Refractory mortar for building refractory bricks of carbon roasting furnace and preparation method of refractory mortar

By using a combination of specific powder materials and bonding agents, a highly efficient refractory mud for refractory brick masonry of carbon roasting furnaces was prepared, which solved the problem of shrinking and softening of existing refractory mud at high temperatures and improved the stability of the roasting furnace. The performance and service life also reduce costs and meet the requirements of carbon roasting furnaces in high temperature environment.

CN119019159APending Publication Date: 2024-11-26HENAN XINCHENG IND REFRACTORY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411121363.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing refractory mud for refractory brick masonry of carbon roasting furnaces is prone to shrink and soften at high temperatures, resulting in the wall of the roasting furnace, affecting production efficiency and product quality, and at the same time, the cost is high and lacks market competitiveness.

Method used

Refractory mud is made of materials such as 50-grade high-alumina bauxite clinker fine powder, cyanite tailings fine powder, waste silicon brick fine powder, clay raw material fine powder, montmorillonite fine powder and corundum dust collecting powder. Combining sodium tripolyphosphate, sodium hexametaphosphate and pregelatinized starch as binding agents, the flexural bonding strength and high-temperature performance of refractory mud are improved through the high-temperature expansion and non-contraction characteristics and the role of thickener.

Benefits of technology

It significantly improves the flexural bonding strength and high temperature stability of refractory mud, extends the service life of the roasting furnace, reduces production costs, and meets the stability and durability requirements of the carbon roasting furnace in the high temperature environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995186590000081
    Figure BDA0004995186590000081
  • Figure BDA0004995186590000082
    Figure BDA0004995186590000082
  • Figure BDA0004995186590000092
    Figure BDA0004995186590000092
Patent Text Reader

Abstract

The invention belongs to the field of refractory materials, and relates to refractory mortar for building refractory bricks of a carbon roasting furnace, which is prepared from a mixed powder material and a binding agent, and the mixed powder material is prepared from the following five or more powder materials in percentage by weight: 45-60% of 50-grade high-alumina bauxite clinker fine powder, 10-20% of 50-grade high-alumina bauxite clinker fine powder, 5-10% of 50-grade high-alumina bauxite clinker fine powder, 5-10% of 50-grade high-alumina bauxite clinker fine powder and 5 the fine powder of the kyanite tailings accounts for 5-25% by weight, the fine powder of the waste silica bricks accounts for 5-25% by weight, the fine powder of the pyrophyllite raw ore accounts for 10-25% by weight, the fine powder of the clay raw material accounts for 10-30% by weight, the fine powder of the montmorillonite accounts for 5-15% by weight, the fine powder of the montmorillonite accounts for 10-20% by weight, and the corundum dust collection powder accounts for 10-20% by weight; and the binding agent accounts for 3-5% of the mixed powder material. Compared with the prior art, all parameter indexes are higher than the national standard, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of refractory materials for carbon roasting furnaces, and in particular to refractory mud for building refractory bricks for carbon roasting furnaces and a preparation method thereof. Background Art

[0002] Carbon roasting furnace is one of the main equipment for roasting carbon products such as crucibles, negative electrode materials, graphite electrodes, and anode carbon blocks for aluminum. Carbon products are roasted in the material box of the roasting furnace in an indirect manner, isolating the air, and burning off the volatiles in the carbon product materials to form carbon products. The wall material of the material box of the carbon roasting furnace is built with refractory bricks. Its masonry height is more than 5.5 meters, and more than 55 layers of refractory bricks are required. Refractory mud is used to bond the refractory bricks. The use requirements also limit the AL203 content of the refractory mud to between 42 and 45%, so as to ensure that it can withstand the use conditions of the carbon roasting furnace at 1150℃ to 1300℃. Under this standard, how to ensure that such a high wall has good stability under high temperature, the brick joints are firmly combined, the refractory mud used for masonry does not shrink, improve the bearing capacity of the refractory mud, and keep the wall from sinking, the refractory mud used is particularly important. In the prior art, some refractory muds used for laying refractory bricks are selected according to the national standards GB / T14982-2008 and NN-42, with an AL203 content greater than 42%. Others are selected according to the GB / T14982-2008 and NN-45 refractory mud standards, with an AL203 content greater than 45%, but these standards do not have requirements for the 0.2MPa load softening temperature. Some choose the national standard YB / T4443-2014 high-temperature cement standard for carbon roasting furnaces, among which the refractory muds listed in the range of 45-50% of GWJN-45A, GWJN-50A, GWJN-45B, GWJN-50B, and AL203 have no requirements for the 0.2MPa load softening temperature and the permanent line change rate of 1200℃×3h heating. The refractory muds used all have requirements for the flexural bonding strength. However, in actual use, this type of refractory mud will shrink and soften, causing the fire channel wall of the roasting furnace to sink to varying degrees in the range of 60-120mm during the baking process. In the long-term use process, as the refractory mud gradually softens, deforms and shrinks, the wall of the roasting furnace will sink more and more. Due to the influence of the sinking, the refractory bricks of the fire channel wall of the roasting furnace will also have falling cracks of varying sizes, which will affect the normal production of the roasting furnace and reduce the quality of the baked carbon products.

[0003] In the prior art, influenced by market price competition and cost control factors, the refractory mud for preparing refractory bricks for roasting furnaces mostly adopts GB / T14982-2008 and NN-42 refractory mud standards. The refractory mud with AL203 content in the range of 42 to 45% can be used at a temperature between 1150°C and 1300°C, and the market sales price is between 950 and 1300 yuan / ton. Therefore, influenced by market price factors, the production cost of refractory mud for carbon roasting furnace refractory bricks is too high, and there is no market competitiveness and demand.

[0004] Patent document CN109437939B discloses a refractory mud and a preparation method thereof, which discloses that the material is composed of: 20-50 parts of waste corundum bricks, 5-10 parts of alumina powder, 20-50 parts of homogenizing powder, 3-5 parts of carbonized silicon powder, 5-10 parts of Guangxi white mud, 5-10 parts of graphite powder, 2-5 parts of binder and 23-26 parts of bonding agent. The content of AL203 in the waste corundum bricks used is greater than 90%, the content of AL203 in the alumina powder is greater than 99%, and the content of AL203 in the homogenizing powder is greater than 80%. All the materials used are high-grade materials. The prepared refractory mud is mainly used for the sliding water nozzle of the ladle and the tundish in steel smelting, and the masonry of the ladle air bricks. The use temperature is above 1580°C. Its cost is too high in the field of refractory brick masonry of carbon roasting furnaces. The use effect is not very good between 1150°C and 1300°C, the cost is also high, and there is no market demand.

[0005] Patent document CN115403359A discloses a refractory clay and a preparation method thereof, which discloses that the material is composed of: 50-80 parts of hollow alumina ball aggregate, 20-30 parts of thermal conductive material, 10-30 parts of porous filler, 2-8 parts of high thermal insulation material, 1-5 parts of activated alumina powder, 1-5 parts of graphite powder, 0.1-0.5 parts of polyacrylamide, and 0.5-2 parts of sodium alginate. The material is both thermally conductive and thermally insulating, but the purpose and effect described are unclear. The particle size of the hollow alumina ball is 0.2-5mm, which is somewhat large and is not suitable for use in refractory clay for carbon roasting furnaces.

[0006] Patent document CN102311270A discloses that the material is composed of: 5-35% of white corundum particles 1-0.088mm, 30-75% of white corundum fine powder 150-325 mesh, and uses white corundum as the main material. The prepared refractory mud AL203 content is greater than 90%, and the refractory temperature is above 1790°C. However, the refractory brick masonry of carbon roasting furnace does not require such high-temperature resistant refractory mud, and the cost of white corundum is high, so it is not suitable for carbon roasting furnace.

[0007] Patent document CN115700235A discloses a method for preparing refractory mud from waste electrical porcelain and waste cordierite slabs, which discloses that the material is composed of: 50-75% waste electrical porcelain, 20-45% waste cordierite slabs, 3-8% clay, 0.5-2.5% aluminum dihydrogen phosphate, and 2-6% pyrophyllite. The prepared refractory mud belongs to heat-resistant and alkali-resistant refractory mud, and its main raw material is waste electrical porcelain. However, the refractoriness of waste electrical porcelain is relatively low, which cannot meet the requirements of 0.2MPa load softening temperature and 1200℃×3h heating permanent linear change rate of refractory mud in the field of carbon roasting furnace refractory brick masonry.

[0008] Patent document CN102807377B discloses a method for preparing refractory mud for refractory brick masonry of a roasting furnace flue wall, which discloses that the material is composed of high-alumina clinker with different AL203 contents, mullite clinker, alumina powder, and high-quality white clay material. The prepared refractory mud has an AL203 content of more than 65%, and mainly meets the index of flexural bonding strength. However, the 0.2MPa load softening temperature and 1200℃×3h heating permanent line change rate index of the refractory mud are not described. The materials used, high-alumina clinker grade I and II, mullite clinker, and alumina powder are expensive, and the production cost of the refractory mud is high.

[0009] Therefore, it is urgently necessary to use refractory mud for refractory brick masonry of refractory walls over 5.5 meters high for carbon roasting furnaces, which should be higher than the existing national standards, to improve the load-bearing capacity of the refractory mud, reduce the sinking and deformation of the roasting furnace walls during use, extend the service life of the roasting furnace, and reduce costs. Summary of the invention

[0010] The refractory mud for refractory brick masonry of carbon roasting furnace provided by the present invention and its preparation method, the refractory mud has an AL203 content between 42% and 45%, meets the use standard of carbon roasting furnace, and the refractory mud has a bending strength of ≥1.5MPa after drying at 110℃, ≥3.5MPa at 1200℃×3h, and a load softening temperature of ≥0.2MPa.

[0011] The permanent line change rate of heating at 1200°C and 1200°C×3h reaches -3 to +1%, and the cost is low compared to the refractory clay in the prior art.

[0012] In order to solve the above technical problems, the refractory mud for refractory brick masonry of carbon roasting furnace and the preparation method thereof are implemented as follows:

[0013] A refractory mud for refractory brick masonry of a carbon roasting furnace is made of a mixed powder material and a binder. The mixed powder material is made of the following five or more powder materials: 50-grade high-alumina bauxite clinker fine powder, kyanite tailings fine powder, waste silica brick fine powder, pyrophyllite ore fine powder, clay raw material fine powder, montmorillonite fine powder, 60-grade high-alumina bauxite clinker dust collection powder and corundum dust collection powder. Among the five or more powder materials: the 50-grade high-alumina bauxite clinker fine powder accounts for 45-60% by weight, and the The kyanite tailings fine powder accounts for 5-25% by weight, the waste silicon brick fine powder accounts for 5-25% by weight, the pyrophyllite ore fine powder accounts for 10-25% by weight, the clay raw material fine powder accounts for 10-30% by weight, the montmorillonite fine powder accounts for 5-15% by weight, the 60-grade high-alumina bauxite clinker dust powder accounts for 10-20% by weight, and the corundum dust powder accounts for 10-20% by weight; the binder accounts for 3-5% of the mixed powder material.

[0014] The 50-grade high-alumina clinker fine powder of the present invention is a high-alumina clinker fine powder with an AL2O3 content of 50%, which mainly provides the AL2O3 required in the refractory mud; the 60-grade high-alumina clinker dust collecting powder is a high-alumina clinker fine powder with an AL2O3 content of 60%, which can also provide the AL2O3 required in the refractory mud. The kyanite tailings fine powder is a surplus product beyond the grade left when screening the kyanite concentrate. It has a unique high-temperature expansion characteristic. At a high temperature of 1000°C, part of the material is converted into mullite, which plays a role in volume stability and non-contraction in the refractory mud, and also has waste utilization. Waste silica brick fine powder is waste silica bricks collected from various kilns after years of use. Its SiO2 content is more than 90%. The waste silica bricks are processed into fine powder with a particle size greater than or equal to 180 mesh and added to the mixed powder of refractory mud. After reacting with AL2O3 in the mixed powder at high temperature, mullite rock phase is formed. It also plays a role in volume stability and non-contraction in refractory mud, and also achieves waste utilization. Pyrophyllite ore fine powder is a raw material directly processed into fine powder from ore mined from mines. This material has the performance of slight volume expansion at high temperature, which can make up for the shortcomings of high temperature indicators of other materials. 60-grade high-alumina bauxite clinker dust collection powder and corundum dust collection powder are dust removal powders collected by dust removal equipment when processing segment sand particles. The dust removal powder particles are finer and can reach more than 230 meshes. Adding some finer subdivisions can increase the bulk density of the mixed powder in the refractory mud mixed powder, fill the gaps between fine particles, increase the density and bonding strength of the refractory mud, and improve the high-temperature bending resistance index of the refractory mud. Montmorillonite fine powder belongs to clay mineral. Montmorillonite fine powder with a particle size of 180 mesh is added to the mixed powder of the present invention as a thickener and suspension stabilizer to increase the viscosity of the refractory clay. At the same time, a solvated film and a three-dimensional network structure can be formed on the surface of the base material particles of the mixed powder to support and prevent the particles from sinking, which can reduce the sintering temperature of the refractory clay and improve the high-temperature bonding strength of the refractory clay.

[0015] Various fine powder raw materials of the present invention are added and mixed in different proportions to make up for each other's performance deficiencies. Clay raw material fine powder and montmorillonite fine powder can increase the viscosity and consistency of refractory mud and play the role of suspension stabilizer, but will shrink in volume at a high temperature of 1100°C. By adding kyanite tailings fine powder, waste silica brick fine powder, and pyrophyllite ore fine powder, the material properties of no volume shrinkage and slight expansion at a high temperature of 1100°C are utilized, and the mullite rock phase is formed after reacting with AL2O3 in the material at high temperature, which makes up for the volume shrinkage of refractory mud at high temperature and improves the high temperature performance indicators of refractory mud such as high temperature bending resistance, heating permanent linear change rate, and load softening temperature.

[0016] Optionally, the AL203 content of the 60-grade high-alumina clinker dust powder is greater than 58%, the AL203 content of the 50-grade high-alumina clinker fine powder is greater than 50%, the AL203 content of the kyanite tailings fine powder is greater than 45%, the AL203 content of the clay raw material fine powder is greater than 28%, and the AL203 content of the corundum dust fine powder is greater than 80%; the SiO2 content of the waste silica brick fine powder is greater than 92%, the SiO2 content of the phyllite ore fine powder is greater than 70%, and the SiO2 content of the montmorillonite fine powder is greater than 65%.

[0017] Optionally, the particle size of the 50-grade high-alumina bauxite clinker fine powder is ≥180 mesh, the particle size of the kyanite tailings fine powder is ≥180 mesh, the particle size of the waste silicon brick fine powder is ≥180 mesh, the particle size of the phyllite ore fine powder is ≥180 mesh, the particle size of the clay raw material fine powder is ≥180 mesh, the particle size of the montmorillonite fine powder is ≥180 mesh, the particle size of the 60-grade high-alumina bauxite clinker dust collection powder is ≥230 mesh, and the particle size of the corundum dust collection powder is ≥230 mesh.

[0018] Optionally, the AL203 content of the 60-grade high-alumina bauxite clinker dust powder is greater than 58%, the AL203 content of the 50-grade high-alumina bauxite clinker fine powder is greater than 50%, the AL203 content of the kyanite tailings fine powder is greater than 45%, the AL203 content of the clay raw material fine powder is greater than 28%, the AL203 content of the corundum dust powder is greater than 80%, the SiO2 content of the waste silica brick fine powder is greater than 92%, the SiO2 content of the phyllite ore fine powder is greater than 70%, and the SiO2 content of the montmorillonite fine powder is greater than 65%.

[0019] Optionally, the binder is made of the following raw materials in weight percentage: 0.5-1% sodium tripolyphosphate, 0.5-1% sodium hexametaphosphate and 1-3% pregelatinized starch.

[0020] The present invention limits the content of the binder to 3% to 5%. If the content of the binder is too high or too low, it may affect the chemical stability, bonding strength, etc. of the refractory clay, and each component in the binder also needs to be maintained within the range specified in the present invention. If the content of the binder is too high or too low, it will affect the stability and bonding strength of the refractory clay.

[0021] Optionally, the mixed powder is made of powder materials with the following weight percentages: the 50-grade high-alumina clinker fine powder accounts for 49% by weight, the phyllite ore fine powder accounts for 13% by weight, the clay raw material fine powder accounts for 15% by weight, the montmorillonite fine powder accounts for 5% by weight, and the 60-grade high-alumina clinker dust powder accounts for 18% by weight; the binder accounts for 4.3% of the mixed powder material.

[0022] Optionally, the mixed powder is made of powder materials with the following weight percentages: the 50-grade high-alumina clinker fine powder accounts for 54% by weight, the kyanite tailings fine powder accounts for 13% by weight, the clay raw material fine powder accounts for 13% by weight, the montmorillonite fine powder accounts for 5% by weight, the 60-grade high-alumina clinker dust powder accounts for 15% by weight, and the corundum dust powder accounts for 12% by weight; the binder accounts for 3% of the mixed powder material.

[0023] Optionally, the mixed powder is made of powder materials with the following weight percentages: the 50-grade high-alumina clinker fine powder accounts for 47% by weight, the kyanite tailings fine powder accounts for 10% by weight, the waste silicon brick fine powder accounts for 22% by weight, the montmorillonite fine powder accounts for 8% by weight, and the 60-grade high-alumina clinker dust powder accounts for 13% by weight; the binder accounts for 3-5% of the mixed powder material.

[0024] A method for preparing refractory mud for refractory brick masonry of a carbon roasting furnace, comprising weighing the powder raw material in claim 1 according to a proportion, adding the powder raw material into a mixing mixer and mixing for 10 to 15 minutes to form a mixed powder, and then putting the mixed powder into a 50kg or 25kg double-layer coated plastic woven bag and sealing it;

[0025] The binder raw materials of claim 1 are weighed in proportion and packed into a 2 kg small plastic bag, which is then sealed and placed into the 50 kg or 25 kg double-layer coated plastic woven bag.

[0026] A method for using refractory mud for refractory brick masonry of a carbon roasting furnace is characterized in that a bag of mixed powder and a bag of binder are added into a mud mixer, and tap water accounting for 30% to 35% of the total mass of the mixed powder and the binder is added and stirred for 10 to 15 minutes until the refractory mud reaches a viscous and wire-drawn state before use.

[0027] The main material sources of the refractory mud of the present invention are finished clinker powder materials, which reduces the amount of raw ore powder materials used and reduces the cost of the refractory mud; some powder materials that expand but do not shrink at high temperatures are added, and powder materials with a fineness greater than 300 mesh are added to increase the density of the refractory mud and improve the bonding strength effect, and different proportions of additional binders are added to achieve the purpose of the present invention.

[0028] The performance indicators of the present invention are as follows: AL203 content is between 42% and 45%, the flexural bonding strength of the refractory mud after drying at 110°C is ≥1.5MPa and 1200°C×3h is ≥3.5MPa, the softening temperature under 0.2MPa load is ≥1200°C, and the permanent line change rate after heating at 1200°C×3h reaches -3 to +1%, which are higher than the national standards. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail in the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0030] The present invention limits the mesh size of the raw materials used, the particle size of the 50-grade high-alumina bauxite clinker fine powder is ≥180 mesh, the particle size of the kyanite tailings fine powder is ≥180 mesh, the particle size of the waste silicon brick fine powder is ≥180 mesh, the particle size of the pyrophyllite ore fine powder is ≥180 mesh, the particle size of the clay raw material fine powder is ≥180 mesh, the particle size of the montmorillonite fine powder is ≥180 mesh, the particle size of the 60-grade high-alumina bauxite clinker dust collection powder is ≥230 mesh, and the particle size of the corundum dust collection powder is ≥230 mesh, wherein the minimum mesh size defined is the minimum usage standard. Considering the cost and market conditions, the present invention can also be realized by selecting fine powder slightly larger than the mesh size of the present invention.

[0031] The AL203 content of the present invention is detected in accordance with the GB / T21114-2019 standard, and the 110°C flexural bonding strength, 1200°C×3h flexural bonding strength, 200°C×3h permanent linear change and load softening temperature are detected according to the GB / T22459.7-2019 standard.

[0032] The method for preparing refractory mud for refractory brick masonry of a carbon roasting furnace of the present invention comprises the following steps: weighing the powder raw materials according to a proportion, adding the powder raw materials into a mixing and stirring machine and mixing for 10 to 15 minutes to form a mixed powder, and then putting the mixed powder into a 50kg or 25kg double-layer coated plastic woven bag and sealing the bag;

[0033] The binder raw materials are weighed in proportion and put into a 2 kg small plastic bag together, which is then sealed and put into the 50 kg or 25 kg double-layer film-covered plastic woven bag.

[0034] The present invention provides a method for using refractory mud for refractory brick masonry of carbon roasting furnace, which is a method for preparing refractory mud and water before construction, adding a bag of mixed powder and a bag of binder into a mud mixer, adding tap water of 30% to 35% of the total mass of the mixed powder and the binder, stirring for 10 to 15 minutes, stirring until the refractory mud reaches a viscous wire drawing state, and then using it. After the refractory mud is stirred with water, it can be used for construction.

[0035] The following provides a detailed embodiment of the refractory mud for refractory brick masonry of the carbon roasting furnace of the present invention. The preparation method and use method of the refractory mud are suitable for the following embodiments.

[0036] Embodiment 1

[0037] Example 1 The weight percentages of raw material components are shown in Table 1:

[0038]

[0039] Table 1

[0040] Embodiment 1 Refractory clay performance parameters:

[0041] AL2O3 content is 43.35%, flexural bonding strength index after drying at 110℃: 2.8MPa, 1200℃×3h: 4.2MPa, 1200℃×3h heating permanent line change rate -0.3%, load softening temperature (0.2MPa, 0.6%) 1235℃.

[0042] Embodiment 2

[0043] Example 2 The weight percentages of raw material components are shown in Table 2:

[0044]

[0045]

[0046] Table 2

[0047] Example 2 Refractory clay performance parameters:

[0048] AL2O3 content is 43.19%, flexural bonding strength index after drying at 110℃: 2.5MPa, 1200℃×3h: 4.5MPa, 1200℃×3h heating permanent line change rate -0.1%, load softening temperature (0.2MPa, 0.6%) 1275℃.

[0049] Embodiment 3

[0050] Example 3 The weight percentages of raw material components are shown in Table 3:

[0051]

[0052] Table 3

[0053] Example 3 Refractory clay performance parameters:

[0054] AL2O3 content is 43.05%, flexural bonding strength index after drying at 110℃: 2.3MPa, 1200℃×3h: 3.8MPa, 1200℃×3h heating permanent line change rate -0.2%, load softening temperature (0.2MPa, 0.6%) 1228℃.

[0055] Embodiment 4

[0056] The weight percentages of the raw material components of Example 4 are shown in Table 4:

[0057]

[0058]

[0059] Table 4

[0060] Embodiment 4 Refractory clay performance parameters:

[0061] AL2O3 content is 43.35%, flexural bonding strength index after drying at 110℃: 2.2MPa, 1200℃×3h: 4.3MPa, 1200℃×3h heating permanent line change rate -0.2%, load softening temperature (0.2MPa, 0.6%) 1235℃.

[0062] Embodiment 5

[0063] Example 5 The weight percentages of raw material components are shown in Table 5:

[0064]

[0065] Table 5

[0066] Example 5 Refractory Clay Performance Parameters:

[0067] AL2O3 content is 43.45%, flexural bonding strength index after drying at 110℃: 2.3MPa, 1200℃×3h: 4.2MPa, 1200℃×3h heating permanent line change rate -0.15%, load softening temperature (0.2MPa, 0.6%) 1240℃.

[0068] Embodiment 6

[0069] Example 6 The weight percentages of raw material components are shown in Table 6:

[0070]

[0071] Table 6

[0072] Example 6 Refractory Clay Performance Parameters:

[0073] AL2O3 content is 43.75%, flexural bonding strength index after drying at 110℃: 2.3MPa, 1200℃×3h: 4.3MPa, 1200℃×3h heating permanent line change rate -0.15%, load softening temperature (0.2MPa, 0.6%) 1235℃.

[0074] Embodiment 7

[0075] Example 7 The weight percentages of raw material components are shown in Table 7:

[0076]

[0077] Table 7

[0078] Embodiment 7 Refractory clay performance parameters:

[0079] AL2O3 content is 42.8%, flexural bonding strength index after drying at 110℃: 2.1MPa, 1200℃×3h: 4.3MPa, 1200℃×3h heating permanent line change rate -0.5%, load softening temperature (0.2MPa, 0.6%) 1230℃.

[0080] Embodiment 8

[0081] Example 8 The weight percentages of raw material components are shown in Table 8:

[0082]

[0083] Table 8

[0084] Embodiment 8 Refractory clay performance parameters:

[0085] AL2O3 content is 43.85%, flexural bonding strength index after drying at 110℃: 2.4MPa, 1200℃×3h: 4.6MPa, 1200℃×3h heating permanent line change rate -0.3%, load softening temperature (0.2MPa, 0.6%) 1255℃.

[0086] Embodiment 9

[0087] Example 9 The weight percentages of raw material components are shown in Table 9:

[0088]

[0089]

[0090] Table 9

[0091] Embodiment 9 Refractory clay performance parameters:

[0092] AL2O3 content is 43.05%, flexural bonding strength index after drying at 110℃: 2.6MPa, 1200℃×3h: 3.9MPa, 1200℃×3h heating permanent line change rate -0.1%, load softening temperature (0.2MPa, 0.6%) 1226℃.

[0093] Embodiment 10

[0094] Example 10 The weight percentages of the raw material components are shown in Table 10:

[0095]

[0096] Table 10

[0097] Embodiment 10 Refractory clay performance parameters:

[0098] AL2O3 content is 45%, flexural bonding strength index after drying at 110℃: 2.3MPa, 1200℃×3h: 4.4MPa, 1200℃×3h heating permanent line change rate is 0.3%, load softening temperature (0.2MPa, 0.6%) is 1248℃.

[0099] Embodiment 11

[0100] Example 11 The weight percentages of raw material components are shown in Table 11:

[0101]

[0102] Table 11

[0103] Embodiment 11 Refractory clay performance parameters:

[0104] AL2O3 content is 42.9%, flexural bonding strength index after drying at 110℃: 2.2MPa, 1200℃×3h: 4.1MPa, permanent line change rate after heating at 1200℃×3h is 0.2%, and load softening temperature (0.2MPa, 0.6%) is 1245℃.

[0105] Embodiment 12

[0106] Example 12 The weight percentages of raw material components are shown in Table 12:

[0107]

[0108] Table 12

[0109] Embodiment 12 Refractory clay performance parameters:

[0110] AL2O3 content is 42.8%, flexural bonding strength index after drying at 110℃: 2.5MPa, 1200℃×3h: 4.2MPa, 1200℃×3h heating permanent line change rate is 1%, load softening temperature (0.2MPa, 0.6%) is 1238℃.

[0111] There is little difference between the embodiments 1 to 12, which shows that the range of the content of each substance in the present invention is reasonably configured. The Al2O3 content in embodiment 6 is slightly larger, which may be due to the higher content of alumina clinker fine powder; the load softening temperature is not much different; the 110℃ drying flexural bonding strength, 1200℃×3h flexural bonding strength and load softening temperature in embodiments 2 and 8 are slightly larger, which may be due to the high mesh number of corundum dust collecting powder, the large content of 60-grade alumina clinker fine powder and the content of 50-grade alumina clinker fine powder, the higher Al2O3 content and the larger content of fine powder, which make the refractory mud have higher fluidity and plasticity, but its 1200℃×3h permanent line change is not as good as that in embodiments 5 and 9. The various indicators of embodiments 6 and 8 are relatively moderate, indicating that their material combination Al2O3 content and microstructure are good.

[0112] Embodiment 13

[0113] Example 13 The weight percentages of the raw material components are shown in Table 13:

[0114]

[0115] Table 13

[0116] Example 13 Refractory clay performance parameters:

[0117] AL2O3 content is 45%, flexural bonding strength index after drying at 110℃: 3.2MPa, 1200℃×3h: 5.0MPa, 1200℃×3h heating permanent line change rate -0.3%, load softening temperature (0.2MPa, 0.6%) 1280℃.

[0118] Embodiment 14

[0119] Example 14 The weight percentages of the raw material components are shown in Table 14:

[0120]

[0121] Table 14

[0122] Example 14 Refractory clay performance parameters:

[0123] AL2O3 content is 42.1%, flexural bonding strength index after drying at 110℃: 1.8MPa, 1200℃×3h: 3.6MPa, 1200℃×3h heating permanent line change rate -0.3%, load softening temperature (0.2MPa, 0.6%) 1280℃.

[0124] Embodiment 15

[0125] Example 15 The weight percentages of raw material components are shown in Table 15:

[0126]

[0127]

[0128] Table 15

[0129] Embodiment 15 Refractory clay performance parameters:

[0130] AL2O3 content is 42.5%, flexural bonding strength index after drying at 110℃: 1.7MPa, 1200℃×3h: 3.6MPa, 1200℃×3h heating permanent line change rate -3%, load softening temperature (0.2MPa, 0.6%) 1210℃.

[0131] Embodiment 16

[0132] Example 16 The weight percentages of the raw material components are shown in Table 16:

[0133]

[0134] Table 16

[0135] Embodiment 16 Refractory clay performance parameters:

[0136] AL2O3 content is 42.3%, flexural bonding strength index after drying at 110℃: 1.5MPa, 1200℃×3h: 3.5MPa, 1200℃×3h heating permanent line change rate is 0.5%, load softening temperature (0.2MPa, 0.6%) is 1225℃.

[0137] Embodiment 17

[0138] Example 17 The weight percentages of the raw material components are shown in Table 17:

[0139]

[0140]

[0141] Table 17

[0142] Embodiment 17 Refractory clay performance parameters:

[0143] AL2O3 content is 44.5%, flexural bonding strength index after drying at 110℃: 3.5MPa, 1200℃×3h: 4.2MPa, permanent line change rate after heating at 1200℃×3h is 1%, and load softening temperature (0.2MPa, 0.6%) is 1300℃.

[0144] Embodiment 18

[0145] Example 18 The weight percentages of the raw material components are shown in Table 18:

[0146]

[0147] Table 18

[0148] Embodiment 18 Refractory clay performance parameters:

[0149] AL2O3 content is 43.1%, flexural bonding strength index after drying at 110℃: 2.5MPa, 1200℃×3h: 4.3MPa, 1200℃×3h heating permanent line change rate is 1%, load softening temperature (0.2MPa, 0.6%) is 1290℃.

[0150] In Example 13 to Example 18, experiments were conducted on the critical values ​​of the contents of each component in the refractory mud of the present invention, and the test parameters were analyzed as follows: in Example 13, the content of 50-grade high-alumina bauxite clinker fine powder reached the highest range, the content of kyanite tailings fine powder was the smallest range, the alumina content of the refractory mud reached 45%, the load softening temperature was also relatively high, and the permanent line change of 1200°C×3h also reached the critical value; in Example 14, the content of kyanite tailings fine powder reached the largest range, the content of 50-grade high-alumina bauxite clinker fine powder reached the smallest range, and the various parameter indicators decreased accordingly. Although the kyanite tailings fine powder can improve the load softening performance index of the refractory mud to a certain extent, if the content is too high, it will cause the parameter index to decrease; in Example 15, the content of waste silicon brick powder is the largest. In order to match the other ingredients in the formula, the content of 50-grade high-alumina bauxite clinker fine powder reaches the smallest range, and in Example 10 All the parameters of Example 5 are in a moderate state, only the permanent line at 1200℃×3h changes slightly, reaching the critical value specified in the present invention. The silicon dioxide and alumina in the waste silicon bricks form a mullite phase structure. When the content of the waste silicon bricks is too large, the parameter index will decrease instead; in Example 16, the clay raw material fine powder reaches the maximum, and the content of 50-grade high-alumina bauxite clinker fine powder reaches the minimum range to match the other ingredients in the formula. All the parameters are at the critical value required by the present invention. It may be that the content of clay raw material fine powder is too large, which affects the refractory mud; in Examples 17 and 18, 50-grade high-alumina bauxite clinker fine powder is not used, and the content of 60-grade high-alumina bauxite clinker fine powder and corundum dust collection powder increases accordingly. All the performance parameter indicators have increased, and the permanent line change at 1200℃×3h is also the largest, and the shrinkage rate is small, which may be due to the increase in aluminum content. Moreover, increasing the corundum content will increase the cost a lot.

[0151] Although some parameter indicators of the refractory clay of Examples 13 to 18 are at the minimum or maximum requirements of the present invention, they all meet the requirements of the present invention. If the content of each component is greater than or less than the content specified in the present invention, it may cause various performance indicators to fail to meet the requirements of the present invention.

[0152] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A refractory mud for refractory brick masonry of carbon roasting furnace, characterized in that: The invention is made of a mixed powder material and a binder, wherein the mixed powder material is made of the following five or more powder materials: 50-grade high-alumina bauxite clinker fine powder, kyanite tailings fine powder, waste silica brick fine powder, pyrophyllite ore fine powder, clay raw material fine powder, montmorillonite fine powder, 60-grade high-alumina bauxite clinker dust collection powder and corundum dust collection powder, among the five or more powder materials: the 50-grade high-alumina bauxite clinker fine powder accounts for 45-60% by weight, the kyanite tailings fine powder accounts for The weight percentage is 5-25%, the waste silicon brick fine powder accounts for 5-25% by weight, the pyrophyllite ore fine powder accounts for 10-25% by weight, the clay raw material fine powder accounts for 10-30% by weight, the montmorillonite fine powder accounts for 5-15% by weight, the 60-grade high-alumina bauxite clinker dust powder accounts for 10-20% by weight, and the corundum dust powder accounts for 10-20% by weight; the binder accounts for 3-5% of the mixed powder material.

2. The refractory mortar for refractory brick masonry of carbon roasting furnace according to claim 1, characterized in that: The AL203 content of the 60-grade high-alumina bauxite clinker dust powder is greater than 58%, the AL203 content of the 50-grade high-alumina bauxite clinker fine powder is greater than 50%, the AL203 content of the kyanite tailings fine powder is greater than 45%, the AL203 content of the clay raw material fine powder is greater than 28%, and the AL203 content of the corundum dust powder is greater than 80%; the SiO2 content of the waste silica brick fine powder is greater than 92%, the SiO2 content of the phyllite ore fine powder is greater than 70%, and the SiO2 content of the montmorillonite fine powder is greater than 65%.

3. The refractory mortar for refractory brick masonry of carbon roasting furnace according to claim 1, characterized in that: The particle size of the 50-grade high-alumina bauxite clinker fine powder is ≥180 mesh, the particle size of the kyanite tailings fine powder is ≥180 mesh, the particle size of the waste silicon brick fine powder is ≥180 mesh, the particle size of the pyrophyllite ore fine powder is ≥180 mesh, the particle size of the clay raw material fine powder is ≥180 mesh, the particle size of the montmorillonite fine powder is ≥180 mesh, the particle size of the 60-grade high-alumina bauxite clinker dust collection powder is ≥230 mesh, and the particle size of the corundum dust collection powder is ≥230 mesh.

4. The refractory mortar for refractory brick masonry of carbon roasting furnace according to claim 1, characterized in that: The AL203 content of the 60-grade high-alumina bauxite clinker dust powder is greater than 58%, the AL203 content of the 50-grade high-alumina bauxite clinker fine powder is greater than 50%, the AL203 content of the kyanite tailings fine powder is greater than 45%, the AL203 content of the clay raw material fine powder is greater than 28%, the AL203 content of the corundum dust powder is greater than 80%, the SiO2 content of the waste silica brick fine powder is greater than 92%, the SiO2 content of the phyllite ore fine powder is greater than 70%, and the SiO2 content of the montmorillonite fine powder is greater than 65%.

5. The refractory mortar for refractory brick masonry of carbon roasting furnace according to any one of claims 1 to 4, characterized in that: The binder is made of the following raw materials in weight percentage: 0.5-1% sodium tripolyphosphate, 0.5-1% sodium hexametaphosphate and 1-3% pregelatinized starch.

6. The refractory mortar for refractory brick masonry of carbon roasting furnace according to claim 5, characterized in that: The mixed powder is made of powder materials with the following weight percentages: the 50-grade high-alumina bauxite clinker fine powder accounts for 49% by weight, the phyllite ore fine powder accounts for 13% by weight, the clay raw material fine powder accounts for 15% by weight, the montmorillonite fine powder accounts for 5% by weight, and the 60-grade high-alumina bauxite clinker dust powder accounts for 18% by weight; the binder accounts for 4.3% of the mixed powder material.

7. The refractory mortar for refractory brick masonry of carbon roasting furnace according to claim 5, characterized in that: The mixed powder is made of powder materials with the following weight percentages: the 50-grade high-alumina bauxite clinker fine powder accounts for 54% by weight, the kyanite tailings fine powder accounts for 13% by weight, the clay raw material fine powder accounts for 13% by weight, the montmorillonite fine powder accounts for 5% by weight, the 60-grade high-alumina bauxite clinker dust powder accounts for 15% by weight, and the corundum dust powder accounts for 12% by weight; the binder accounts for 3% of the mixed powder material.

8. The refractory mortar for refractory brick masonry of carbon roasting furnace according to claim 5, characterized in that: The mixed powder is made of powder materials with the following weight percentages: the 50-grade high-alumina bauxite clinker fine powder accounts for 47% by weight, the kyanite tailings fine powder accounts for 10% by weight, the waste silicon brick fine powder accounts for 22% by weight, the montmorillonite fine powder accounts for 8% by weight, and the 60-grade high-alumina bauxite clinker dust powder accounts for 13% by weight; the binder accounts for 3-5% of the mixed powder material.

9. The method for preparing refractory mud for refractory brick masonry of carbon roasting furnace according to claim 1, characterized in that: After weighing the powder raw material in claim 1 according to the proportion, add it into a mixing mixer and mix it for 10 to 15 minutes to form a mixed powder, and then put it into a 50kg or 25kg double-layer coated plastic woven bag and seal it; The binder raw materials of claim 1 are weighed in proportion and packed into a 2 kg small plastic bag, which is then sealed and placed into the 50 kg or 25 kg double-layer coated plastic woven bag.

10. The method for using the refractory mortar for refractory brick masonry of carbon roasting furnace according to claim 1, characterized in that: Add a bag of mixed powder and a bag of binder into the mud mixer, add tap water which accounts for 30% to 35% of the total mass of the mixed powder and the binder, and stir for 10 to 15 minutes until the refractory mud reaches a viscous and wire-drawn state before use.

Citation Information

Patent Citations

  • Wet refractory mortar and preparation method thereof

    CN102020473A

  • Method for preparing refractory mortar for laying refractory bricks of flame path wall of calcining kiln

    CN102807378A

  • Aluminum-carbon refractory mortar added with sliding plate regenerated fine powder and preparation method of aluminum-carbon refractory mortar

    CN108358651A

  • Joint sealing material for flame path wall of carbon furnace and preparation method of joint sealing material

    CN117923918A