plate 206. In one or more examples, the positioning plate 206 is coupled to a platform 220 that is configured to move the mandrel 118 relative to the cold spray device 120. As an example, the platform 220 is configured to selectively rotate the positioning plate 206, and therefore the mandrel 118, about a longitudinal axis of the mandrel 118 and / or relative to the cold spray device 120. In one or more examples, the cold spray device 120 is coupled to or includes a motion control device 208, such as a robotic arm, an overhead gantry, or other automated motion control device, that is configured to move the cold spray device 120 relative to the mandrel 118, for example, along the longitudinal axis of the mandrel 118, while depositing the metal powder 132 during the cold spray process.

[0052] In one or more examples, the mandrel 118 is designed and manufactured to enable easy release of the inner surface 124 from the tool surface 122 and thereby facilitate simple removal of the metal body 198 of the leading edge structure 102 manufactured using a cold spray process, such as without requiring or using a release layer located between the tool surface 122 and the inner surface 124 (e.g., the inner layer 136) of the metal body 198 of the leading edge structure 102.

[0053] In one or more examples, the mandrel 118 is a unitary structure. The mandrel 118 as a unitary structure provides a continuous tool surface 122. The tool surface 122 as a continuous surface eliminates the possibility of the metal powder 132 colliding, deforming, and bonding within seams or discontinuities in the tool surface 122, which may hinder the release of the leading edge structure 102 from the mandrel 118. Moreover, the use of a cold spray process to manufacture the leading edge structure 102 as a single unitary structure on the mandrel 118 eliminates seam discontinuities when multiple tools and multiple deposits are combined to produce a net deposit. Seams in leading edge protection weaken the structure and create significant deficiencies in resisting erosion and damage.

[0054] In one or more examples, the mandrel 118 includes or is made of a material having a first hardness 140. As an example, the mandrel 118 can be manufactured using a hardened steel material. The particles of the metal powder 132 include a second hardness 142. In one or more examples, the first hardness 140 is greater than the second hardness 142. For example, the first hardness 140 is sufficiently higher than the second hardness 142 so that the particles of the metal powder 132 do not deform or erode the tool surface 122 when they impact. Therefore, the inner layer 136 of the metal body 198 of the leading edge structure 102 manufactured using the cold spray process tends not to be firmly bonded to the tool surface 122, thereby enabling the leading edge structure 102 to be released from the mandrel 118.

[0055] In one or more examples, the cold spray device 120 is selectively controlled to enable easy release of the inner surface 124 from the tool surface 122 and thereby facilitate simple removal of the metal body 198 of the leading edge structure 102 manufactured using the cold spray process, such as without requiring or using a release layer located between the tool surface 122 and the inner surface 124 (e.g., the inner layer 136) of the metal body 198 of the leading edge structure 102.

[0056] In one or more examples, the velocity of the metal powder 132 sprayed or deposited on the tool surface 122 is selectively controlled and / or adjusted throughout the cold spray process so that at least the inner layer 136 of the metal body 198 of the leading edge structure 102 manufactured using the cold spray process tends not to adhere or bond firmly to the tool surface 122, thereby enabling easier release of the leading edge structure 102 from the mandrel 118. In one or more examples, at least the inner layer 136 and optionally one or more intermediate layers 224 are formed by depositing the metal powder 132 at a velocity that is lower than (e.g., lower than about 5% to 25%) the adhesion level of the metal powder 132. After the formation of the inner layer 136 and optionally one or more intermediate layers 224, the intermediate layers 224 and the remainder of the outer layer 138 are formed by depositing the metal powder 132 at a velocity that is equal to or higher than the adhesion level of the metal powder 132.

[0057] In one or more examples, adhesion or adhesion level of the metal powder 132 refers to a level of adhesion (e.g., cohesion) that describes permanent adhesion between the cold spray and the substrate, temporary adhesion between the cold spray and the mandrel prior to release, and / or between particles and particle layers that can translate into material strength, ductility, toughness, erosion resistance, etc.

[0058] In one or more examples, the particle size and / or particle shape of the metal powder 132 is selected and / or controlled to affect adhesion. The particle size and / or particle shape of the metal powder 132 is indirectly related to the impact velocity based on its flow rate within the carrier gas. However, in other examples, the carrier gas is most directly used to control the particle velocity, such as by using different gas densities, changing the gas temperature, and / or changing the gas pressure.

[0059] In one or more examples, other process parameters may be selected, modified, and / or controlled to control the level of adhesion of the metal powder 132. Examples of such parameters include the type of nozzle used with the cold spray device 120, the distance of the nozzle to the mandrel / part surface (e.g., standoff distance), the nozzle angle, the nozzle geometry, the nozzle motion, and / or control of the powder plume size and resulting deposit.

[0060] In one or more examples, the leading edge structure 102 includes or is made of a relatively light and strong metal material using a cold spray device 120, which is heat and wear resistant. In one or more examples, the metal body 198 of the leading edge structure 102 is made of a single (e.g., single component) metal material 204. In one or more examples, the leading edge structure 102 is made of niobium 144 (e.g., niobium 144 is a single component metal material 204). In one or more examples, the leading edge structure 102 is made of another type of refractory metal 154, such as tungsten, molybdenum, tantalum, rhenium, and alloys or combinations thereof.

[0061] In other examples, the cold spray process uses non-metallic powders. As an example, the powder material used by the cold spray device 120 to manufacture the leading edge structure 102 using the cold spray process is a ceramic powder. As an example, the powder material used by the cold spray device 120 to manufacture the leading edge structure 102 using the cold spray process is a ceramic-metal powder (referred to as a cermet).

[0062] In one or more examples, the leading edge structure 102 is manufactured from a metal powder 132 using a cold spray process. In one or more examples, the metal powder 132 is a niobium powder 134. In one or more examples, the metal powder 132 is another suitable type of refractory metal powder 150. Niobium powder 134 provides many particularly unique advantages over conventional cold spray powder materials. For example, niobium powder has a high melting temperature and is relatively soft, thereby facilitating better consolidation (e.g., deformation and bonding) through cold spraying. After consolidation, the niobium part has a relatively high toughness. In addition, using niobium powder 134 as a single-component build material for manufacturing the leading edge structure 102 eliminates material incompatibility issues that may be common in cold spray manufacturing.

[0063] In one or more examples, niobium 144 is a preferred material because it can be formed into a consolidated deposit of layers that form the metal body 198 of the leading edge structure 102. The niobium powder 134 is relatively soft and can be further refined using powder processing, such as heat treatment (e.g., prior to cold spraying) or adjusting the particle shape and / or size distribution. Niobium cold spraying forms a dense deposit that is well consolidated, has high cohesion between particles and deposited layers, and has low porosity / inherent defects. Niobium can be deposited thinly or thickly to meet airfoil leading edge protection requirements. Once cold sprayed, niobium provides high erosion resistance, which few other materials can achieve, including those that are significantly harder (which leads to low erosion resistance, rapid damage initiation and propagation) due to the presence of defects, poor inter-particle and inter-layer cohesion / adhesion (e.g., titanium, nickel, steel, etc. and their alloys). In addition, different particle spraying methods, such as thermal spraying, are required for very hard and / or ceramic-type particles. The higher hardness material also provides low strain capability of the leading edge protection system and strain mismatch at the glue line (or coupling) between the outer leading edge and the inner structure. In addition, the deposit has low fatigue strength, low or even no yield strength, low failure ductility, high erosion rate and rapid failure mechanism. Although the softer material can provide high strain and strain matching, the static strength and fatigue strength of the deposit are lower, and the erosion performance is reduced to below that of conventional material solutions.

[0064] The present disclosure recognizes that the difference between cold spraying niobium parts and niobium coatings on secondary metal substrates is that cold spraying niobium parts eliminates the need for machining and manufacturing of secondary metal substrates (which is much more difficult due to complex geometry). The benefits of cold spraying niobium parts include avoiding fatigue strength degradation of the substrate, residual stress deformation, and adhesion limitations between the coating and the substrate. The present disclosure also recognizes that niobium is not considered for use in stand-alone components because the traditional form is too soft and not conducive to stand-alone components, such as the leading edge protection structure disclosed herein. Use in powder form is traditionally sintered using powder metallurgy, and the result is also soft. Niobium has a very high melting point, which makes it very difficult to melt, and the use of alloy elements and binders reduces its erosion characteristics and mechanical properties. Cold spraying of coatings (and repairs) is also generally challenged by residual stresses, which appear to make parts (and particularly relatively thin shelled parts) difficult to manufacture due to dimensional and shape distortions (primarily due to the impact on the substrate). Only after evaluating the properties after spraying and heat treatment in addition to the substrate can the properties and shape stability of the deposit be properly evaluated.

[0065] General Reference Figures 1 to 9 And specific reference Fig.10, which schematically illustrates an example of a manufacturing environment 202 in which a system 100 uses a cold spray process to manufacture a leading edge structure 102 for an airfoil 104, such as a rotor blade 106. The following is a list of examples of a system 100 according to the present disclosure. Some elements, features, and / or components described in one example may be combined in various ways with other examples without including other features described in those other examples, even if one or more such combinations are not explicitly described herein by example.

[0066] In one or more examples, the system 100 includes a mandrel 118. The mandrel 118 includes a tool surface 122. The system 100 includes a cold spray additive manufacturing device 120. The cold spray additive manufacturing device 120 is configured to deposit a metal powder 132 on the tool surface 122 of the mandrel 118 to form an inner layer 136 of the leading edge structure 102. The cold spray additive manufacturing device 120 is configured to deposit the metal powder 132 on the inner layer 136 to form an intermediate layer 224 of the leading edge structure 102. The cold spray additive manufacturing device 120 is configured to deposit the metal powder 132 on the intermediate layer 224 to form an outer layer 138 of the leading edge structure 102. The inner layer 136 forms an inner surface 124 of the leading edge structure 102. The outer layer 138 forms an outer surface 126 of the leading edge structure 102 opposite the inner surface 124. Intermediate layer 224 forms the thickness of leading edge structure 102 between inner surface 124 and outer surface 126. Inner surface 124 of leading edge structure 102 is configured to be coupled to airfoil 104 such that outer surface 126 of leading edge structure 102 forms a portion of leading edge 108 and a portion of aerodynamic surface 152 of airfoil 104. As expressed above, the use of mandrel 118 and cold spray device 120 provides a unique and advantageous means of manufacturing protectors for leading edges of airfoils and rotor blades as compared to conventional techniques.

[0067] In one or more examples, the metal powder 132 includes a niobium powder 134. In one or more examples, the metal powder 132 consists essentially of the niobium powder 134. In one or more examples, the metal powder 132 consists of the niobium powder 134. In one or more examples, the metal powder 132 includes a refractory metal powder 150. As described above, for example, using the niobium powder 134 as the primary or sole constituent material of the cold spray process for manufacturing the leading edge structure 102 provides unique advantages over conventional cold spray materials.

[0068] In one or more examples, the cold spray additive manufacturing device 120 is configured to deposit the metal powder 132 at a first speed 146 to form at least the inner layer 136. The cold spray additive manufacturing device 120 is configured to deposit the metal powder 132 at a second speed 148 to form one or more of the intermediate layer 224 and the outer layer 138. The first speed 146 is less than the second speed 148. As expressed above, selectively controlling the deposition rate of the metal powder 132 (e.g., niobium powder 134) at different points in the cold spray process enables easier separation of the leading edge structure 102 from the mandrel 118 when the manufacturing process is completed.

[0069] In one or more examples, the first speed 146 is lower than the adhesion level of the metal powder 132. In one or more examples, the second speed 148 is equal to or higher than the adhesion level of the metal powder 132. In one or more examples, the first speed 146 is at least 5% less than the second speed 148 or the adhesion level. In one or more examples, the first speed 146 is at least 10% less than the second speed 148 or the adhesion level. In one or more examples, the first speed 146 is at least 15% less than the second speed 148 or the adhesion level. In one or more examples, the first speed 146 is at least 20% less than the second speed 148 or the adhesion level. In one or more examples, the first speed 146 is at least 25% less than the second speed 148 or the adhesion level.

[0070] In one or more examples, the threshold for adhesion is considered to be 50% particle adhesion, and this speed for a given material is called the critical speed and also the critical speed ratio "1". The critical speed for niobium is 585 m / s. The upper end of the speed scale is the beginning of substrate / mandrel erosion and should be avoided. Typical values ​​for the quality of the build (for strength and reduced defect consolidation) are about 1.5 or slightly higher. Percentages below the critical speed will reduce the number of particles that adhere and reduce the adhesion strength. For deposition on hard surfaces, this is a variable that affects the speed required for adhesion, driving it higher. For a softer mandrel, a material that may work at 1.2 will easily debond for a harder mandrel. A critical speed ratio somewhere between 1 and 1.5 is desired in the adhesion level for the mandrel. For example, a balance between adhesion and at the same time limiting adhesion to facilitate release is achieved at 1.4 during the entire build process. If it is reduced too much, the bonding layer will debond prematurely, and this may also occur after the subsequent build layer is applied. Raising it too high will increase the amount of force or energy required to separate at the interface. Mandrel geometry and net part thickness also influence the balance of adhesion, so it depends on the part and tool design.

[0071] In one or more examples, the various layers of the metal body 198 of the leading edge structure 102 formed by the cold spray process may have different densities (e.g., deposition densities). As an example, the inner layer 136 includes a first density. One or more of the intermediate layers 224 include a second density. The outer layer 138 includes a third density. In one or more examples, the first density, the second density, and the third density are different. In one or more examples, the second density is greater than the first density and the third density is greater than the second density. For example, the inner layer 136 is the least dense, each subsequent intermediate layer 224 becomes denser, and the outer layer 138 is the densest. In one or more examples, as the ratio becomes lower, the density of the deposit is related to the particle velocity. In general, the density can also be controlled by the impact angle. For example, when spraying at a low angle (e.g., less than 45 degrees), the gap will increase. Any adverse effects on the surface quality can be corrected and consolidated by subsequent construction layers.

[0072] In one or more examples, the various layers of the metal body 198 of the leading edge structure 102 formed by the cold spray process may have different surface areas (e.g., deposit surface areas). As an example, the inner layer 136 includes a first surface area. One or more intermediate layers 224 include a second surface area. The outer layer 138 includes a third surface area. In one or more examples, the first surface area, the second surface area, and the third surface area are different. In one or more examples, the second surface area is less than the first surface area and the third surface area is less than the second surface area. For example, the inner layer 136 has the largest surface area, the surface area of ​​each subsequent intermediate layer 224 becomes smaller, and the outer layer 138 has the smallest surface area.

[0073] In one or more examples, the inner surface 124 of the leading edge structure 102 can be released from the tool surface 122 of the mandrel 118. In one or more examples, the mandrel 118 is a unitary structure. The tool surface 122 is a continuous surface. In one or more examples, the mandrel 118 includes a first hardness 140. The metal powder 132 includes a second hardness 142. The first hardness 140 is greater than the second hardness 142. As expressed above, the material and / or surface characteristics of the mandrel 118 are selected so that the leading edge structure 102 can be more easily separated from the mandrel 118 when the manufacturing process is completed.

[0074] General Reference Figures 1 to 9 And special reference Fig.10, which schematically illustrates an example of a leading edge structure 102 of an airfoil 104 (such as a rotor blade 106) manufactured using a cold spray process. The following is a list of examples of leading edge structures 102 according to the present disclosure. Some elements, features, and / or components described in one example may be combined in various ways with other examples without including other features described in those other examples, even if one or more such combinations are not explicitly described herein by example.

[0075] In one or more examples, the leading edge structure 102 includes an inner surface 124 configured to be coupled to the airfoil 104. The leading edge structure 102 includes an outer surface 126 that is opposite the inner surface 124 and is configured to form a portion of the leading edge 108 and a portion of the aerodynamic surface 152 of the airfoil 104. The leading edge structure 102 is manufactured by depositing niobium powder 134 on the tool surface 122 of the mandrel 118 using a cold spray additive manufacturing process.

[0076] In one or more examples, the leading edge structure 102 is manufactured by depositing the niobium powder 134 at a first speed 146 to form at least an inner layer 136 on the tool surface 122 of the mandrel 118. The leading edge structure 102 is further manufactured by depositing the niobium powder 134 at a second speed 148 to form one or more intermediate layers 224 on the inner layer 136 and an outer layer 138 on the intermediate layer 224. The first speed 146 is less than the second speed 148.

[0077] In one or more examples, the first speed 146 is lower than the adhesion level of the metal powder 132. The second speed 148 is equal to or higher than the adhesion level of the metal powder 132. In one or more examples, the first speed 146 is at least 20% less than the second speed 148 or the adhesion level.

[0078] General Reference Figures 1 to 9 And special reference Fig.10 , which schematically illustrates an example of an airfoil 104 (such as a rotor blade 106) that includes a leading edge structure 102 manufactured using a cold spray process. The following is a list of examples of airfoils 104 according to the present disclosure. Some elements, features, and / or components described in one example may be combined in various ways with other examples without including other features described in those other examples, even if one or more such combinations are not explicitly described herein by example.

[0079] In one or more examples, the airfoil 104 includes a composite body 174. The composite body 174 includes a tip 114 and a root 116 opposite the tip 114. The composite body 174 includes a leading edge 108. The leading edge 108 includes a leading edge first portion 128 extending from the root 116 toward the tip 114. The composite body 174 includes a trailing edge 112 opposite the leading edge 108 and extending from the root 116 to the tip 114. The airfoil 104 includes a leading edge structure 102 coupled to the leading edge 108 of the composite body 174. The leading edge structure 102 forms a leading edge second portion 130 extending from the leading edge first portion 128 to the tip 114. The leading edge structure 102 is manufactured by depositing a niobium powder 134 on a tool surface 122 of a mandrel 118 using a cold spray additive manufacturing process.

[0080] General Reference Figures 1 to 10 And special reference Fig.11 , which shows an example of a method 1000 for manufacturing a leading edge structure 102 using a cold spray process. In one or more examples, the method 1000 uses the system 100 ( Fig.10 ) is implemented. The following is a list of examples of method 1000 according to the present disclosure. Some elements, steps and / or operations described in one example can be combined with other examples in various ways without including other steps described in those other examples, even if one or more such combinations are not explicitly described by example in this article.

[0081] In one or more examples, the method 1000 includes the step of cold spraying the metal powder 132 (e.g., an initial portion or first portion of the metal powder 132) onto the tool surface 122 of the mandrel 118 to form the inner layer 136 of the leading edge structure 102 (block 1002). The method 1000 includes the step of cold spraying the metal powder 132 (e.g., a subsequent portion or second portion of the metal powder 132) onto the inner layer 136 to form the intermediate layer 224 of the leading edge structure 102 (block 1004). The method 1000 includes the step of cold spraying the metal powder 132 (e.g., a subsequent portion or third portion of the metal powder 132) onto the intermediate layer 224 (e.g., an outermost intermediate layer of the intermediate layers 224) to form the outer layer 138 of the leading edge structure 102 (block 1006). In these examples, the inner layer 136 forms the inner surface 124 of the leading edge structure 102. The outer layer 138 forms an outer surface 126 of the leading edge structure 102 opposite the inner surface 124. The intermediate layer 224 forms a thickness of the leading edge structure 102 between the inner surface 124 and the outer surface 126. The inner surface 124 of the leading edge structure 102 is configured to be coupled to the airfoil 104 such that the outer surface 126 of the leading edge structure 102 forms a portion of the leading edge 108 of the airfoil 104 and a portion of the aerodynamic surface 152.

[0082] In one or more examples, according to the method 1000, the metal powder 132 includes a niobium powder 134. In one or more examples, according to the method 1000, the metal powder 132 consists essentially of the niobium powder 134. In one or more examples, according to the method 1000, the metal powder 132 consists of the niobium powder 134. In one or more examples, according to the method 1000, the metal powder 132 includes a refractory metal powder 150.

[0083] In one or more examples, the method 1000 includes depositing the metal powder 132 (e.g., a first portion of the metal powder 132) at a first speed 146 to form at least the inner layer 136 (block 1008). The method 1000 includes depositing the metal powder 132 (e.g., a second portion of the metal powder 132) at a second speed 148 to form one or more intermediate layers 224 and depositing the metal powder 132 (e.g., a third portion of the metal powder 132) at the second speed 148 to form the outer layer 138 (block 1010). In these examples, the first speed 146 is less than the second speed 148.

[0084] In one or more examples, according to the method 1000 , the first speed 146 is below the adhesion level of the metal powder 132 . The second speed 148 is equal to or above the adhesion level of the metal powder 132 .

[0085] In one or more examples, the first speed 146 is at least 5% less than the second speed 148 according to the method 1000. In one or more examples, the first speed 146 is at least 10% less than the second speed 148 according to the method 1000. In one or more examples, the first speed 146 is at least 15% less than the second speed 148 according to the method 1000. In one or more examples, the first speed 146 is at least 20% less than the second speed 148 according to the method 1000. In one or more examples, the first speed 146 is at least 25% less than the second speed 148 according to the method 1000.

[0086] In one or more examples, the method 1000 includes a step of releasing the inner surface 124 of the leading edge structure 102 from the tool surface 122 of the mandrel 118 (block 1012). Releasing the mandrel 118 may be performed without requiring an intermediate release layer or melt layer.

[0087] In one or more examples, the leading edge structure 102 may be subjected to post-fabrication heat treatment based on desired material properties.

[0088] In one or more examples, the method 1000 includes a step of forming the mandrel 118 (block 1014). The mandrel 118 is formed (eg, processed, manufactured, machined, etc.) such that the mandrel 118 is a unitary structure and the tool surface 122 is a continuous surface.

[0089] In one or more examples, according to the method 1000, the mandrel 118 includes a first hardness 140. The metal powder 132 includes a second hardness 142. The first hardness 140 is greater than the second hardness 142.

[0090] In one or more examples, the method 1000 includes a step (box 1016) of repairing the damaged portion 156 of the leading edge structure 102 by depositing a metal powder 132 on the outer surface 126 of the leading edge structure 102 using a cold spray additive manufacturing process to repair the damaged portion 156 and form a repaired portion 158 having at least approximately the same shape as the originally manufactured outer surface 126.

[0091] General Reference Figures 1 to 10 And special reference Fig.12 , which shows an example of a method 2000 for manufacturing an airfoil 104. The following is a list of examples of methods 2000 according to the present disclosure. Some elements, steps, and / or operations described in one example may be combined with other examples in various ways without including other steps described in those other examples, even if one or more such combinations are not explicitly described herein by example.

[0092] In one or more examples, the method 2000 includes the step of manufacturing the composite body 174 of the airfoil 104 (block 2002). The composite body 174 includes the tip 114 and the root 116 opposite the tip 114. The composite body 174 includes the leading edge 108. The leading edge 108 includes a leading edge first portion 128 extending from the root 116 toward the tip 114. The composite body 174 includes a trailing edge 112 opposite the leading edge 108 and extending from the root 116 to the tip 114. The method 2000 includes the step of manufacturing the leading edge structure 102 by using a cold spray additive manufacturing process (block 2004) by depositing niobium powder 134 on a tool surface 122 of a mandrel 118. The method 2000 includes the step of coupling the leading edge structure 102 to the leading edge 108 of the composite body 174 to form a leading edge second portion 130 of the leading edge 108 extending from the leading edge first portion 128 to the tip 114 (block 2006).

[0093] Thus, the example of the system 100 and method 1000 for manufacturing the leading edge structure 102 from the niobium powder 134 using the cold spray process provides many unique advantages over conventional leading edge protectors. As an example, the use of the niobium powder 134, the material hardness and surface characteristics of the mandrel 118, the operating parameters of the cold spray device 120 throughout the cold spray process, or a combination thereof facilitates easier removal of the leading edge structure 102 from the mandrel 118 after the manufacturing is completed. For example, by applying energy (such as thermal energy and / or mechanical energy) to the leading edge structure 102 and / or the mandrel 118, the leading edge structure 102 can be separated and removed from the tool surface 122 of the mandrel 118. As another example, the cold spray process also enables the manufacturing of leading edge structures 102 with complex aerodynamic shapes. As yet another example, the use of the niobium powder 134 in the cold spray process reduces or eliminates the internal stresses and strains that are typically generated in heat-based manufacturing techniques, and does not degrade or change the metallurgical characteristics of the leading edge structure 102 during and after manufacturing. As yet another example, the cold spray process enables the leading edge structure 102 to be manufactured to a near net shape, thereby reducing material input, material waste, and overall manufacturing time. In addition, by manufacturing the leading edge structure 102 from the niobium powder 134 on the mandrel 118 using the cold spray process, the leading edge structure 102 benefits from improved strength properties while still allowing a post-manufacturing heat treatment process to further improve the material properties of the leading edge structure 102.

[0094] In addition, the example of the leading edge structure 102 includes an inner surface 124 that advantageously defines an inner mold line of the leading edge structure 102 produced by manufacturing using the system 100 and / or according to the method 1000. The present disclosure recognizes that the thin release layer required by other cold spray manufacturing techniques is not negligible and introduces significant dimensional offset errors to the machined surface and the resulting part inner mold line surface of the cold spray deposit used for bonding. In addition, the release layer tends to introduce defects such as contamination or intermetallic alloys (e.g., zinc niobium) between the melt release layer and the cold spray deposit, resulting in undesirable mechanical properties, as well as rough surface textures caused by mixing effects caused by bonding requirements. In addition, post-heat treatment of the cold spray deposit is challenged by the presence of low melting point release layer materials or residual contaminants (e.g., inherent in the fusible release layer), which cannot be present in a high temperature vacuum furnace.

[0095] Reference now Fig.13 and Fig.14 Examples of the system 100, method 1000, leading edge structure 102, airfoil 104, and method 2000 described herein may be used in conjunction with Fig.13 Aircraft manufacturing and service method 1100 and the like are shown in a flowchart Fig.14Schematically illustrated is related to or used in the context of an aircraft 1200. As an example, the aircraft 1200 and / or the aircraft production and service method 1100 may include one or more airfoils 104, such as one or more rotor blades 106, propeller blades, fan blades, etc., including a leading edge structure 102 manufactured using the system 100 and / or according to the method 1000.

[0096] Reference Fig.14 , which shows an example of an aircraft 1200. In one or more examples, the aircraft 1200 includes one or more airfoils 104 having a leading edge structure 102. As an example, the aircraft 1200 is a rotorcraft including a plurality of rotor blades 106, an airplane including a plurality of propeller blades, or a jet aircraft including a plurality of fan blades. In general, the aircraft 1200 includes a fuselage 1202 having an interior 1206. The aircraft 1200 includes a plurality of onboard systems 1204 (e.g., advanced systems). Examples of onboard systems 1204 of the aircraft 1200 include a propulsion system 1208. The propulsion system 1208 includes one or more airfoils 104. Other examples of onboard systems 1204 include a hydraulic system 1212, an electrical system 1210, and an environmental system 1214. In other examples, the onboard systems 1204 also include one or more control systems coupled to the fuselage 1202 of the aircraft 1200. In yet another example, the onboard systems 1204 also include one or more other systems, such as, but not limited to, communication systems, avionics systems, software distribution systems, network communication systems, passenger information / entertainment systems, guidance systems, radar systems, weapon systems, and the like.

[0097] Reference Fig.13 During pre-production of the aircraft 1200, the manufacturing and service method 1100 includes specification and design of the aircraft 1200 (block 1102) and material procurement (block 1104). During production of the aircraft 1200, component and subassembly manufacturing (block 1106) and system integration (block 1108) of the aircraft 1200 occurs. Thereafter, the aircraft 1200 is certified and delivered (block 1110) to be placed in service (block 1112). Routine service and maintenance (block 1114) includes modification, reconfiguration, refurbishment, etc., of one or more systems of the aircraft 1200.

[0098] Fig.13 Each process of the manufacturing and maintenance method 1100 shown in the figure can be performed or carried out by a system integrator, a third party and / or an operator (e.g., a customer). For the purpose of this description, a system integrator may include, but is not limited to, any number of spacecraft manufacturers and major system subcontractors; a third party may include, but is not limited to, any number of suppliers, subcontractors, and suppliers; an operator may be an airline, a leasing company, a military entity, a maintenance organization, etc.

[0099] Examples of the system 100 , method 1000 , leading edge structure 102 , airfoil 104 , and method 2000 shown and described herein may be found at Fig.13 The manufacturing and maintenance method 1100 shown in the flowchart shown may be employed during any one or more stages. In one example, the use of the system 100 and / or the manufacturing of the leading edge structure 102 according to the method 1000 and the manufacturing of the airfoil 104 having the leading edge structure 102 according to the method 2000 may form part of component and subassembly manufacturing (block 1106) and / or system integration (block 1108). In addition, the use of the system 100 and / or the manufacturing of the leading edge structure 102 according to the method 1000 and the manufacturing of the airfoil 104 having the leading edge structure 102 according to the method 2000 may be implemented in a manner similar to components or subassemblies prepared when the aircraft 1200 is in service (block 1112). Moreover, the use of the system 100 and / or the manufacturing of the leading edge structure 102 according to the method 1000 and the manufacturing of the airfoil 104 having the leading edge structure 102 according to the method 2000 may be used during system integration (block 1108) and certification and delivery (block 1110). Similarly, the leading edge structure 102 may be manufactured or repaired using the system 100 and / or according to the method 1000 , for example, without limitation, while the aircraft 1200 is in service (block 1112 ) and during maintenance and service (block 1114 ).

[0100] The foregoing detailed description refers to the accompanying drawings, which illustrate specific examples described in the present disclosure. Other examples with different structures and operations do not depart from the scope of the present disclosure. In different drawings, the same reference numerals may refer to the same features, elements or components. Throughout the present disclosure, any one of a plurality of items may be individually referred to as a project, and a plurality of items may be collectively referred to as a project and may be referred to by the same reference numerals. In addition, as used herein, a feature, element, component or step preceded by the word "one" or "an" should be understood as not excluding a plurality of features, elements, components or steps, unless such exclusion is explicitly stated. .

[0101] Illustrative, non-exhaustive examples of the subject matter of the present disclosure are provided above, which may be, but not necessarily, claimed. Reference to "example" herein means that one or more features, structures, elements, parts, characteristics and / or operating steps described in conjunction with the example are included in at least one aspect, embodiment and / or specific implementation of the subject matter of the present disclosure. Therefore, the phrases "an example", "another example", "one or more examples" and similar language throughout the present disclosure may but may not refer to the same example. In addition, the subject matter representing any one example may but may not include the subject matter representing any other example. In addition, the subject matter representing any one example may but may not be combined with the subject matter representing any other example.

[0102] As used herein, a system, device, equipment, structure, article, element, component, or hardware that is "configured to" perform a specified function is indeed capable of performing the specified function without any changes, rather than having the potential to perform the specified function only after further modification. In other words, a system, device, equipment, structure, article, element, component, or hardware that is "configured to" perform a specified function is specifically selected, created, implemented, utilized, programmed, and / or designed for the purpose of performing the specified function. As used herein, "configured to" represents an existing characteristic of a system, device, structure, article, element, component, or hardware that enables the system, device, structure, article, element, component, or hardware to perform the specified function without further modification. For the purposes of this disclosure, a system, device, equipment, structure, article, element, component, or hardware that is described as "configured to" perform a specific function may be additionally or alternatively described as "adapted to" and / or "operable to" perform that function.

[0103] Unless otherwise indicated, the terms "first," "second," "third," etc. are used herein merely as labels, and are not intended to impose order, position, or hierarchy requirements on the items to which these terms refer. Furthermore, reference to, for example, a "second" item does not require or preclude the presence of, for example, a "first" or lower-numbered item and / or, for example, a "third" or higher-numbered item.

[0104] As used herein, the phrase "at least one of" when used with a list of items means that different combinations of one or more of the listed items may be used and only one of each item in the list may be required. For example, "at least one of item A, item B, and item C" may include, but is not limited to, item A or item A and item B. This example may also include item A, item B, and item C, or item B and item C. In other examples, "at least one of" may be, for example, but not limited to, two of item A, one of item B, and ten of item C; four of item B and seven of item C; and other suitable combinations. As used herein, the term "and / or" and the " / " symbol include any and all combinations of one or more of the associated listed items.

[0105] For the purposes of this disclosure, the term "coupled" and similar terms refer to two or more elements that are joined, linked, fastened, attached, connected, placed in communication, or otherwise associated (e.g., mechanically, electrically, fluidically, optically, electromagnetically) with each other. In various examples, the elements may be associated directly or indirectly. As an example, element A may be directly associated with element B. As another example, element A may be indirectly associated with element B, for example, via another element C. It will be understood that not all associations between the various disclosed elements are necessarily represented. Therefore, there may also be couplings other than those depicted in the figures.

[0106] As used herein, the term "about" refers to or indicates a condition that is close to, but not exactly, the condition that still performs the desired function or achieves the desired result. As an example, the term "about" refers to a condition that is within an acceptable predetermined tolerance or accuracy, such as a condition within 10% of the condition. However, the term "about" does not exclude conditions that are exactly the condition. As used herein, the term "substantially" refers to a condition that is substantially the condition that performs the desired function or achieves the desired result.

[0107] The above mentioned Figures 1 to 10 and Fig.14 The above-mentioned structures may be modified, added and / or omitted. In addition, those skilled in the art will understand that the above-mentioned structures are not necessarily implied. Figures 1 to 10 and Fig.14 All elements, features, and / or components described and shown in the present invention need to be included in every example, and not all elements, features, and / or components described herein need to be depicted in every illustrative example. Figures 1 to 10 and Fig.14 Some elements, features and / or components described and shown in the drawings may be combined in various ways without necessarily including Figures 1 to 10 and Fig.14, other drawings and / or the accompanying disclosure, even if one or more such combinations are not explicitly shown herein. Similarly, additional features not limited to the examples presented may be combined with some or all of the features shown and described herein. Unless explicitly stated otherwise, the above-mentioned Figures 1 to 10 and Fig.14 The schematic diagrams of the examples depicted in the are not meant to imply structural limitations with respect to the illustrative examples. On the contrary, although an illustrative structure is indicated, it should be understood that the structure may be modified when appropriate. Therefore, modifications, additions, and / or omissions may be made to the illustrated structure. In addition, Figures 1 to 10 and Fig.14 In each of the embodiments, elements, features and / or components that serve similar or at least substantially similar purposes are labeled with like numerals, and such elements, features and / or components may not be referred to herein. Figures 1 to 10 and Fig.14 Similarly, all elements, features and / or components may not be discussed in detail. Figures 1 to 10 and Fig.14 Each of the is labeled in , but for consistency, the reference numerals associated therewith may be used herein.

[0108] exist Figures 11 to 13 In the above, the frame can represent an operation, a step and / or its part, and the line connecting each frame does not imply any particular order or dependency of the operation or its part. It should be understood that all dependencies between the various disclosed operations are not necessarily represented. Figures 11 to 13 The attached disclosures describing the operations of the disclosed methods set forth herein should not be construed as necessarily determining the order in which the operations must be performed. On the contrary, although an exemplary order is indicated, it should be understood that the order of the operations can be modified when appropriate. Therefore, the operations shown can be modified, added and / or omitted, and some operations can be performed in different orders or simultaneously. In addition, those skilled in the art will appreciate that not all described operations need to be performed.

[0109] In addition, references throughout this specification to features, advantages, or similar language used herein do not mean that all features and advantages that can be implemented using the examples disclosed herein should be or are in any single example. Instead, language referring to features and advantages is understood to mean that a particular feature, advantage, or characteristic described in conjunction with an example is included in at least one example. Therefore, discussions of features, advantages, and similar language used throughout this disclosure may, but do not necessarily, refer to the same example.

[0110] The described features, advantages and characteristics of an example may be combined in one or more other examples in any suitable manner. Those skilled in the relevant art will recognize that the examples described herein may be practiced without one or more specific features or advantages of a particular example. In other cases, additional features and advantages that may not be present in all examples may be recognized in certain examples. In addition, although various examples of the system 100, method 1000, leading edge structure 102, airfoil 104 and method 2000 have been shown and described, modifications may be conceivable to those skilled in the art after reading the specification. The present application includes such modifications and is limited only by the scope of the claims.

Claims

1. A system (100) for manufacturing a leading edge structure (102) of an airfoil (104), the system (100) comprising: a mandrel (118) comprising a tool surface (122); and A cold spray additive manufacturing device (120), wherein the cold spray additive manufacturing device is configured to: depositing a metal powder (132) on the tool surface (122) of the mandrel (118) to form an inner layer (136) of the leading edge structure (102); depositing the metal powder (132) on the inner layer (136) to form a plurality of intermediate layers (224) of the leading edge structure (102); as well as depositing the metal powder (132) on one of the intermediate layers (224) to form an outer layer (138) of the leading edge structure (102), in: The inner layer (136) forms an inner surface (124) of the leading edge structure (102); The outer layer (138) forms an outer surface (126) of the leading edge structure (102) opposite the inner surface (124); The intermediate layer (224) forms the thickness of the leading edge structure (102) between the inner surface (124) and the outer surface (126); and The inner surface (124) of the leading edge structure (102) is configured to be coupled to the airfoil (104) such that the outer surface (126) of the leading edge structure (102) forms a portion of a leading edge (108) and a portion of an aerodynamic surface (152) of the airfoil (104).

2. The system (100) of claim 1, wherein the metal powder (132) comprises niobium powder (134).

3. The system (100) of claim 1, wherein the metal powder (132) comprises a refractory metal powder (150).

4. The system (100) of claim 1, wherein: The cold spray additive manufacturing device (120) is further configured to deposit the metal powder (132) at a first speed (146) to form the inner layer (136) and to deposit the metal powder (132) at a second speed (148) to form one or more of the middle layer (224) and the outer layer (138); and The first speed (146) is less than the second speed (148).

5. The system (100) of claim 4, wherein: The first speed (146) is below an adhesion level of the metal powder (132); and The second speed (148) is higher than the adhesion level of the metal powder (132).

6. The system (100) of claim 4, wherein the first speed (146) is about 5% to about 25% less than the second speed (148).

7. The system (100) of claim 1, wherein: The mandrel (118) is a unitary structure; and The tool surface (122) is a continuous surface.

8. The system (100) of claim 1, wherein: The mandrel (118) includes a first hardness (140); The metal powder (132) comprises a second hardness (142); and The first hardness (140) is greater than the second hardness (142).

9. A method (1000) for manufacturing a leading edge structure (102) of an airfoil (104), the method (1000) comprising: cold spraying a metal powder (132) onto a tool surface (122) of a mandrel (118) to form an inner layer (136) of the leading edge structure (102); cold spraying the metal powder (132) onto the inner layer (136) to form a plurality of intermediate layers (224) of the leading edge structure (102); as well as cold spraying the metal powder (132) onto one of the intermediate layers (224) to form an outer layer (138) of the leading edge structure (102), in: The inner layer (136) forms an inner surface (124) of the leading edge structure (102); The outer layer (138) forms an outer surface (126) of the leading edge structure (102) opposite the inner surface (124); The intermediate layer (224) forms the thickness of the leading edge structure (102) between the inner surface (124) and the outer surface (126); and The inner surface (124) of the leading edge structure (102) is configured to be coupled to the airfoil (104) such that the outer surface (126) of the leading edge structure (102) forms a portion of a leading edge (108) and a portion of an aerodynamic surface (152) of the airfoil (104).

10. The method (1000) of claim 9, wherein the metal powder (132) comprises niobium powder (134).

11. The method (1000) of claim 9, wherein the metal powder (132) consists essentially of niobium powder (134).

12. The method (1000) of claim 9, wherein the metal powder (132) consists of niobium powder (134).

13. The method (1000) of claim 9, wherein the metal powder (132) comprises a refractory metal powder (150).

14. The method (1000) of claim 9, further comprising: depositing the metal powder (132) at a first speed (146) to form the inner layer (136); as well as depositing the metal powder (132) at a second speed (148) to form one or more of the intermediate layer (224) and the outer layer (138), The first speed (146) is less than the second speed (148).

15. The method (1000) of claim 14, wherein: The first speed (146) is below an adhesion level of the metal powder (132); and The second speed (148) is higher than the adhesion level of the metal powder (132).

16. The method (1000) of claim 14, wherein the first speed (146) is about 5% to about 25% less than the second speed (148).

17. The method (1000) of claim 9, further comprising releasing the inner surface (124) of the leading edge structure (102) from the tool surface (122) of the mandrel (118), in: The mandrel (118) is a unitary structure; The tool surface (122) is a continuous surface; The mandrel (118) includes a first hardness (140); The metal powder (132) comprises a second hardness (142); and The first hardness (140) is greater than the second hardness (142).

18. A leading edge structure (102) of an airfoil (104), comprising: an inner surface (124) configured to be coupled to the airfoil (104); and an outer surface (126) opposite the inner surface (124) and configured to form a portion of a leading edge (108) and a portion of an aerodynamic surface (152) of the airfoil (104), The leading edge structure (102) is manufactured by depositing niobium powder (134) on a tool surface (122) of a mandrel (118) using a cold spray additive manufacturing process.

19. The leading edge structure (102) of claim 18, wherein: The leading edge structure (102) is manufactured by: depositing the niobium powder (134) at a first speed (146) to form an inner layer (136) on the tool surface (122) of the mandrel (118); depositing the niobium powder (134) at a second speed (148) to form one or more intermediate layers (224) on the inner layer (136); and depositing the niobium powder (134) at the second speed (148) to form an outer layer (138) on the intermediate layer (224); and The first speed (146) is less than the second speed (148).