Positive electrode material and preparation method thereof, battery and electric device
By using a colloidal solution of thickener and a variety of transition metal ions in the preparation of positive electrode material, a gel-like material is formed and the particle growth rate is controlled, the problem of difficult and poor circulation performance of positive electrode material preparation in the prior art is solved. Significantly improves the cycle performance and life of the battery.
Patent Information
- Application Number
- CN202410989690.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-22
AI Technical Summary
In the prior art, the synthesis process control of the preparation of positive electrode materials is difficult, the circulation performance is poor, and there are microcrack problems in battery applications.
Prepare a first colloidal solution containing a variety of transition metal ions by adding thickener, and then pour the lithium salt solution into a gel-like material to control the particle growth rate to optimize the crystal phase structure of the positive electrode material, reduce microcracks, and improve the battery Cyclic performance.
A better crystal phase structure of the positive electrode material is achieved, microcracks are reduced, and the circulation performance and life of the battery are significantly improved.
Smart Images

Figure CN119018942A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a positive electrode material and a preparation method thereof, a battery and an electrical device. Background Art
[0002] The synthesis process for preparing positive electrode materials in the related art requires too many conditions to be monitored, which makes the control difficult; moreover, the battery using the positive electrode materials prepared by the preparation method in the related art has poor cycle performance. Therefore, there is room for improvement. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, one purpose of the present invention is to provide a method for preparing a positive electrode material, by adding a thickener to prepare a first colloidal solution containing a plurality of transition metal ions, and then pouring a lithium salt solution into the first colloidal solution to form a gel-like material, the viscosity of the solution can be increased, making it easier to control the particle growth rate; and by controlling the particle growth rate, the crystal phase structure of the generated positive electrode material can be good, microcracks can be reduced, and the battery cycle performance is better.
[0004] The present invention also provides a positive electrode material prepared using the preparation method of the positive electrode material.
[0005] The invention also provides a battery having the positive electrode material.
[0006] The invention also provides an electrical device having the battery.
[0007] According to the first aspect of the present invention, the method for preparing a positive electrode material of an embodiment includes: preparing a first colloidal solution, wherein the first colloidal solution contains water, a thickener and transition metal ions, wherein the transition metal ions include first transition metal ions, second transition metal ions and third transition metal ions; preparing a lithium salt solution; pouring the lithium salt solution into the first colloidal solution to form a gel-like material; drying the gel-like material to obtain a precursor; and calcining the precursor to obtain the positive electrode material.
[0008] According to the method for preparing the positive electrode material of an embodiment of the present invention, a thickener is added to prepare a first colloidal solution containing multiple transition metal ions, and then a lithium salt solution is poured into the colloidal solution to form a gel-like material. The viscosity of the solution can be increased, making the particle growth rate easier to control; and by controlling the particle growth rate, the crystal phase structure of the generated positive electrode material can be good, microcracks can be reduced, and the battery cycle performance is better.
[0009] According to some embodiments of the present invention, preparing the first colloidal solution includes: mixing a thickener with water and stirring to form a second colloidal solution; preparing a metal salt solution containing the transition metal ions; mixing the metal salt solution with the second colloidal solution and stirring to form the first colloidal solution.
[0010] According to some embodiments of the present invention, the thickener accounts for 0.05 wt % to 0.15 wt % in the second colloidal solution.
[0011] According to some embodiments of the present invention, the stirring to form a second colloidal solution includes: stirring at a first stirring speed for a first preset time, gradually increasing the stirring speed to a second stirring speed, and stirring at the second stirring speed for a second preset time, the second preset time being greater than the first preset time.
[0012] According to some embodiments of the present invention, the first stirring speed ranges from 180rpm to 220rpm, and the second stirring speed ranges from 500rpm to 700rpm; and / or, the first stirring time ranges from 3min to 8min, and the second stirring time ranges from 45min to 75min.
[0013] According to some embodiments of the present invention, the stirring to form the first colloidal solution includes: stirring at a third stirring speed for a third preset time, the third stirring speed ranges from 500rpm to 700rpm, and the third preset time ranges from 3min to 8min.
[0014] According to some embodiments of the present invention, preparing a metal salt solution containing the transition metal ions includes: weighing a soluble salt of a first transition metal, a soluble salt of a first transition metal, and a soluble salt of a first transition metal according to a stoichiometric ratio and dissolving them in water to form the metal salt solution.
[0015] According to some embodiments of the present invention, the soluble salt of the first transition metal includes at least one of nickel sulfate, nickel acetate, nickel nitrate and nickel chloride, the soluble salt of the second transition metal includes at least one of cobalt sulfate, cobalt acetate, cobalt nitrate and cobalt chloride, and the soluble salt of the third transition metal includes at least one of manganese sulfate, manganese acetate, manganese nitrate and manganese chloride.
[0016] According to some embodiments of the present invention, the concentration of the metal salt solution ranges from 1 mol / L to 2 mol / L.
[0017] According to some embodiments of the present invention, drying the gel-like material includes: drying at a set drying temperature, wherein the set drying temperature ranges from 70°C to 90°C.
[0018] According to some embodiments of the present invention, calcining the precursor includes: sintering at a first calcination temperature for a first calcination time in an oxygen atmosphere, then heating to a second calcination temperature, and sintering at the second calcination temperature for a second calcination time, wherein the second calcination time is greater than the first calcination time.
[0019] According to some embodiments of the present invention, the first calcination temperature ranges from 400°C to 500°C, and the second calcination temperature ranges from 800°C to 900°C; and / or, the first calcination time ranges from 4h to 6h, and the second calcination time ranges from 10h to 14h.
[0020] According to some embodiments of the present invention, preparing the lithium salt solution includes: dissolving a lithium salt in water to form the lithium salt solution; wherein the lithium salt includes at least one of lithium hydroxide, lithium carbonate, lithium chloride, lithium nitrate, lithium acetate and lithium oxalate.
[0021] According to some embodiments of the present invention, the thickener includes at least one of carboxymethyl cellulose, alginic acid, konjac glucomannan, xanthan gum, carrageenan, locust bean gum and guar gum; and / or the first transition metal ion is nickel ion, the second transition metal ion is cobalt ion, and the third transition metal ion is manganese ion or aluminum ion.
[0022] According to the positive electrode material of the second embodiment of the present invention, the positive electrode material is prepared by the preparation method of the first embodiment of the present invention, the positive electrode material is a single crystal structure and the chemical formula of the positive electrode material is LiNi x Co y Mn z O2, where 0 <x<1,0<y<1,0<z<1,x+y+z=1。
[0023] The positive electrode material according to the embodiment of the present invention is prepared by using the preparation method according to the first aspect of the embodiment of the present invention. During the preparation, a thickener is added to prepare a first colloidal solution containing multiple transition metal ions, and then a lithium salt solution is poured into the colloidal solution to form a gel-like material, so that the lithium-nickel mixing rate of the positive electrode material is low, microcracks can be reduced, and the produced positive electrode material has better cycle performance.
[0024] The battery according to the embodiment of the third aspect of the present invention is characterized in that it includes: a battery shell; an electrode group, which is arranged in the battery shell and includes stacked positive and negative electrode sheets, the positive electrode sheet includes a positive electrode collector and a positive electrode active material layer coated on the positive electrode collector, and the positive electrode active material layer includes the positive electrode material according to the embodiment of the second aspect of the present invention.
[0025] The battery according to the embodiment of the present invention includes the positive electrode material according to the embodiment of the second aspect of the present invention. The positive electrode material has a good crystal phase structure, can reduce microcracks, and has better cycle performance of the lithium battery.
[0026] The electrical device according to the fourth embodiment of the present invention is characterized by comprising: a battery according to the third embodiment of the present invention.
[0027] The electric device according to the embodiment of the present invention comprises the battery according to the embodiment of the third aspect of the present invention, so the battery has better cycle performance and longer life.
[0028] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0030] Figure 1 1 are XRD patterns of positive electrode materials prepared by the preparation methods of some embodiments of the present invention: (a) is the full XRD spectrum of Embodiment 1, Embodiment 2 and Embodiment 3, (b) is the (006) / (102) diffraction peak regional spectrum of Embodiment 1, Embodiment 2 and Embodiment 3, (c) is the (018) / (110) diffraction peak regional spectrum of Embodiment 1, Embodiment 2 and Embodiment 3, (d), (e) and (f) are the XRD refined spectra of Embodiment 1, Embodiment 2 and Embodiment 3 respectively;
[0031] Figure 2 are SEM images of positive electrode materials prepared according to the preparation methods of some embodiments of the present invention, wherein (a) and (d) are from Embodiment 1, (b) and (e) are from Embodiment 2, and (c) and (f) are from Embodiment 3;
[0032] Figure 3 is an XPS spectrum of an X-ray photoelectron spectroscopy (XPS) test of the positive electrode material of Example 2;
[0033] Figure 4 The results of characterizing the cathode material of Example 2 using TEM, selected area electron diffraction (SEAD) and EDS Mapping, wherein (a) is a TEM image, (b) is a TEM magnified image, (c) is an FFT image, (d) and (e) are IFFT images, (f) is a Mapping image, and (g) is a selected area electron diffraction image;
[0034] Figure 5The cross-sectional SEM images of the button-type batteries in Example 2 and Comparative Example 1 after 200 cycles, wherein (a) and (b) are from Example 2, and (c) and (d) are from Comparative Example 1;
[0035] Figure 6 The electrochemical performance diagram of the positive electrode material prepared according to the preparation method of some embodiments of the present invention and the positive electrode material prepared in the related technology. DETAILED DESCRIPTION
[0036] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0037] The following describes a method for preparing a positive electrode material according to an embodiment of the present invention.
[0038] A method for preparing a positive electrode material according to a first embodiment of the present invention comprises:
[0039] A first colloidal solution is prepared, the first colloidal solution comprising water, a thickener and transition metal ions. By adding the thickener to the first colloidal solution, the first colloidal solution can be made colloidal and have increased viscosity, thereby making it easier to control the growth rate of the crystal particles.
[0040] For example, the prepared positive electrode material is a ternary positive electrode material, and the transition metal ions include three transition metal ions.
[0041] The transition metal ions include a first transition metal ion, a second transition metal ion, and a third transition metal ion. For example, the first transition metal ion may be a nickel ion, the second transition metal ion may be a cobalt ion, and the third transition metal ion may be a manganese ion. For another example, the first transition metal ion may be a nickel ion, the second transition metal ion may be a cobalt ion, and the third transition metal ion may be an aluminum ion. By mixing a plurality of transition metal ions first, the transition ions can be dispersed more fully and evenly.
[0042] Prepare a lithium salt solution, for example, the lithium salt may be lithium hydroxide, lithium carbonate, etc.;
[0043] The lithium salt solution is poured into the first colloidal solution to form a gel-like material.
[0044] The gel-like material is dried to obtain a precursor.
[0045] The precursor is calcined to obtain the positive electrode material.
[0046] According to the method for preparing the positive electrode material of an embodiment of the present invention, a thickener is added to prepare a first colloidal solution containing multiple transition metal ions, and then a lithium salt solution is poured into the colloidal solution to form a gel-like material. The viscosity of the solution can be increased, making the particle growth rate easier to control; and by controlling the particle growth rate, the crystal phase structure of the generated positive electrode material can be good, microcracks can be reduced, and the battery cycle performance is better.
[0047] According to some embodiments of the present invention, preparing a first colloidal solution includes:
[0048] mixing a thickener with water and stirring to form a second colloidal solution;
[0049] By mixing the thickener with water to prepare the second colloidal solution, the viscosity of the second colloidal solution can be increased, thereby increasing the viscosity of the first colloidal solution subsequently prepared using the second colloidal solution, making the growth rate of the particles easier to control;
[0050] A metal salt solution containing transition metal ions is prepared, wherein the metal salt solution includes a first transition metal ion, a second transition metal ion, and a third transition metal ion.
[0051] The metal salt solution is mixed with the second colloidal solution and stirred to form a first colloidal solution.
[0052] According to some embodiments of the present invention, the mass proportion of the thickener in the second colloidal solution is 0.05wt% to 0.15wt%. For example, the mass proportion of the thickener in the second colloidal solution can be 0.05wt%, 0.07wt%, 0.10wt%, 0.12wt%, 0.15wt%, etc. By making the proportion of the thickener in the second colloidal solution not less than 0.05wt%, the concentration of the thickener will not be too small, so that the thickener can achieve the effect of increasing viscosity; by making the proportion of the thickener in the second colloidal solution not more than 0.15wt%, the concentration of the thickener will not be too high, so as to avoid the solution being too viscous and reducing the yield.
[0053] According to some embodiments of the present invention, stirring to form a second colloidal solution includes: stirring at a first stirring speed for a first preset time, gradually increasing the stirring speed to a second stirring speed, and stirring at the second stirring speed for a second preset time, wherein the second preset time is greater than the first preset time. The thickener is difficult to dissolve in water. By first stirring at the first stirring speed for a first preset time, wherein the first stirring speed is less than the second stirring speed, and the second preset time is greater than the first preset time, the thickener can be fully dissolved first; by subsequently increasing the stirring speed and stirring at the second stirring speed for a second preset time, the thickener can be fully dispersed and the efficiency of making the second colloidal solution can be improved.
[0054] According to some embodiments of the present invention, the first stirring speed ranges from 180rpm to 220rpm, and the second stirring speed ranges from 500rpm to 700rpm. For example, the first stirring speed may be 180rpm, 190rpm, 200rpm, 210rpm, 220rpm, etc., and the second stirring speed may be 500rpm, 550rpm, 600rpm, 650rpm, 700rpm, etc. By making the first stirring speed not less than 180rpm, the thickener can be fully dissolved in water and the dissolution rate of the thickener can be accelerated; by making the first stirring speed not higher than 220rpm, the difficulty of stirring caused by the low initial solubility of the thickener can be avoided. By making the second stirring speed not less than 500rpm, the thickener can be fully dissolved and dispersed in water to form a uniform and stable second colloidal solution; by making the second stirring speed not higher than 700rpm, the performance can be saved while ensuring that the thickener can be fully dispersed.
[0055] According to some embodiments of the present invention, the first stirring time ranges from 3 min to 8 min, and the second stirring time ranges from 45 min to 75 min. For example, the first stirring time may be 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, etc., and the second stirring time may be 45 min, 55 min, 65 min, 75 min, etc. By making the first stirring time shorter than the second stirring time, the thickener can be fully dissolved and then fully and efficiently dispersed.
[0056] According to some embodiments of the present invention, stirring to form a first colloidal solution includes: stirring at a third stirring speed for a third preset time, the third stirring speed ranges from 500rpm to 700rpm, and the third preset time ranges from 3min to 8min. For example, the third stirring speed may be 500rpm, 550rpm, 600rpm, 650rpm, 700rpm, etc., and the third preset time may be 3min, 4min, 5min, 6min, 7min, 8min, etc. By making the third stirring speed not less than 500rpm, lithium ions can be fully diffused in the colloidal solution, and lithium ions can be evenly dispersed in the transition metal; by making the third stirring speed not higher than 700rpm, performance can be saved while ensuring that lithium ions can be fully dispersed.
[0057] According to some embodiments of the present invention, preparing a metal salt solution containing transition metal ions includes: weighing a soluble salt of a first transition metal, a soluble salt of a second transition metal, and a soluble salt of a third transition metal according to a stoichiometric ratio of the transition metal ions and dissolving them in water to form a metal salt solution. By preparing soluble salt solutions of multiple transition metals, the multiple transition metals can be fully and evenly mixed with each other.
[0058] According to some embodiments of the present invention, the soluble salt of the first transition metal includes at least one of nickel sulfate, nickel acetate, nickel nitrate and nickel chloride, the soluble salt of the second transition metal includes at least one of cobalt sulfate, cobalt acetate, cobalt nitrate and cobalt chloride, and the soluble salt of the third transition metal includes at least one of manganese sulfate, manganese acetate, manganese nitrate and manganese chloride. By making the salts of the first transition metal, the second transition metal and the third transition metal all soluble salts, the first transition metal, the second transition metal and the third transition metal can be more easily dispersed and mixed with each other in water.
[0059] Optionally, the soluble salt of the first transition metal is nickel nitrate, the soluble salt of the second transition metal is cobalt nitrate, and the soluble salt of the third transition metal is manganese nitrate.
[0060] According to some embodiments of the present invention, the concentration of the metal salt solution ranges from 1 mol / L to 2 mol / L. For example, the concentration of the metal salt solution may be 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, 2 mol / L, etc. By making the concentration of the metal salt solution not less than 1 mol / L, it is possible to ensure that there are sufficient metal salt ions in the solution and reduce the drying and sintering time; by making the concentration of the metal salt solution not greater than 2 mol / L, it is possible to avoid excessive concentration of metal salt ions and excessively fast crystallization speed, which is difficult to control.
[0061] According to some embodiments of the present invention, drying the gel material includes: drying at a set drying temperature, wherein the set drying temperature ranges from 70°C to 90°C. For example, the drying temperature may be 70°C, 75°C, 80°C, 85°C, 90°C, etc. The drying process may remove moisture from the gel material and may also reduce the time and condition restrictions for calcination. By setting the drying temperature at 70°C to 90°C, it may be ensured that the moisture in the gel material is fully evaporated.
[0062] Optionally, the equipment used for drying is an air blast drying oven. By using an air blast drying oven to dry the gel-like material, moisture in the material can be removed more efficiently and quickly.
[0063] According to some embodiments of the present invention, calcining the precursor includes: sintering at a first calcination temperature for a first calcination time in an oxygen atmosphere, then heating to a second calcination temperature, and sintering at the second calcination temperature for a second calcination time, wherein the second calcination time is longer than the first calcination time. By making the second calcination time longer than the first calcination time, the precursor can be calcined more fully.
[0064] According to some embodiments of the present invention, the first calcination temperature ranges from 400° C. to 500° C., and the second calcination temperature ranges from 800° C. to 900° C. By pre-calcining the precursor and then calcining it at a high temperature, the precursor can be calcined sufficiently, so that the precursor can be converted from a gel form to a solid state to facilitate the preparation of a positive electrode material.
[0065] According to some embodiments of the present invention, the first calcination time ranges from 4 hours to 6 hours, and the second calcination time ranges from 10 hours to 14 hours. By making the second calcination time not less than 10 hours, the precursor can be fully calcined; by making the second calcination time not more than 14 hours, it is possible to avoid wasting time and improve production efficiency while ensuring that the precursor is fully calcined.
[0066] According to some embodiments of the present invention, preparing a lithium salt solution includes: dissolving a lithium salt in water to form a lithium salt solution; wherein the lithium salt includes at least one of lithium hydroxide, lithium carbonate, lithium chloride, lithium nitrate, lithium acetate, and lithium oxalate. For example, the lithium salt includes lithium hydroxide. For another example, the lithium salt includes lithium hydroxide and lithium carbonate.
[0067] According to some embodiments of the present invention, the thickener includes at least one of carboxymethyl cellulose, alginic acid, konjac glucomannan, xanthan gum, carrageenan, locust bean gum and guar gum. For example, the thickener includes konjac glucomannan; for another example, the thickener includes carboxymethyl cellulose; for another example, the thickener includes carboxymethyl cellulose and alginic acid.
[0068] According to some embodiments of the present invention, the first transition metal ion is a nickel ion, the second transition metal ion is a cobalt ion, and the third transition metal ion is a manganese ion or an aluminum ion. When the first transition metal ion is a nickel ion, by controlling the growth rate of the particles, the generated positive electrode material can have a good crystal phase structure, a low lithium-nickel mixing rate, can reduce microcracks, and have better battery cycle performance.
[0069] For example, when the first transition metal ion is nickel ion, the second transition metal ion is cobalt ion, and the third transition metal ion is aluminum ion, the second calcination temperature is greater than 850° C. When the third transition metal ion is aluminum ion, a higher calcination temperature is required to fully calcine the precursor.
[0070] The positive electrode material according to the embodiment of the second aspect of the present invention is characterized in that the positive electrode material is prepared by the preparation method according to the embodiment of the first aspect of the present invention, the positive electrode material has a single crystal structure and the chemical formula of the positive electrode material is LiNi x Co y Mn z O2, where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1. For example, the chemical formula of the positive electrode material may be LiNi 0.8 Co 0.1 Mn 0.1 O2
[0071] The positive electrode material according to the embodiment of the present invention is prepared by using the preparation method according to the embodiment of the first aspect of the present invention. During production, a thickener is added to prepare a first colloidal solution containing a variety of transition metal ions, and then a lithium salt solution is poured into the colloidal solution to form a gel-like material, so that the lithium-nickel mixing rate of the positive electrode material is low, microcracks can be reduced, and the produced positive electrode material has better cycling performance.
[0072] The battery according to the embodiment of the third aspect of the present invention is characterized in that it includes: a battery case and an electrode assembly. The electrode assembly is disposed in the battery case and the electrode assembly includes stacked positive electrode sheets and negative electrode sheets. The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on the positive electrode current collector, and the positive electrode active material layer includes the positive electrode material according to the embodiment of the second aspect of the present invention.
[0073] The battery according to the embodiment of the present invention, by including the positive electrode material according to the embodiment of the second aspect of the present invention, has a good crystal phase structure of the positive electrode material, can reduce microcracks, and the battery has better cycling performance.
[0074] For example, the battery is a lithium battery. By including the positive electrode material according to the embodiment of the second aspect of the present invention, the positive electrode material has a good crystal phase structure and a low lithium-nickel mixing rate, can reduce microcracks, and the battery has better cycling performance.
[0075] The electrical device according to the embodiment of the fourth aspect of the present invention is characterized in that it includes: the battery according to the embodiment of the third aspect of the present invention.
[0076] The electrical device according to the embodiment of the present invention, by including the battery according to the embodiment of the third aspect of the present invention, the battery has better cycling performance and longer life.
[0077] The positive electrode material of the embodiment of the present invention will be further described below in conjunction with some embodiments and comparative examples.
[0078] I. Preparation of materials.
[0079] (1), Preparation of nickel-cobalt-manganese positive electrode materials for each embodiment and comparative example.
[0080] Prepare nickel-cobalt-manganese positive electrode materials. The nickel-cobalt-manganese positive electrode materials of the following embodiments are prepared by the preparation method according to the embodiment of the first aspect of the present invention, and the nickel-cobalt-manganese positive electrode materials of the comparative example are prepared by the coprecipitation method in the related art.
[0081] Example 1: Dissolve carboxymethyl cellulose in 400 mL of deionized water at a ratio of 0.1 wt%, stir at 200 rpm for 5 min, then gradually increase the speed to 600 rpm and stir for 1 h to form a colorless colloidal solution. Weigh 8.72 g Ni(NO3)2·6H2O, 1.09 g Co(NO3)2·6H2O and 1.88 g Mn(NO3)2·4H2O and add them to 30 mL of deionized water, stir at 500 rpm, and after all dissolved, add them to the colorless colloidal solution and stir at 600 rpm for 5 min to form a uniform colloidal solution. According to TM:Li + =1:1.05 ratio, weigh LiOH·H2O and dissolve it in 30mL deionized water, gradually pour it into the colloidal solution, and after precipitation occurs, transfer it to an 80℃ forced air drying oven for drying. The precursor is first calcined at 450℃ in oxygen for 5h, then calcined at 850℃ for 12h, and ground to obtain the nickel-cobalt-manganese positive electrode material.
[0082] Example 2: Dissolve alginic acid in 400 mL of deionized water at a ratio of 0.1 wt%, stir at 200 rpm for 5 min, then gradually increase the speed to 600 rpm and stir for 1 h to form a colorless colloidal solution. Weigh 8.72 g Ni(NO3)2·6H2O, 1.09 g Co(NO3)2·6H2O and 1.88 g Mn(NO3)2·4H2O and add them to 30 mL of deionized water, stir at 500 rpm, and after all dissolved, add them to the colorless colloidal solution and stir at 600 rpm for 5 min to form a uniform colloidal solution. According to TM:Li + =1:1.05 ratio, weigh LiOH·H2O and dissolve it in 30mL deionized water, gradually pour it into the colloidal solution, and after precipitation occurs, transfer it to an 80℃ forced air drying oven for drying. The precursor is first calcined at 450℃ in oxygen for 5h, then calcined at 850℃ for 12h, and ground to obtain the nickel-cobalt-manganese positive electrode material.
[0083] Example 3: Dissolve konjac glucomannan in 400 mL of deionized water at a ratio of 0.1 wt%, stir at 200 rpm for 5 min, then gradually increase the speed to 600 rpm and stir for 1 h to form a colorless colloidal solution. Weigh 8.72 g Ni(NO3)2·6H2O, 1.09 g Co(NO3)2·6H2O and 1.88 g Mn(NO3)2·4H2O and add them to 30 mL of deionized water, stir at 500 rpm, and after all dissolved, add them to the colorless colloidal solution and stir at 600 rpm for 5 min to form a uniform colloidal solution. According to TM:Li+ =1:1.05 ratio, weigh LiOH·H2O and dissolve it in 30mL deionized water, gradually pour it into the colloidal solution, and after precipitation occurs, transfer it to an 80℃ forced air drying oven for drying. The precursor is first calcined at 450℃ in oxygen for 5h, then calcined at 850℃ for 12h, and ground to obtain the nickel-cobalt-manganese positive electrode material.
[0084] Comparative Example 1: Selecting polycrystalline precursor material Ni 0.8 Mn 0.1 Co 0.1 (OH)2 was used as the nickel-cobalt-manganese ternary precursor. 5g of commercial polycrystalline precursor and 2.386g of LiOH·H2O were weighed and ground according to the ratio of TM:Li+=1:1.05, and calcined at 450℃ for 5h in oxygen, and then calcined at 850℃ for 12h to obtain the nickel-cobalt-manganese positive electrode material.
[0085] (2) Preparation of positive electrode sheets of various embodiments and comparative examples.
[0086] The nickel-cobalt-manganese positive electrode material, conductive carbon black (Super-P) and a binder polyvinylidene fluoride (PVDF) containing N-methyl-2-pyrrolidone (NMP) prepared above were mixed in a mass ratio of 8:1:1, stirred for 0.5 h using a magnetic stirrer to obtain a positive electrode slurry, and the positive electrode slurry was evenly coated on one side of a clean aluminum foil surface, dried, and cut into pieces to obtain a positive electrode sheet for testing.
[0087] (3) Preparation of button-type half-cells of various embodiments and comparative examples.
[0088] In a glove box with moisture and oxygen below 10 ppm and filled with argon, the obtained positive electrode sheet was used, a lithium sheet was used as the negative electrode, 1 mol / L LiPF6 (solvent is EC:DMC:EMC=1:1:1) electrolyte was added, and a polypropylene separator with a thickness of 20 μm was used to assemble a CR2032 button battery.
[0089] 2. Related tests
[0090] (1) XRD test was performed on the positive electrode materials prepared in Example 1, Example 2 and Example 3.
[0091] Reference Figure 1 , Figure 1 The XRD patterns obtained by XRD testing the positive electrode materials prepared in Example 1, Example 2 and Example 3. Figure 1In the figure, (a) is the full XRD spectrum of Example 1, Example 2 and Example 3, (b) is the (006) / (102) diffraction peak regional spectrum of Example 1, Example 2 and Example 3, (c) is the (018) / (110) diffraction peak regional spectrum of Example 1, Example 2 and Example 3, (d), (e) and (f) are the XRD refined spectra of Example 1, Example 2 and Example 3, respectively.
[0092] from Figure 1 It can be seen from (a) that the characteristic peaks of the positive electrode materials of Examples 1, 2 and 3 are all α-NaFeO2 structures of the R-3m space group. Figure 1 (b) and Figure 1 In (c), it can be seen that the (006) / (102) and (018) / (110) peaks of the positive electrode materials of Examples 1, 2 and 3 are clearly split, indicating that a good layered structure is formed. The c / a ratios of the positive electrode materials of Examples 1, 2 and 3 are all greater than 4.92, indicating that the positive electrode materials of Examples 1, 2 and 3 have formed an excellent hexagonal structure.
[0093] The XRD spectra of the positive electrode materials of Example 1, Example 2 and Example 3 were refined using Fullprof software, and the unit cell parameters of the positive electrode materials of Example 1, Example 2 and Example 3 were obtained as shown in Table 1.
[0094] Table 1
[0095]
[0096] It can be seen from Table 1 that the ratio of I(003) / I(104) of Example 1 and Example 3 is slightly less than 1.2, so their Li+ / Ni 2+ The mixing ratio is higher, 5.6% and 6.6%. The ratio of I(003) / I(104) in Example 2 is greater than 1.2, and its Li+ / Ni 2+ The degree of mixing is relatively low, at only 3.6%.
[0097] (2) Electron microscope scanning was performed on the positive electrode materials prepared in Example 1, Example 2 and Example 3 respectively to obtain SEM images of the positive electrode materials prepared in Example 1, Example 2 and Example 3.
[0098] Reference Figure 2 , Figure 2 is a SEM image of the positive electrode materials prepared in Example 1, Example 2 and Example 3, wherein Figure 2 In the embodiment, (a) and (d) are embodiment 1, (b) and (e) are embodiment 2, and (c) and (f) are embodiment 3.
[0099] Reference Figure 2 , Figure 2 The positive electrode material LiNi 0.8 Co 0.1 Mn 0.1 SEM image of O2. Figure 2 It can be seen that the primary particle size of Example 1 and Example 3 is about 1-3 μm, most of them are irregular in shape, and a small amount of materials have obvious edges and corners. The primary particle size of Example 2 is about 0.5-2 μm, which is more uniform than the other two materials, and they are also irregular in shape, but their morphology is more rounded.
[0100] (3) The XPS spectrum of the positive electrode material of Example 2 obtained by X-ray photoelectron spectroscopy (XPS) testing.
[0101] Reference Figure 3 , Figure 3 The XPS spectrum of the positive electrode material of Example 2 is shown.
[0102] from Figure 3 It can be seen that the binding energy peaks of Ni 2p3 / 2 and Ni 2p1 / 2 are 855.17eV and 872.78eV respectively, and the two satellite peaks are 861.08eV and 879.38eV respectively. The higher the binding energy of the Ni 2p3 / 2 peak, the higher the average valence of the Ni ion. The binding energy peaks of Co 2p3 / 2 and Co 2p1 / 2 are 780.88eV and 795.58eV respectively. The binding energy peaks of Mn 2p3 / 2 and Mn 2p1 / 2 are 642.38eV and 654.08eV respectively. The XPS data of the material using Avantage software were further separated and fitted. The main peak at 855.38eV belongs to Ni 2+ , the main peak at 856.68 eV belongs to Ni 3+ , where Ni 2+ The ratio is 65.15%, Ni 3+ The ratio is 34.85%.
[0103] (4) The cathode material of Example 2 was characterized by TEM, selected area electron diffraction (SEAD) and EDS Mapping.
[0104] Reference Figure 4 , Figure 4 The characterization results of Example 2 using TEM, selected area electron diffraction (SEAD) and EDS Mapping are shown, wherein Figure 4 (a) is the TEM image, (b) is the TEM magnified image, (c) is the FFT image, (d) and (e) are the IFFT images, (f) is the Mapping image, and (g) is the selected area electron diffraction image.
[0105] from Figure 4 (a) and Figure 4 In (b), it can be seen that the lattice spacing of the sample is 0.4774nm, corresponding to the (003) crystal plane. Figure 4 In the TEM magnified image (b), the darker layer is the lithium layer, the brighter layer is the transition metal layer, and in the yellow frame, some gray spots can be seen in the darker lithium layer, indicating that there are transition metal atoms in the lithium layer and lithium-nickel mixed arrangement in the material. EDS spectrum of the material Figure 4 (f) shows that Ni, Co, Mn and O elements are uniformly distributed throughout the primary particles. Figure 4 The diffraction pattern in the SAED image of (g) is a hexagonal lattice, indicating that the material is a single crystal material. After calibration, the structure of the material is a hexagonal layered structure.
[0106] (5) After the button-type batteries in Example 2 and Comparative Example 1 were cycled for 200 cycles, cross-sectional SEM images were obtained.
[0107] Reference Figure 5 , Figure 5 The cross-sectional SEM images of the button-type batteries in Example 2 and Comparative Example 1 after 200 cycles are shown. From Figure 5, it can be seen that the button-type battery in Example 2 can maintain the initial structure after 200 cycles without obvious intracrystalline microcracks, while the button-type battery in Comparative Example 1 has obvious microcracks in the center of the secondary particles along the grain boundaries.
[0108] (6) The button cells in Example 1, Example 2, Example 3 and Comparative Example 1 were subjected to electrochemical performance tests, and the electrochemical performance tests included:
[0109] The cycle performance test was carried out by charging to 4.5V at a constant current of 1.0C and then discharging to 2.5V at a constant current for 200 cycles at room temperature to obtain the room temperature cycle performance data.
[0110] Reference Figure 6 , Figure 6 The electrochemical performance graphs obtained by electrochemical performance testing of the button-type batteries in Example 1, Example 2, Example 3 and Comparative Example 1 are shown, and the cycle performance test results of the button-type batteries in Example 1, Example 2, Example 3 and Comparative Example 1 are shown.
[0111] In order to highlight the difference in cycle performance among Example 1, Example 2, Example 3 and Comparative Example 1, the voltage window is increased from the conventional 3 to 4.2 V to 2.5 to 4.5 V to accelerate the attenuation of the material during the cycle process.
[0112] from Figure 6It can be seen that the capacities of the four materials (i.e., the positive electrode materials involved in Example 1, Example 2, Example 3 and Comparative Example 1) at a rate of 1C are 159.39 mAh / g, 176.98 mAh / g, 159.94 mAh / g and 183.48 mAh / g, and the discharge specific capacity of Comparative Example 1 is still the highest. The discharge specific capacity of Example 2 is higher than that of Example 1 and Example 3.
[0113] After 200 cycles, the discharge specific capacities of the four materials were 98.18 mAh / g, 101.09 mAh / g, 97.94 mAh / g and 31.87 mAh / g, respectively, and the capacity retention rates were 61.60%, 57.12%, 61.24% and 17.37%, respectively.
[0114] The cycle retention rates of Example 1, Example 2, and Example 3 are all much higher than those of Comparative Example 1.
[0115] In the description of the present invention, "first feature" or "second feature" may include one or more of the features.
[0116] In the description of the present invention, "plurality" means two or more.
[0117] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0118] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A method for preparing a positive electrode material, characterized in that: include: preparing a first colloidal solution, wherein the first colloidal solution comprises water, a thickener, and transition metal ions, wherein the transition metal ions comprise first transition metal ions, second transition metal ions, and third transition metal ions; preparing a lithium salt solution; Pouring the lithium salt solution into the first colloidal solution to form a gel-like material; Drying the gel-like material to obtain a precursor; The precursor is calcined to obtain the positive electrode material.
2. The method for preparing the positive electrode material according to claim 1, characterized in that: The first colloidal solution is prepared, comprising: mixing a thickener with water and stirring to form a second colloidal solution; preparing a metal salt solution containing the transition metal ion; The metal salt solution and the second colloidal solution are mixed and stirred to form the first colloidal solution.
3. The method for preparing the positive electrode material according to claim 2, characterized in that: The thickener accounts for 0.05 wt % to 0.15 wt % in the second colloidal solution.
4. The method for preparing the positive electrode material according to claim 2, characterized in that: The stirring to form a second colloidal solution comprises: After stirring at a first stirring speed for a first preset time, the stirring speed is gradually increased to a second stirring speed, and stirring is performed at the second stirring speed for a second preset time, wherein the second preset time is greater than the first preset time.
5. The method for preparing the positive electrode material according to claim 4, characterized in that: The first stirring speed ranges from 180 rpm to 220 rpm, and the second stirring speed ranges from 500 rpm to 700 rpm; and / or, the first stirring time ranges from 3 min to 8 min, and the second stirring time ranges from 45 min to 75 min.
6. The method for preparing the positive electrode material according to claim 2, characterized in that: The stirring to form the first colloidal solution comprises: Stirring at a third stirring speed for a third preset time, wherein the third stirring speed ranges from 500 rpm to 700 rpm, and the third preset time ranges from 3 min to 8 min.
7. The method for preparing the positive electrode material according to claim 2, characterized in that: The method comprises preparing a metal salt solution containing the transition metal ion, comprising: The transition metal ions are weighed according to a stoichiometric ratio, and the soluble salt of the first transition metal, the soluble salt of the second transition metal and the soluble salt of the first transition metal are dissolved in water to form the metal salt solution.
8. The method for preparing the positive electrode material according to claim 7, characterized in that: The soluble salt of the first transition metal includes at least one of nickel sulfate, nickel acetate, nickel nitrate and nickel chloride, the soluble salt of the second transition metal includes at least one of cobalt sulfate, cobalt acetate, cobalt nitrate and cobalt chloride, and the soluble salt of the third transition metal includes at least one of manganese sulfate, manganese acetate, manganese nitrate and manganese chloride.
9. The method for preparing the positive electrode material according to claim 7, characterized in that: The concentration range of the metal salt solution is 1 mol / L to 2 mol / L.
10. The method for preparing the positive electrode material according to claim 1, characterized in that: The gel-like material is dried, comprising: The drying is performed at a set drying temperature, wherein the set drying temperature ranges from 70°C to 90°C.
11. The method for preparing the positive electrode material according to claim 1, characterized in that: Calcining the precursor comprises: The first calcination time is sintered at a first calcination temperature in an oxygen atmosphere, and then the temperature is increased to a second calcination temperature, and sintered at the second calcination temperature for a second calcination time, wherein the second calcination time is longer than the first calcination time.
12. The method for preparing the positive electrode material according to claim 11, characterized in that: The first calcination temperature ranges from 400°C to 500°C, and the second calcination temperature ranges from 800°C to 900°C; and / or the first calcination time ranges from 4h to 6h, and the second calcination time ranges from 10h to 14h.
13. The method for preparing the positive electrode material according to claim 1, characterized in that: The method for preparing the lithium salt solution comprises: dissolving a lithium salt in water to form the lithium salt solution; Wherein, the lithium salt includes at least one of lithium hydroxide, lithium carbonate, lithium chloride, lithium nitrate, lithium acetate and lithium oxalate.
14. The method for preparing a positive electrode material according to claim 1, characterized in that: The thickener comprises at least one of carboxymethyl cellulose, alginic acid, konjac glucomannan, xanthan gum, carrageenan, locust bean gum and guar gum; and / or the first transition metal ion is nickel ion, the second transition metal ion is cobalt ion, and the third transition metal ion is manganese ion or aluminum ion.
15. A positive electrode material, characterized in that: The positive electrode material is prepared by the preparation method according to any one of claims 1 to 14, the positive electrode material is a single crystal structure and the chemical formula of the positive electrode material is LiNi x Co y Mn z O2, where 0 <x<1,0<y<1,0<z<1,x+y+z=1。 16. A battery, characterized in that: include: Battery housing; An electrode group is arranged in the battery casing and includes a stacked positive electrode sheet and a negative electrode sheet, the positive electrode sheet includes a positive electrode collector and a positive electrode active material layer coated on the positive electrode collector, and the positive electrode active material layer includes the positive electrode material according to claim 15.
17. An electrical device, characterized in that: include: A battery according to claim 16.
Citation Information
Patent Citations
Method for preparing lithium-rich manganese-based cathode material for lithium ion battery
CN102881887A
Preparation method of lithium battery cathode material solid solution micropowder
CN103985855A
Lithium-rich manganese-based lithium-ion battery cathode material and preparation method thereof
CN105280909A
Preparation method of lithium nickel cobalt manganese oxide positive electrode material
CN106654227A
Preparation method of nickel-cobalt-lithium manganate material and cathode material for lithium battery
CN109775767A