Ain joined body

By using flux in the AlN joint to form a diffusion layer and optimizing the bonding conditions, cracks and quality problems during the bonding process of the AlN joint are solved, and high-quality bond production is achieved.

CN119019176APending Publication Date: 2024-11-26NGK INSULATORS LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411133300.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-08-23
Filing Date
2022-06-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing AlN joints are prone to cracks during the bonding process, resulting in poor bonding, and the flux exudation amount and fine particles are generated, which affects the quality of the finished product.

Method used

The first and second AlN components are bonded with fluxes such as calcium oxide, alumina and yttrium trioxide to form a diffusion layer, optimizing bonding conditions to bond at low loads, ensuring bonding strength and crack-free.

Benefits of technology

A good AlN joint is achieved, reducing flux exudation and particle generation, improving bonding strength and bonding quality, and avoiding cracks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019176A_ABST
    Figure CN119019176A_ABST
Patent Text Reader

Abstract

Provided is an AlN bonded body that is satisfactorily bonded and has no cracks. An AlN bonded body (10) is obtained by bonding a first AlN member (11) and a second AlN member (12). The yttrium oxide content of the first AlN member (11) is equal to or less than the detection limit. The second AlN member (12) contains yttrium oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application number 2022106785490, application date June 16, 2022, and invention name “AlN joint body”. Technical Field

[0002] The present invention relates to an AlN joint body. Background Art

[0003] In the past, a ceramic heater was known, which comprises: an AlN plate having a chip loading surface for loading a chip and a built-in resistance heating element; and an AlN cylindrical shaft connected to the back side of the plate opposite to the chip loading surface (see patent document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 6878677 Summary of the invention

[0007] The ceramic heater is manufactured by applying flux to a plate made of AlN containing 5% by mass of yttrium trioxide and a cylindrical shaft made of AlN containing 5% by mass of yttrium trioxide. In recent years, in order to measure the peripheral temperature of the plate using a thermocouple, a groove for thermocouples is sometimes provided on the plate. In addition, as a countermeasure during wafer film formation, a groove for gas purging is sometimes provided on the plate. Therefore, a study was conducted on joining a cylindrical shaft to a plate with a groove formed thereon. As a result, it was found that in the existing joining method, cracks were generated starting from the groove. The cracks were generated because the pressing pressure during joining was high.

[0008] The present invention has been made to solve the above-mentioned problems, and a main object of the present invention is to provide an AlN bonded body that is well bonded and has no cracks.

[0009] One embodiment of the AlN bonded body of the present invention is an AlN bonded body obtained by bonding a first AlN component to a second AlN component.

[0010] The yttrium trioxide content of the first AlN component is below the detection limit,

[0011] The second AlN member contains yttrium trioxide.

[0012] Another embodiment of the AlN bonded body of the present invention is an AlN bonded body obtained by bonding a first AlN component to a second AlN component.

[0013] The first AlN member has a first diffusion layer formed by bonding,

[0014] the second AlN member has a second diffusion layer formed by bonding,

[0015] The yttrium trioxide content of the first AlN member except the first diffusion layer is below the detection limit,

[0016] A portion of the second AlN member other than the second diffusion layer contains yttrium trioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a front view of the AlN bonded structure 10 .

[0018] Figure 2 It is a front view of the AlN bonded structure 20 .

[0019] Figure 3 It is a front view of the AlN bonded structure 30 .

[0020] Figure 4 It is a front view of the AlN bonded structure 40 .

[0021] Figure 5 It is a longitudinal cross-sectional view of the ceramic heater 50 .

[0022] Figure 6 It is a manufacturing process diagram of the ceramic heater 50.

[0023] Figure 7 It is a longitudinal cross-sectional view of the ceramic heater 60 .

[0024] Explanation of symbols

[0025] 10, 20, 30, 40…AlN joint body, 11, 31…first AlN component, 12, 32…second AlN component, 13, 33…third AlN component, 31a…first diffusion layer, 32a…second diffusion layer, 33a…third diffusion layer, 50…ceramic heater, 51…intermediate ring, 52…circular plate, 52a…chip loading surface, 52b…resistance heating element, 52c…thermocouple groove, 53…cylindrical shaft, 53a…flange, 60…ceramic heater, 61…first circular plate, 61c…linear groove, 62…second circular plate, 62a…chip loading surface, 62b…resistance heating element, 63…third circular plate, 63c…through hole, 64…cylindrical shaft, 64a…flange, 65…stacked plate, 66…thermocouple groove. DETAILED DESCRIPTION

[0026] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. Figure 1 to Figure 4 is a front view of an AlN joint body 10 to 40, Figure 52 is a longitudinal cross-sectional view of the ceramic heater (a cross-sectional view when the ceramic heater is cut along a plane including the central axis). Figure 1 It should be noted that up and down, left and right, front and back are only relative positional relationships. In this specification, "to" indicating a numerical range is used to mean that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0027] Figure 1 The AlN joint body 10 shown is obtained by joining a first AlN component 11 and a second AlN component 12 using a flux (paste for joining). As the flux, for example, a material containing calcium oxide (CaO), aluminum oxide (Al2O3) and yttrium trioxide (Y2O3) can be used. The first AlN component 11 and the second AlN component 12 are circular plate components of the same size. The yttrium trioxide content of the first AlN component 11 is below the detection limit, and the second AlN component 12 contains yttrium trioxide. The yttrium trioxide content of the second AlN component 12 is preferably 0.07% by mass or more. The first AlN component 11 preferably contains at least one oxide selected from the group consisting of rare earth metal oxides other than yttrium trioxide, magnesium oxide (MgO) and titanium dioxide (TiO2). The total amount of oxide added can be, for example, 0.1 to 3% by mass. As rare earth oxides, for example, cerium dioxide (CeO2), samarium oxide (Sm2O3) and the like can be cited. The first AlN member 11 preferably contains a rare earth metal oxide other than yttrium trioxide or magnesium oxide and titanium dioxide, and more preferably contains magnesium oxide and titanium dioxide.

[0028] Figure 2 The AlN joint body 20 shown is obtained by joining the third AlN component 13 to the surface of the first AlN component 11 of the AlN joint body 10 on the opposite side of the joining surface of the second AlN component 12 using a flux. As the flux, for example, a material containing calcium oxide, aluminum oxide and yttrium trioxide can be used. The third AlN component 13 is a circular plate component of the same size as the first and second AlN components 11 and 12. The third AlN component 13 contains yttrium trioxide. The yttrium trioxide content of the third AlN component 13 is preferably 0.07 mass% or more.

[0029] Figure 3The AlN joint body 30 shown is obtained by joining a first AlN component 31 and a second AlN component 32 using a flux. As the flux, for example, a material containing calcium oxide (CaO), aluminum oxide (Al2O3) and yttrium trioxide (Y2O3) can be used. The first AlN component 31 and the second AlN component 32 are circular plate components of the same size. The first AlN component 31 has a first diffusion layer 31a formed by joining. The second AlN component 32 has a second diffusion layer 32a formed by joining. The first and second diffusion layers 31a, 32a are layers obtained by diffusion of flux components. The yttrium trioxide content of the portion of the first AlN component 31 other than the first diffusion layer 31a is below the detection limit, and the portion of the second AlN component 32 other than the second diffusion layer 32a contains yttrium trioxide. The yttrium trioxide content of the portion of the second AlN component 32 other than the second diffusion layer 32a is preferably 0.07 mass % or more. The first AlN component 31 preferably contains at least one oxide selected from the group consisting of rare earth metal oxides other than yttrium trioxide, magnesium oxide (MgO) and titanium dioxide (TiO2). The total amount of oxides added may be, for example, 0.1 to 3% by mass. Examples of rare earth oxides include cerium dioxide (CeO2) and samarium oxide (Sm2O3). The first AlN component 31 preferably contains rare earth metal oxides other than yttrium trioxide or magnesium oxide and titanium dioxide, and more preferably contains magnesium oxide and titanium dioxide.

[0030] Figure 4 The AlN joint body 40 shown is obtained by joining the third AlN component 33 to the surface of the first AlN component 31 of the AlN joint body 30 on the opposite side of the joining surface with the second AlN component 32 using a flux. As the flux, for example, a material containing calcium oxide, aluminum oxide and yttrium trioxide can be used. The third AlN component 33 is a circular plate component of the same size as the first and second AlN components 31 and 32. The first AlN component 31 has another first diffusion layer 31a formed by joining with the third AlN component 33. The third AlN component 33 has a third diffusion layer 33a formed by joining. The third diffusion layer 33a is a layer obtained by diffusion of flux components. The yttrium trioxide content of the portion other than the two first diffusion layers 31a of the first AlN component 31 is below the detection limit. The portion other than the third diffusion layer 33a of the third AlN component 33 contains yttrium trioxide. The yttrium trioxide content of the portion of the third AlN member 33 excluding the third diffusion layer 33 a is preferably 0.07 mass % or more.

[0031] Figure 5The ceramic heater 50 shown comprises: a circular plate 52 having a chip placement surface 52a and implanted with a resistance heating element 52b; a cylindrical shaft 53 having a diameter smaller than that of the circular plate 52; and an intermediate ring 51 sandwiched between the circular plate 52 and the cylindrical shaft 53. The circular plate 52 has a thermocouple groove 52c arranged along the radial direction inside. The cylindrical shaft 53 has a flange 53a on the side opposite to the circular plate 52. The intermediate ring 51 and the circular plate 52 are joined with a flux, and the intermediate ring 51 and the cylindrical shaft 53 are also joined with a flux. As the flux, for example, a material containing calcium oxide, aluminum oxide and yttrium trioxide can be used. As for the joining method, such as Figure 6 As shown, first, the circular plate 52 is placed on the workbench with the wafer placement surface 52a of the circular plate 52 facing downward, and flux P is applied in a ring shape on the surface opposite to the wafer placement surface 52a. The intermediate ring 51 is placed on the flux P, and flux P is applied to the upper surface of the intermediate ring 51. The cylindrical shaft 53 is placed on the flux P with the flange 53a facing downward. In this state, a load (e.g., 10 to 40 kg / cm2) is applied from above to the flange 53a. 2 ) and processed at a specified bonding temperature (e.g. 1600-1700°C). Figure 5 , the circular plate 52 corresponds to the second AlN member 12, 32, the cylindrical shaft 53 corresponds to the third AlN member 13, 33, and the intermediate ring 51 corresponds to the first AlN member 11, 31. It should be noted that as a countermeasure during wafer film formation, a groove for gas purge may be provided on the circular plate 52 instead of the thermocouple groove 52c, or in addition to the thermocouple groove 52c, as a countermeasure during wafer film formation, a groove for gas purge may be provided on the circular plate 52.

[0032] Figure 7 The ceramic heater 60 shown comprises: a second circular plate 62 having a chip placement surface 62a and implanted with a resistive heating element (heater) 62b; a third circular plate 63 joined to a cylindrical shaft 64; and a first circular plate 61 sandwiched between the second circular plate 62 and the third circular plate 63. The first to third circular plates 61 to 63 are joined to each other using a flux to form a stacked plate 65. As a flux, for example, a material containing calcium oxide, aluminum oxide and yttrium trioxide can be used. The stacked plate 65 has a thermocouple groove 66 arranged along the radial direction inside. The thermocouple groove 66 is composed of a straight groove 61c formed in the first circular plate 61 and a through hole 63c penetrating the third circular plate 63 in the up and down direction. The cylindrical shaft 64 has a flange 64a on the side opposite to the third circular plate 63, and the flange 64a is joined to the third circular plate 63. It can be arranged according to Figure 6 Make the connection. Figure 7, the second circular plate 62 corresponds to the second AlN component 12, 32, the third circular plate 63 corresponds to the third AlN component 13, 33, and the first circular plate 61 corresponds to the first AlN component 11, 31. It should be noted that as a countermeasure during wafer film formation, a groove for gas purge may be provided on the stacking plate 65 instead of the thermocouple groove 66, or in addition to the thermocouple groove 66, as a countermeasure during wafer film formation, a groove for gas purge may be provided on the stacking plate 65.

[0033] According to the AlN joint bodies 10 to 40 and the ceramic heaters 50 and 60 of the embodiments described in detail above, the components can be joined with a low load. Therefore, the joint is good and cracks are not easily generated in the components. In addition, the amount of flux seepage for joining is reduced, and the amount of particles generated during use is also reduced. In addition, the deformation of each component is reduced.

[0034] It should be noted that the present invention is not limited to the above-described embodiment and can be implemented in various forms as long as they fall within the technical scope of the present invention.

[0035] For example, in the above embodiment, the first to third AlN members 11 to 13 are disk members of the same size, but the present invention is not limited thereto. For example, the first to third AlN members 11 to 13 may be members of different shapes and sizes. The same applies to the first to third AlN members 31 to 33.

[0036] In the above-mentioned embodiment, flux (paste for bonding) is used, but a sheet for bonding may be used instead of the flux.

[0037] In addition, a thick AlN plate containing yttrium trioxide can be used to sandwich a thin AlN plate that does not contain yttrium trioxide (below the detection limit) to obtain a stacked AlN plate with high thermal conductivity. The higher the yttrium trioxide content of the AlN plate, the higher the thermal conductivity. In the obtained stacked AlN plate, the proportion of the plate containing yttrium trioxide is relatively large, so the thermal conductivity is good.

[0038] When thermocouple grooves, gas grooves, etc. are provided in the plates by utilizing the joining of the plates, sintering can be performed at a lower pressure, deformation can be prevented, and a plate with good thermal conductivity can be produced.

[0039] By alternately stacking aluminum nitride containing yttrium trioxide and aluminum nitride in which yttrium trioxide is below the detection limit, three or more layers can be stacked.

[0040] Example

[0041] Hereinafter, examples of the present invention will be described. It should be noted that the following examples do not limit the present invention in any way.

[0042] [Example 1]

[0043] 1. Production of circular plate

[0044] Y2O3 powder is added to the AlN raw material powder, mixed by a ball mill to prepare a mixed powder, and the mixed powder is granulated by spray drying. Y2O3 powder is added in a manner of 5 mass % relative to the whole. Next, a disc-shaped molded body is made using the obtained particles. Then, the molded body is hot-pressed to prepare a circular plate as an AlN sintered body. During the hot-pressing sintering, the maximum temperature (sintering temperature) during sintering is set to 1650-1850°C, the holding time at the sintering temperature is set to 2 hours, the pressing pressure is set to 20MPa, and the atmosphere is set to a nitrogen atmosphere.

[0045] 2. Production of cylindrical shaft

[0046] Add Y2O3 powder to AlN raw material powder, mix by ball mill, make mixed powder, and granulate the mixed powder by spray drying. Add Y2O3 powder in a manner that the content in the sintered body is 5% by mass. Next, use the obtained particles to make a molded body. Then, the molded body is sintered at normal pressure to make an AlN sintered body (cylindrical shaft). The maximum temperature during sintering (sintering temperature) is set to 1750-1900°C, the holding time at the sintering temperature is set to 1-5 hours, and the atmosphere is a nitrogen atmosphere.

[0047] 3. Production of the intermediate ring

[0048] MgO powder and TiO2 powder are added to the AlN raw material powder, and the mixture is mixed by a ball mill to prepare a mixed powder, and the mixed powder is granulated by spray drying. MgO powder is added in a manner that the content in the sintered body is 1% by mass, and TiO2 powder is added in a manner that the content in the sintered body is 0.5% by mass. Next, the obtained particles are used to make a molded body. Then, the molded body is hot-pressed to make an AlN sintered body. During the hot-pressing sintering, the maximum temperature during sintering (sintering temperature) is 1750-1850°C, the holding time at the sintering temperature is 1-5 hours, the pressing pressure is 20MPa, and the atmosphere is a nitrogen atmosphere. The center of the sintered plate is hollowed out by machining to make an intermediate ring with a thickness of 3mm. It should be noted that the intermediate ring can be sintered after being formed into a ring shape.

[0049] 4. Fabrication of the joint body

[0050] Prepare the flux (paste for joining) as follows. The paste is made according to the following steps: (a) Mix CaO, Al2O3 and Y2O3 in a total of 100 and a mass ratio of 35-40:42-47:17-22 to obtain a mixed powder, and heat treat the mixed powder at 1330-1390°C to obtain a synthetic powder; (b) Mix the synthetic powder and AlN powder in a mass ratio of 100:60-70, and crush them into an average particle size of less than 30μm to obtain a crushed powder; (c) Knead with ethanol as a solvent. Using a circular plate, a cylindrical shaft, an intermediate ring and a flux, a joint (a plate with a shaft) is made as follows. Image Figure 6 In this way, the circular plate, paste, intermediate ring, paste, and cylindrical shaft are stacked in order from the bottom. The maximum temperature of the joint is 1600-1700°C and the load is 10-40kg / cm 2 It should be noted that a sheet for bonding may be used instead of the flux.

[0051] 5. Evaluation

[0052] The obtained joint body was inspected for defects on the joint surface using an ultrasonic flaw detector. As a result, no defects were confirmed on the joint surface. In addition, the SEM photograph of the joint surface was observed. As a result, no defects were seen on the joint surface, confirming good jointability. The appearance of the joint body was observed. As a result, the circular plate and the cylindrical shaft were white, and the intermediate ring was gray (considered to be the influence of TiO2). In the intermediate ring, a diffusion layer obtained by the diffusion of flux components near the joint surface with the circular plate and the joint surface with the cylindrical shaft was observed. The Y2O3 content of the part other than these diffusion layers was measured using high-frequency inductively coupled plasma emission analysis (ICP-AES9). The result was below the detection limit (below 5 mass ppm). A diffusion layer was seen near the joint surface of the circular plate and the intermediate ring. The Y2O3 content of the part other than the diffusion layer was similarly measured. The result was 5 mass%. A diffusion layer was seen near the joint surface of the cylindrical shaft and the intermediate ring. The Y2O3 content of the part other than the diffusion layer was similarly measured. The result was 5 mass%. The bonding strength was measured by a four-point bending method in accordance with JIS1601 and was 370 MPa.

[0053] [Comparative Example 1]

[0054] The same circular plate and cylindrical shaft as in Example 1 were used to produce a joint body as follows. That is, the same flux as in Example 1 was applied between the circular plate and the cylindrical shaft to perform the joint. The joint was performed at a maximum temperature of 1630°C and a load of 80 kg / cm 2 The obtained bonded body was observed with the naked eye, and cracks were found in the circular plate.

[0055] [Comparative Example 2]

[0056] The same circular plate and cylindrical shaft as in Example 1 were used to produce a joint body as follows. That is, the same flux as in Example 1 was applied between the circular plate and the cylindrical shaft to perform the joint. The joint was performed at a maximum temperature of 1630°C and a load of 40 kg / cm 2 The bonding strength of the obtained bonded body was low, and the SEM observation results confirmed that flux was condensed at the bonding interface.

[0057] It should be noted that in the above-mentioned Example 1, the circular plate containing 5 mass% of yttrium trioxide and the cylindrical shaft containing 5 mass% of yttrium trioxide are joined via an intermediate ring with a low concentration of yttrium trioxide. However, the circular plate containing 5 mass% of yttrium trioxide and the cylindrical shaft with a low concentration of yttrium trioxide can be joined without an intermediate ring.

[0058] Alternatively, a circular plate containing several mass % of yttrium trioxide and a cylindrical shaft containing yttrium trioxide at a concentration lower than that of the circular plate may be joined via an intermediate ring having a lower yttrium trioxide concentration than the circular plate and the cylindrical shaft. In this case, by using an intermediate ring having yttrium trioxide below the detection limit, a stronger joint body can be obtained.

Claims

1. An AlN joint body, wherein: A first AlN member and a second AlN member are bonded to each other, and a third AlN member is bonded to a surface of the first AlN member opposite to a bonding surface of the second AlN member. The AlN joint body is characterized in that: The second AlN component is a circular plate having a wafer placement surface and contains yttrium trioxide. The third AlN component is a cylindrical shaft having a diameter smaller than that of the circular plate, and contains yttrium trioxide. The first AlN member is a ring sandwiched between the circular plate and the cylindrical shaft, and has a yttrium trioxide content below the detection limit.

2. The AlN joint body according to claim 1, characterized in that: The second AlN member has an yttrium trioxide content of 0.07 mass % or more.

3. The AlN joint body according to claim 1 or 2, characterized in that: The first AlN member includes at least one oxide selected from the group consisting of rare earth metal oxides other than yttrium trioxide, magnesium oxide, and titanium dioxide.

4. The AlN joint body according to claim 3, characterized in that: The first AlN component includes magnesium oxide and titanium dioxide.

5. The AlN joint body according to claim 1 or 2, characterized in that: The third AlN member has an yttrium trioxide content of 0.07 mass % or more.

6. An AlN joint body, wherein: A first AlN member and a second AlN member are bonded to each other, and a third AlN member is bonded to a surface of the first AlN member opposite to a bonding surface of the second AlN member. The AlN joint body is characterized in that: The second AlN component is a circular plate having a wafer placement surface and has a second diffusion layer formed by bonding. The third AlN member is a cylindrical shaft having a diameter smaller than that of the circular plate, and has a third diffusion layer formed by bonding. The first AlN member is a ring sandwiched between the circular plate and the cylindrical shaft, and has a first diffusion layer formed by bonding with the second AlN member and another first diffusion layer formed by bonding with the third AlN member. The yttrium trioxide content of the first AlN member except the two first diffusion layers is below the detection limit. The second AlN member contains yttrium trioxide in a portion other than the second diffusion layer. A portion of the third AlN member other than the third diffusion layer contains yttrium trioxide.

7. The AlN joint body according to claim 6, characterized in that: The yttrium trioxide content of the portion of the second AlN member excluding the second diffusion layer is 0.07 mass % or more.

8. The AlN joint body according to claim 6 or 7, characterized in that: The first AlN member includes at least one oxide selected from the group consisting of rare earth metal oxides other than yttrium trioxide, magnesium oxide, and titanium dioxide.

9. The AlN joint body according to claim 8, characterized in that: The first AlN component includes magnesium oxide and titanium dioxide.

10. The AlN joint body according to claim 6 or 7, characterized in that: The yttrium trioxide content of a portion of the third AlN member excluding the third diffusion layer is 0.07 mass % or more.

11. The AlN joint body according to claim 1 or 6, characterized in that: The circular plate has a groove.

Citation Information

Patent Citations

  • Member for a semiconductor manufacturing device, manufacturing method therefor and shaft-equipped heater

    CN106653652A

  • Ceramic bonded body and its producing method, and ceramic structure for semiconductor wafer

    CN1460094A

  • Aluminum nitride sintered compact and its production

    JP1996157261A

  • Bonding agent, aluminum nitride composite body, and manufacturing method of the same

    US20060110624A1