Organic-inorganic hybrid zirconium-based halide scintillator material and preparation method and application thereof

By developing organic-inorganic hybrid zirconium-based halide scintillator material [C7H20N2]2ZrCl8, the problems of poor stability and heavy metal pollution of existing scintillator materials are solved, and efficient X-ray scintillation performance and low-cost industrial production are achieved. in X-ray medical imaging and non-destructive testing.

CN119019260APending Publication Date: 2024-11-26NORTHWEST NORMAL UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411073134.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The scintillator materials used in existing X-ray detectors have problems such as poor stability, low luminous efficiency, afterglow length and heavy metal pollution, which limit their widespread use in medical and industrial applications.

Method used

Develop an organic-inorganic hybrid zirconium-based halide scintillator material [C7H20N2]2ZrCl8, prepared by reacting N,N,2,2 tetramethyl-1,3-propylene diamine with zirconium chloride at low temperature to form The scintillator single crystal and thin film with zero-dimensional lattice structure have high radiation recombination efficiency and good stability.

Benefits of technology

It achieves efficient X-ray scintillation performance, good stability, the emission spectrum is located in the blue light area of ​​485nm, and the PLQY is 13.5%. It overcomes the heavy metal pollution and high energy consumption problems of traditional scintillator materials, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019260A_ABST
    Figure CN119019260A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of scintillation materials, and particularly discloses an organic-inorganic hybrid zirconium-based halide scintillator material, and the chemical formula of the scintillator material is [C7H20N2] 2ZrCl8. The invention also provides a preparation method and application of the scintillator material. The scintillator material does not contain heavy metal, and the scintillator single crystal has a zero-dimensional structure and can realize blue luminescence with high matching degree with photoelectric detectors such as a photomultiplier; the preparation method is simple, the cost is low, large-scale industrial production can be realized, and the scintillator material can be applied to the fields of X-ray medical imaging, nondestructive testing, industrial flaw detection and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of scintillating materials, and in particular relates to an organic-inorganic hybrid zirconium-based halide scintillator material and a preparation method and application thereof. Background Art

[0002] X-rays have strong transmittance and can be used to detect internal information of objects that are invisible to the human eye. They are widely used in medical radiological diagnosis, industrial non-destructive testing, and core components of high-value instruments. Among them, X-ray detectors with scintillators as the mainstream material play a key role in converting invisible X-ray signals into visible light / ultraviolet light signals in the entire detection and imaging process, and are the core components of the entire system's photoelectric conversion. Therefore, the performance of the scintillator material determines the number of converted photons and the signal strength, and plays a decisive role in the performance of the X-ray instrument.

[0003] The energy conversion materials used in commercialized X-ray detectors are mainly bismuth germanate Bi4Ge3O 12 , lutetium yttrium silicate LYSO:Ce, sodium iodide NaI:Tl and cesium iodide CsI:Tl, but each has its own disadvantages, such as easy deliquesce, low luminous efficiency and long afterglow. In recent years, thanks to the vigorous development of lead-based halide perovskites in the field of luminescence, their high efficiency luminescence and high defect tolerance have also attracted wide attention in the field of scintillators. However, they have poor stability and lack of large-area scintillator film preparation technology, which seriously restricts their industrialization process.

[0004] Therefore, the development of high-performance X-ray detection materials with good ionizing radiation stability, strong blocking ability, high energy conversion efficiency, and fast linear response speed has become the foothold for improving the level of detectors. At the same time, it is also necessary to be free of heavy metals, environmentally friendly, and easy to process, which has become an important research direction for new scintillation materials. Summary of the invention

[0005] The first object of the present invention is to overcome the above problems and provide an organic-inorganic hybrid zirconium-based halide scintillator material with good stability and excellent X-ray scintillation performance.

[0006] The second object of the present invention is to provide a method for preparing the above scintillator material.

[0007] The third object of the present invention is to provide applications of the above scintillator material.

[0008] The purpose of the present invention is specifically achieved through the following technical solutions:

[0009] An organic-inorganic hybrid zirconium-based halide scintillator material, the chemical formula of the scintillator material is [C7H20 N2]2ZrCl8.

[0010] The method for preparing the above-mentioned organic-inorganic hybrid zirconium-based halide scintillator material comprises the following steps:

[0011] (1) dissolving N,N,2,2-tetramethyl-1,3-propylenediamine and zirconium chloride, stirring and reacting to obtain a precursor solution;

[0012] (2) filtering the precursor solution obtained in step (1), allowing the filtered precursor solution to stand, and precipitating and growing to obtain a product having a chemical formula of [C7H 20 Organic-inorganic hybrid zirconium-based halide scintillator single crystal of N2]2ZrCl8.

[0013] Furthermore, the method further comprises the following steps:

[0014] (3) washing the scintillator single crystal obtained in step (2) with an organic solvent and then drying it, ball milling it with a ball mill, and then washing the ball-milled scintillator powder with an organic solvent, and drying it to obtain a clean [C7H 20 N2]2ZrCl8 organic-inorganic hybrid zirconium-based halide scintillator powder;

[0015] (4) dissolving the polymer in an organic solvent to obtain a polymer solution;

[0016] (5) The clean scintillator powder obtained in step (3) and the polymer solution obtained in step (4) are mixed and stirred evenly, and the mixed solution is dropped on the substrate and dried to obtain a transparent scintillator film.

[0017] Preferably, in step (1), the molar ratio of N,N,2,2-tetramethyl-1,3-propylenediamine to zirconium chloride is 5:1 to 2:1; the solvent used to dissolve the N,N,2,2-tetramethyl-1,3-propylenediamine and zirconium chloride is a mixture of anhydrous ethanol and concentrated hydrochloric acid, the stirring reaction is carried out at room temperature, and the stirring reaction time is 0.1 to 48 hours; the concentration of zirconium chloride in the precursor solution is 0.1 to 4 mol / L.

[0018] Further preferably, the volume ratio of anhydrous ethanol to concentrated hydrochloric acid in the mixture of anhydrous ethanol and concentrated hydrochloric acid is 5:1 to 20:1.

[0019] Further preferably, in step (2), the precursor solution is allowed to stand for 24 to 120 hours.

[0020] Further preferably, in step (3), the organic solvent used to wash the scintillator single crystal and scintillator powder is one or a mixture of two or more of dimethyl sulfoxide, N,N-dimethylformamide, n-hexane and anhydrous ethanol; and the ball milling is performed at 200 to 2000 rpm for 0.15 to 2 h.

[0021] Further preferably, in step (4), the polymer is polystyrene, polyvinylidene fluoride or polymethyl methacrylate, and the organic solvent used to dissolve the polymer is toluene.

[0022] Further preferably, in step (5), the mass ratio of the clean scintillator powder obtained in step (3) to the polymer in step (4) is 3:5.

[0023] The above organic-inorganic hybrid zirconium-based halide scintillator materials are used in X-ray medical imaging, non-destructive testing, and industrial flaw detection.

[0024] Compared with the prior art, the present invention has the following advantages:

[0025] (1) The present invention provides an organic-inorganic hybrid zirconium-based halide scintillator material having a zero-dimensional lattice structure, wherein the zirconium halide clusters are surrounded by organic cations [C7H 20 N2] 2+ The encapsulation forms a zero-dimensional structure, and the self-trapped excitons generated by light excitation have high radiative recombination efficiency, large Stokes shift, small self-absorption, and its emission spectrum is located in the blue light region of 485nm, with a PLQY of 13.5%;

[0026] (2) The scintillator material of the present invention has good stability and excellent X-ray scintillation performance. The synthesis process can be carried out at room temperature, which is energy-saving and environmentally friendly. The scintillation intensity of the compound is about 44.6% of that of CsI(Tl), and the light yield is 17859 phMeV -1 , and overcomes the shortcomings of heavy metal pollution and high industrial energy consumption in traditional commercial scintillators, and has important commercial application value in the field of scintillating materials;

[0027] (3) The present application provides an X-ray detection and imaging display material, the compound [C7H 20 N2]2ZrCl8 scintillator film has high-performance X-ray detection capability, which can further improve the spatial resolution of imaging display devices, which is crucial for high-quality imaging and has important commercial application value in the field of high-energy particle detection and imaging display materials;

[0028] (4) The preparation method of the scintillator material is simple, and the obtained material has high purity, good crystallinity and high yield, which is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The zirconium-based halide scintillator single crystal [C7H 20 The luminescence of N2]2ZrCl8 under visible light, 254nm ultraviolet light and X-ray excitation; Figure 1 a corresponds to visible light excitation, Figure 1 b corresponds to 254nm ultraviolet light excitation, Figure 1 c corresponds to X-ray excitation;

[0030] Figure 2 The zirconium-based halide scintillating single crystal [C7H 20 Schematic diagram of the crystal structure of N2]2ZrCl8 (the lattice structure is obtained by collecting data from SC-XRD and then single crystal analysis using Olex2 software);

[0031] Figure 3 The zirconium-based halide scintillating single crystal [C7H 20 Simulated XRD of N2]2ZrCl8 (corresponding to Figure 3 The theoretical value in) and the test XRD spectrum (corresponding to Figure 3 Experimental value in) (simulated XRD spectrum is made according to CIF card obtained by single crystal structure analysis, and test XRD is obtained by grinding single crystal into powder test PowderXRD);

[0032] Figure 4 The zirconium-based halide scintillator single crystal [C7H 20 The emission spectrum PL and excitation spectrum PLE diagram of N2]2ZrCl8, including the optimal excitation wavelength and the optimal emission wavelength;

[0033] Figure 5 The zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8 fluorescence quantum efficiency;

[0034] Figure 6 The zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8 time-resolved fluorescence spectrum TRPL;

[0035] Figure 7 The zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8 thermogravimetric-differential thermal spectrum;

[0036] Figure 8 This is a scanning electron microscope (SEM) image of the zirconium-based halide scintillator prepared in Example 1, which was ground into powder using a ball mill;

[0037] Fig. 9 This is a real picture of the zirconium-based halide scintillator transparent film prepared in Example 7 under visible light;

[0038] Fig.10 The X-ray scintillation luminescence spectrum of the zirconium-based halide scintillator single crystal prepared in Example 1 is compared with that of the cesium iodide-doped thallium CsI:Tl wafer;

[0039] Fig.11 is the minimum detection limit of X-ray dose detection of the zirconium-based halide scintillator film prepared in Example 7;

[0040] Fig.12 The zirconium-based halide scintillator transparent film prepared in Example 7 is applied to high-resolution X-ray imaging, and the corresponding imaging objects are Fig.12 a. X-ray imaging of imaging objects Fig.12 b;

[0041] Fig.13 The actual image of the zirconium-based halide scintillator transparent film prepared in Example 7 on the metal product and the corresponding X-ray imaging image, wherein: Fig.13 a is a physical picture of a metal product with a ruler. Fig.13 b is the X-ray imaging of metal products;

[0042] Fig.14 This is an imaging diagram of the zirconium-based halide scintillator transparent film prepared in Example 7 on a standard lead plate and its partial enlarged diagram. DETAILED DESCRIPTION

[0043] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0044] The organic-inorganic hybrid zirconium-based halide scintillator of the present invention is a high-efficiency zirconium-based halide scintillator material, and its chemical formula is [C7H 20 N2]2ZrCl8.

[0045] The preparation of the organic-inorganic hybrid zirconium-based halide scintillator material in the present invention can adopt a low-cost low-temperature solution process, taking the preparation of scintillator single crystals and powders and the preparation of transparent scintillator films as examples, wherein:

[0046] Generally speaking, the preparation method of scintillator single crystal is to slowly volatilize the saturated solution of the precursor and allow the compound to crystallize and grow to obtain a high-efficiency zirconium-based halide single crystal scintillator. Specifically, the following steps are included:

[0047] (1) adding N,N,2,2-tetramethyl-1,3-propylenediamine solution and zirconium chloride powder in a molar ratio of 5:1 to 2:1 to a mixture of anhydrous ethanol and concentrated hydrochloric acid, wherein the volume ratio of anhydrous ethanol to concentrated hydrochloric acid is 5:1 to 20:1, stirring and reacting at room temperature to obtain a clear precursor solution, the stirring time is 0.1 to 48 hours, and the concentration of zirconium chloride in the precursor solution is 0.1 to 4 mol / L;

[0048] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0049] (3) The filtered precursor solution obtained in step (2) was allowed to stand in a glove box for 24 to 120 hours to obtain an organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8 will precipitate and grow;

[0050] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with an organic solvent and naturally dried to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8, the organic solvent used for washing can be one of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), n-hexane, anhydrous ethanol, or a mixed solvent of two or more of the above solutions in any proportion;

[0051] The method for preparing a scintillator thin film specifically comprises the following steps:

[0052] (5) The zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8 was placed in a ball mill and milled at 200-2000 rpm for 0.15-2h;

[0053] (6) The organic-inorganic hybrid zirconium-based halide scintillator powder obtained in step (5) is rinsed with an organic solvent and dried naturally to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator powder [C7H 20 N2]2ZrCl8, the organic solvent used for washing can be one of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), n-hexane, anhydrous ethanol, or a mixed solvent of two or more of the above solutions in any proportion;

[0054] (7) dissolving a polymer (such as polystyrene PS, polyvinylidene fluoride PVDF or polymethyl methacrylate PMMA) in an organic solvent, wherein the organic solvent is toluene;

[0055] (8) The organic-inorganic hybrid zirconium-based halide scintillator powder [C7H 20 N2]2ZrCl8 is mixed and stirred evenly with the polymer solution obtained in step (7), and then drop-coated onto a smooth substrate. The substrate is then placed in a glove box and dried naturally until the solvent evaporates to obtain a scintillator film.

[0056] Unless otherwise specified, the raw materials in the examples of the present invention were purchased through commercial channels, among which N,N,2,2-tetramethyl-1,3-propylenediamine and zirconium chloride were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; toluene and 37wt% concentrated hydrochloric acid were purchased from Sinopharm Group, dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), n-hexane and anhydrous ethanol were purchased from Lianlong Bohua (Tianjin) Pharmaceutical Chemical Co., Ltd., and polystyrene (PS) and polymethyl methacrylate (PMMA) were purchased from Thermo Fisher Scientific (China) Co., Ltd.

[0057] Example 1

[0058] [C7H 20 N2]2ZrCl8 scintillator single crystal and its preparation

[0059] (1) Weighing 10 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 50 mL of anhydrous ethanol and 5 mL of concentrated hydrochloric acid, stirring at room temperature of 25° C. for 1 h to fully react, and obtaining a clear precursor solution;

[0060] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0061] (3) The filtered precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0062] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with anhydrous ethanol and naturally dried to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8.

[0063] Example 2

[0064] [C7H 20 N2]2ZrCl8 scintillator single crystal and its preparation

[0065] (1) Weighing 10 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 50 mL of anhydrous ethanol and 5 mL of concentrated hydrochloric acid, stirring at room temperature of 25° C. for 1 h to fully react, and obtaining a clear precursor solution;

[0066] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0067] (3) The filtered precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0068] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with n-hexane and naturally dried to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8.

[0069] Example 3

[0070] [C7H 20 N2]2ZrCl8 scintillator single crystal and its preparation

[0071] (1) Weighing 10 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 50 mL of anhydrous ethanol and 5 mL of concentrated hydrochloric acid, stirring at room temperature of 25° C. for 1 h to fully react, and obtaining a clear precursor solution;

[0072] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0073] (3) The filtered precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0074] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with DMF and naturally dried to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8.

[0075] Example 4

[0076] [C7H 20N2]2ZrCl8 scintillator single crystal and its preparation

[0077] (1) Weighing 10 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 50 mL of anhydrous ethanol and 5 mL of concentrated hydrochloric acid, stirring at room temperature of 25° C. for 1 h to fully react, and obtaining a clear precursor solution;

[0078] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0079] (3) The filtered precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0080] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with DMSO and naturally dried to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8.

[0081] Example 5

[0082] [C7H 20 N2]2ZrCl8 scintillator single crystal and its preparation

[0083] (1) Weighing 20 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 50 mL of anhydrous ethanol and 5 mL of concentrated hydrochloric acid, stirring at room temperature of 25°C for 1 hour to fully react, and obtaining a clear precursor solution;

[0084] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0085] (3) The precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0086] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with anhydrous ethanol and naturally dried to obtain a clean zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8.

[0087] Example 6

[0088] [C7H 20 N2]2ZrCl8 scintillator single crystal and its preparation

[0089] (1) Weighing 10 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 100 mL of anhydrous ethanol and 10 mL of concentrated hydrochloric acid, stirring at room temperature of 25° C. for 1 h to fully react, and obtaining a clear precursor solution;

[0090] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0091] (3) The filtered precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0092] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with anhydrous ethanol and naturally dried to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8.

[0093] Example 7

[0094] [C7H 20 N2]2ZrCl8 scintillator thin film and its preparation

[0095] (1) Weighing 10 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 100 mL of anhydrous ethanol and 10 mL of concentrated hydrochloric acid, stirring at room temperature of 25° C. for 1 h to fully react, and obtaining a clear precursor solution;

[0096] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0097] (3) The filtered precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0098] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with anhydrous ethanol and naturally dried to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8;

[0099] (5) the organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8 was placed in a ball mill and milled at 300 rpm for 1 h;

[0100] (6) The organic-inorganic hybrid zirconium-based halide scintillator powder obtained in step (5) is rinsed with anhydrous ethanol and dried naturally to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator powder [C7H 20 N2]2ZrCl8;

[0101] (7) Dissolve 5 g of polystyrene in 20 mL of toluene solvent;

[0102] (8) The zirconium-based halide scintillator powder [C7H 20 Weigh 3 g of N2]2ZrCl8 and mix it with the polymer solution obtained in step (7) and stir it evenly. Then use a pipette to take 540 μL of the mixed liquid and drop it onto a smooth 2.45 cm*2.45 cm glass substrate. Then put the substrate into a glove box and dry it naturally until the solvent evaporates to obtain a scintillator film.

[0103] Example 8

[0104] [C7H 20 N2]2ZrCl8 scintillator thin film and its preparation

[0105] (1) Weighing 10 mmol of N,N,2,2-tetramethyl-1,3-propylenediamine solution and 5 mmol of zirconium chloride powder in a molar ratio respectively, adding them to a mixed solution of 100 mL of anhydrous ethanol and 10 mL of concentrated hydrochloric acid, stirring at room temperature of 25° C. for 1 h to fully react, and obtaining a clear precursor solution;

[0106] (2) filtering the precursor solution obtained in step (1) into a glass bottle using a filter head, and placing the glass bottle in a glove box;

[0107] (3) The filtered precursor solution obtained in step (2) is allowed to stand in a glove box for 120 hours, and an organic-inorganic hybrid zirconium-based halide scintillator single crystal will precipitate and grow;

[0108] (4) The organic-inorganic hybrid zirconium-based halide scintillator single crystal obtained in step (3) is rinsed with anhydrous ethanol and naturally dried to obtain a clean zirconium-based halide scintillator single crystal [C7H 20 N2]2ZrCl8;

[0109] (5) the organic-inorganic hybrid zirconium-based halide scintillator single crystal [C7H 20N2]2ZrCl8 was placed in a ball mill and milled at 300 rpm for 1 h;

[0110] (6) The organic-inorganic hybrid zirconium-based halide scintillator powder obtained in step (5) is rinsed with anhydrous ethanol and dried naturally to obtain a clean organic-inorganic hybrid zirconium-based halide scintillator powder [C7H 20 N2]2ZrCl8;

[0111] (7) Dissolve 5 g of polymethyl methacrylate in 20 mL of toluene solvent;

[0112] (8) Weigh 3 g of the organic-inorganic hybrid zirconium-based halide scintillator powder [C7H20N2]2ZrCl8 obtained in step (6), mix it with the polymer solution obtained in step (7), and stir it evenly. Then, use a pipette to take 540 μL of the mixed liquid and drop it onto a smooth 2.45 cm*2.45 cm glass substrate. Then, put the substrate into a glove box and dry it naturally until the solvent evaporates to obtain a scintillator film.

[0113] Structural characterization of the sample of test example 1

[0114] The X-ray single crystal diffraction of the sample in Example 1 was carried out on a Bruker D8VENTURE X-ray single crystal diffractometer from Bruker, Germany, with a light source of micro-focus Mo / Cu light source and a test temperature of 293K, and the structure was analyzed using the deconstruction software Olex. The test results are shown in Figure 1. Figure 2 As shown, Zr has a six-coordinate distorted octahedral geometry, where the Zr-Cl1 bond length is The Zr-Cl2 bond length is 2.4412(17), and the Zr-Cl3 bond length is 2.4443(15). With Zr as the center, the Cl3A-ZrB-Cl1C bond angle is 90.82(6), the Cl2A-ZrB-Cl3C bond angle is 91.77(7), and the Cl2A-ZrB-Cl1C bond angle is 92.34(7), all of which are within the normal numerical range, where A is the symmetry operation code 1-x, 2-y, 1-z, B is x, y, z, and C is 1-x, 2-y, 1-z.

[0115] The X-ray powder diffraction phase analysis (XRD) of the ground samples was performed on a Bruker D8Advance X-RAY small-angle powder diffractometer from Bruker, Germany, using a Cu target. The test results are shown in Figure 3 The XRD diffraction theoretical pattern obtained by X-ray single crystal diffraction fitting is compared with the XRD diffraction pattern measured by X-ray powder diffraction phase analysis. Figure 3As shown, it can be seen that the XRD diffraction pattern obtained by fitting the single crystal data is highly consistent with the XRD diffraction pattern measured experimentally, proving that the obtained sample is a sample of high purity and high crystallinity.

[0116] X-ray powder diffraction (corresponding to Figure 3 Experimental value) and X-ray single crystal diffraction (corresponding to Figure 3 Theoretical value) results show that:

[0117] The crystal structure of the scintillator material belongs to the triclinic system and has a P1 space group structure;

[0118] The unit cell constant of the scintillating material α=107.579(6)°, β=90.435(6)°, γ=102.734(7)°,

[0119] Thermal stability test experiment of sample in Example 1

[0120] The thermal stability of the samples was measured by TGA4000 of PE Company in the United States in air atmosphere. Figure 7 As shown in the figure, the sample has good thermal stability and still maintains structural integrity at 170°C.

[0121] Photoluminescence and fluorescence lifetime test experiment of the sample in Example 1

[0122] The photoluminescence performance of the sample was measured by the Edinburgh FS5 integrated steady-state transient fluorescence spectrometer of the Edinburgh company in the UK. The excitation light source is a Xe lamp, and the ultraviolet light of a specific excitation band can be selected through the filtering system. The excitation slit is 1.5m and the receiving slit is 1.5mm. The experimental spectrum of photoluminescence is shown in Figure 4 As shown. Under the optimal wavelength excitation of ultraviolet light 249nm, it shows 484nm blue light emission; The experimental spectrum of fluorescence lifetime is shown in Figure 6 As shown, the excitation light source used is a μF2 microsecond pulsed xenon lamp, and under the optimal wavelength excitation of ultraviolet light 249nm, it shows a fluorescence lifetime of 5.916μs. The fitting model used in calculating the fluorescence lifetime is ExpDec3, and the fitting coefficient of determination (COD) is 0.9999.

[0123] Quantum efficiency experiment of sample in Example 1

[0124] The quantum efficiency (PLQY) of the sample was obtained using a fluorescence spectrometer (FLS-1000) from Edinburgh, UK, equipped with a Xe lamp. The excitation light source was 249 nm. The calculation formula for PLQY is: QE =I S / (ER -E S ), where I S is the luminescence emission spectrum of the sample, E R is the excitation light spectrum from an empty integrating sphere (without sample), E S is the excitation spectrum of the sample. Figure 5 As shown, the fluorescence efficiency quantum efficiency PLQY is 13.5%.

[0125] Field emission scanning electron microscope (SEM) experiment of the sample of Example 1

[0126] Field emission scanning electron microscopy (SEM) images of the samples were taken using a Thermo Fisher Apreo 2C field emission scanning electron microscope from Thermo Fisher Scientific (China) Co., Ltd. Figure 8 This is a scanning electron microscope image of the powder obtained after ball milling of the crystal obtained in Example 1.

[0127] Example 7 X-ray scintillation performance test experiment of the sample

[0128] The X-ray scintillation performance of the sample was measured by the photodetector spectral response measurement system HVC 1800 of Beijing Zhuoli Hanguang Instrument Co., Ltd. The X-ray source used was the Monoblock ray source of Moxtek (USA).

[0129] The experimental spectrum of X-ray scintillation performance is shown in Fig.10 As shown, the scintillation luminescence of the sample is also at 484 nm.

[0130] Comparative experimental spectra of scintillation performance are shown in Fig.10 When the tube voltage of the X-ray tube is 70 kV, the tube current of the X-ray tube is 170 mA, and the distance between the sample and the X-ray tube is 5 cm, it can be seen that under the same test conditions, the scintillation intensity of the sample is about 0.446 times that of the CsI:Tl wafer (the scintillation intensity of the sample is about 44.6% of that of CsI(Tl)), and the light output is 17859 ph MeV. -1 (The specific value is obtained by comparing the integrated areas. The default light yield of CsI(Tl) is 40,000, and the light yield of the sample is 40,000*44.6%=17,859.) The performance of the scintillating material of the present invention is comparable to that of commercial scintillating materials, but the synthesis is cheaper, which has great advantages.

[0131] Experimental testing of X-ray doses Fig.11As shown, the X-ray dose can be achieved by fixing the tube voltage of the X-ray tube and changing the tube current of the X-ray tube. The actual detected dose is calibrated by the RAMION radiation dosimeter. The detection limit is also an important parameter of the X-ray detector, which determines the minimum detection dose of the X-ray detector. The International Union of Applied Chemistry (IU-PAC) defines the detection limit as the equivalent dose rate that produces a signal greater than 3 times the noise level (signal-to-noise ratio [SNR] = 3). Therefore, the detection limit of the sample can be calculated to be 3.627μGy air / s, lower than the conventional medical diagnostic dose standard of 5.50μGy air / s. This shows that the sample has sensitive X-ray detection capability.

[0132] Imaging experiment Experimental method: The scintillator film prepared in Example 7 is placed close to the imaging object, the X-ray source is placed at the far end of the object side, and the image of the scintillator side is taken with a digital camera. The results are as follows Fig.12 , 13 , as shown in 14. Fig.12 , 13 , 14 respectively give the imaging pictures of three kinds of objects: capsule inner spring, metal pattern and standard lead plate. Fig.14 It can be seen that at 16 line pairs per millimeter (lp / mm), the image is still clear.

[0133] The scintillator material of the present invention is a compound [C7H 20 N2]2ZrCl8, through the introduction of organic cations to achieve the zero-dimensional structure of zirconium-based halide clusters, complete the preparation of organic-inorganic hybrid zirconium-based halide scintillator single crystals and powders, and then achieve high-efficiency blue light emission with a quantum efficiency of 13.5% and a fluorescence lifetime of 5.916μs. Compared with the prior art, it can effectively expand the types of single crystal scintillators and achieve blue light emission with a high degree of matching with photomultiplier tubes and other photodetectors. In addition, the preparation process of the present invention is simple, low-cost, does not contain heavy metals, is green and pollution-free, and can achieve large-scale industrial production; [ZrCl6] 2- The octahedral spatial coordination configuration of [C7H 20 N2] 2+ and Cl - Spatial isolation forms a zero-dimensional structure in the molecular structure. The electron-hole pairs generated by light excitation are localized in the zirconium-halide octahedral clusters, which has a high radiation recombination efficiency. At the same time, the Stokes shift is large, which makes the self-absorption small. The organic-inorganic hybrid zirconium-based halide scintillator composite polymer transparent film of the present invention has a scintillation intensity of about 0.446 times that of the CsI:Tl wafer, and the minimum detection limit is 3.627μGy air / s, and the imaging resolution is about 16lp / mm, which can be effectively applied to X-ray medical imaging, nondestructive testing, industrial flaw detection and other fields. The scintillator screen prepared by the composite of scintillator and polymer based on the present invention can be applied to high-resolution imaging.

[0134] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An organic-inorganic hybrid zirconium-based halide scintillator material, characterized in that: The chemical formula of the scintillator material is [C7H 20 N2]2ZrCl8.

2. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 1, characterized in that: The method comprises the following steps: (1) dissolving N,N,2,2-tetramethyl-1,3-propylenediamine and zirconium chloride, stirring and reacting to obtain a precursor solution; (2) filtering the precursor solution obtained in step (1), allowing the filtered precursor solution to stand, and precipitating and growing to obtain a product having a chemical formula of [C7H 20 Organic-inorganic hybrid zirconium-based halide scintillator single crystal of N2]2ZrCl8.

3. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 2, characterized in that: The method further comprises the steps of: (3) washing the scintillator single crystal obtained in step (2) with an organic solvent and then drying it, ball milling it with a ball mill, and then washing the ball-milled scintillator powder with an organic solvent, and drying it to obtain a clean [C7H 20 N2]2ZrCl8 organic-inorganic hybrid zirconium-based halide scintillator powder; (4) dissolving the polymer in an organic solvent to obtain a polymer solution; (5) The clean scintillator powder obtained in step (3) and the polymer solution obtained in step (4) are mixed and stirred evenly, and the mixed solution is dropped onto a substrate and dried to obtain a transparent scintillator film.

4. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 3, characterized in that: In step (1), the molar ratio of N,N,2,2-tetramethyl-1,3-propylenediamine to zirconium chloride is 5:1 to 2:1; the solvent used to dissolve the N,N,2,2-tetramethyl-1,3-propylenediamine and zirconium chloride is a mixed solution of anhydrous ethanol and concentrated hydrochloric acid, the stirring reaction is carried out at room temperature, and the stirring reaction time is 0.1 to 48 hours; the concentration of zirconium chloride in the precursor solution is 0.1 to 4 mol / L.

5. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 4, characterized in that: The volume ratio of anhydrous ethanol to concentrated hydrochloric acid in the mixed solution of anhydrous ethanol and concentrated hydrochloric acid is 5:1 to 20:

1.

6. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 4, characterized in that: In step (2), the precursor solution is allowed to stand for 24 to 120 hours.

7. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 6, characterized in that: In step (3), the organic solvent used to wash the scintillator single crystal and the scintillator powder is one or a mixture of two or more of dimethyl sulfoxide, N,N-dimethylformamide, n-hexane and anhydrous ethanol; the ball milling is performed at 200 to 2000 rpm for 0.15 to 2 hours.

8. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 7, characterized in that: In step (4), the polymer is polystyrene, polyvinylidene fluoride or polymethyl methacrylate, and the organic solvent used to dissolve the polymer is toluene.

9. The method for preparing the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 8, characterized in that: In step (5), the mass ratio of the clean scintillator powder obtained in step (3) to the polymer in step (4) is 3:

5.

10. Use of the organic-inorganic hybrid zirconium-based halide scintillator material according to claim 1 in X-ray medical imaging, nondestructive testing, and industrial flaw detection.

Citation Information

Cited By

  • Two-dimensional organic-inorganic hybrid lead-based halide scintillation single crystal and preparation method and application thereof

    CN119221130A

  • Metal cation doped zero-dimensional organic-inorganic hybrid zinc-based halide scintillator materials, methods of making and applications thereof