Novel degradable bio-based polyester elastomer and preparation method thereof

Itaconic acid cross-linked polysebasic acid glyceryl ester bioelastomer is prepared by melt polycondensation method using glycerol, sebacic acid and itaconic acid, and the problems of complexity and biocompatibility of the PGS cross-linking process in the prior art are solved, and the problem of achieving the The effect of simplifying the process, improving mechanical properties and antibacterial properties is achieved.

CN119019666APending Publication Date: 2024-11-26EAST CHINA UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411489604.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the crosslinking process of polysebasic glyceryl (PGS) materials is complex and the conditions are harsh, resulting in high equipment requirements and high preparation costs. The crosslinking agent introduced by modification will destroy its biocompatibility, which limits the Its application in the field of bioengineering.

Method used

Itaconic acid crosslinked polysebasic acid glyceryl ester bioelastomer is prepared by melt polycondensation method, simplifying the process flow, improving mechanical properties and imparting antibacterial properties without Solvent and high temperature and high vacuum conditions.

Benefits of technology

The biocompatibility and mechanical properties of polysebasic acid glyceride have been improved, the preparation process is simplified, the equipment requirements and costs are reduced, and antibacteriality is given, meeting the customized needs of different mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019666A_ABST
    Figure CN119019666A_ABST
Patent Text Reader

Abstract

The invention discloses a novel degradable bio-based polyester elastomer and a preparation method thereof, and the preparation method comprises the following steps: under the protection of inert gas, proportionally placing glycerol and sebacic acid in a container, controlling the temperature and the stirring rotating speed for reaction, reducing the vacuum degree of the system, continuing the reaction to obtain an oligomer, proportionally mixing the oligomer with itaconic acid, and performing vacuum drying to obtain the novel degradable bio-based polyester elastomer. Controlling the temperature and the stirring rotating speed to react, adding a catalyst, uniformly mixing, transferring into a polytetrafluoroethylene mold, and continuously reacting under a vacuum condition to obtain the itaconic acid cross-linked polysebacic acid glyceride bioelastomer. According to the preparation method of the novel degradable bio-based polyester elastomer, experimental operation is simple, the requirement for devices and equipment is low, a product is formed in one step, follow-up treatment and processing are not needed, and a new way is provided for cross-linking modification of polysebacic diglyceride; the molecular structure of the prepared novel degradable bio-based polyester elastomer is high in designability, and the introduction of itaconic acid can endow the polysebacic acid glyceride with antibacterial property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biodegradable materials, and in particular to a novel degradable bio-based polyester elastomer and a preparation method thereof. Background Art

[0002] Among many synthetic biodegradable polymer materials, polyglycerol sebacate (PGS) has attracted wide attention due to its good elasticity, biocompatibility and degradability. PGS is a three-dimensional network elastomer prepared by melt polycondensation of bio-based monomers glycerol and sebacic acid. It first forms a prepolymer (pre-PGS) through a polycondensation reaction between -OH and -COOH groups, and then further cures under high temperature vacuum conditions to form a cross-linked thermosetting elastomer.

[0003] By changing the process parameters of prepolymerization and curing, the molecular structure and performance of PGS can be regulated to meet different application requirements. However, due to the harsh reaction conditions for the synthesis of PGS materials, such as the high temperature, high vacuum, and long duration required for the curing reaction, and the shortcomings of PGS such as insufficient hydrophilicity and poor toughness, its application is limited to a certain extent. In recent years, researchers have modified the hydroxyl groups in the prepolymer, or introduced cross-linking agents, and then cured them, which can improve the curing reaction conditions and enhance the performance of PGS to a certain extent. At the same time, the introduction of specific functional groups has also given PGS more functionality, which can effectively broaden its application range.

[0004] Prior art CN110078880A discloses an isocyanate-crosslinked polyethylene glycol-polyisocyanate-crosslinked polyethylene glycol-polyglycerol sebacate bioelastomer and a preparation method and application thereof. The specific method is to react a polyethylene glycol-polyglycerol sebacate prepolymer with hexamethylene diisocyanate in a solvent to obtain an elastomer material. The preparation conditions of the bioelastomer are relatively mild, but when crosslinking the prepolymer, the prepolymer needs to be dissolved in an organic solvent, such as N,N-dimethylamide, tetrahydrofuran, etc., with a minimum concentration of 0.01 g / ml. The organic solvent consumption is huge and has strong environmental hazards. At the same time, the residual organic solvent in the product is likely to reduce the biocompatibility of the product, hindering its application in the field of bioengineering.

[0005] Prior art CN112584822A discloses a urethane elastomer for controlled release in implantable products, which can load active pharmaceutical ingredients. The elastomer is prepared by cross-linking polyglycerol sebacate prepolymer with isocyanate under vacuum, ultrasound and other conditions. The prepolymer reaction time is as long as 50 hours. All components need to be dried and dehydrated before the subsequent cross-linking reaction. The reaction conditions are harsh and the preparation cycle is long.

[0006] Prior art US20130231412 discloses a carbamate cross-linked biodegradable elastomer, which can be used in surgical glue, cell encapsulation and proliferation, medical devices and other tissue engineering. The elastomer is prepared by cross-linking a glyceryl sebacate prepolymer with an isocyanate cross-linking agent using N,N-dimethylamide as a solvent, an organic metal compound and a tertiary amine compound as a catalyst. The subsequent solvent removal takes 3 to 5 days, and the solvent and catalyst are highly toxic, making solvent removal difficult.

[0007] At present, the research on cross-linking modification of PGS mainly includes thermal cross-linking modification of isocyanate cross-linkers and photo-cross-linking modification of acrylate cross-linkers. These processes will face the problems of complex process, harsh reaction conditions, high equipment requirements and high preparation costs. At the same time, the cross-linking agents introduced by the modification will cause certain damage to the biocompatibility of PGS.

[0008] Therefore, in response to the above problems, the present invention provides a novel biodegradable all-biobased polyester elastomer and a preparation method thereof, which effectively simplifies the preparation process of PGS elastomer, improves its mechanical properties and imparts its antibacterial properties while maintaining the good biocompatibility of polysebacic acid glyceryl ester, and realizes the customization of polysebacic acid glyceryl ester-based polymers with different mechanical properties through the design and regulation of the molecular structure of the material. Summary of the invention

[0009] The purpose of the present invention is to provide a novel biodegradable bio-based polyester elastomer and a preparation method thereof. The prepared elastomer has a designable molecular structure and controllable molecular weight, has good biocompatibility and antibacterial properties, and has adjustable mechanical properties; the elastomer preparation process is simple, the preparation process is green and safe, and has low equipment requirements.

[0010] The purpose of the present invention is achieved through the following technical solutions: A novel biodegradable bio-based polyester elastomer, using glycerol, sebacic acid and itaconic acid as reactive monomers, comprising the following structural units: (I); Wherein, n is an integer from 1 to 6; R1 is selected from or or The residues of R2 is selected from or of residues.

[0011] Preferably, the novel biodegradable bio-based polyester elastomer has the following characteristics: (1) Young's modulus is 0.95~24.94MPa; (2) Tensile strength is 0.48~7.82MPa; (3) Elongation at break is 50~120%; (4) Water contact angle is 47.9~88.0 degrees; (5) The mass loss after 7 days of degradation was 4.26~34.88%; (6) Sol content is 3.7~14.0%; (7) Mass swelling degree is 30.5~107.1%; (8) Glass transition temperature is -5.3~-19.8℃; (9) The antibacterial rate was 21.48~53.76%.

[0012] Preferably, the novel biodegradable bio-based polyester elastomer is itaconic acid cross-linked polyglyceryl sebacate bioelastomer.

[0013] Preferably, the novel biodegradable bio-based polyester elastomer can be prepared into a three-dimensional structured elastomer of any shape through different molds, and has sufficiently good mechanical properties to maintain its shape.

[0014] A method for preparing a novel biodegradable bio-based polyester elastomer comprises the following steps: S1. Esterification reaction to generate oligomers: under the protection of inert gas, glycerol and sebacic acid are placed in a container in proportion, the temperature and stirring speed are controlled to react, and then the vacuum degree of the system is reduced to continue the reaction to obtain the oligomer pre-PGS; S2. Preparation of itaconic acid cross-linked polyglyceryl sebacate bioelastomer: Under the protection of inert gas, the oligomer pre-PGS obtained in step S1 and itaconic acid are mixed in proportion, the temperature and stirring speed are controlled to react, a catalyst is added and the mixture is evenly mixed, and then the mixture is transferred to a polytetrafluoroethylene mold, and the reaction is continued under vacuum conditions to obtain itaconic acid cross-linked polyglyceryl sebacate bioelastomer (PGSIA).

[0015] Preferably, in step S1, the glycerol and the sebacic acid are placed in a container at a molar ratio of 0.5 to 1.33; the molar ratio is more preferably 1 or 1.33.

[0016] Preferably, in step S2, the itaconic acid and the oligomer pre-PGS are mixed at a molar ratio of 0.25-1; the molar ratio is more preferably 0.5-1.

[0017] Preferably, in step S2, the catalyst is an organic peroxide, and the peroxide initiator is selected from at least one of dicumyl peroxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

[0018] Preferably, the mass of the catalyst in step S2 is 3% to 7% of the total mass of the oligomer pre-PGS and the itaconic acid; more preferably 3% to 5%.

[0019] Preferably, in step S1, the temperature is controlled to be 120-160° C. for reaction for 4-8 hours, then the vacuum degree of the system is reduced to 50-250 Pa and the reaction is continued for 8-16 hours, and the stirring speed is controlled to be 100-900 rpm.

[0020] Further preferably, in step S1, the temperature is controlled at 140-160° C. for reaction for 4-8 hours, then the vacuum degree of the system is reduced to 100-200 Pa and the reaction is continued for 8-16 hours, and the stirring speed is controlled at 400-500 rpm.

[0021] Preferably, in step S2, the temperature is controlled to be 110-140° C. for the reaction to proceed for 1-4 hours, the reaction is continued under vacuum conditions for 11-23 hours, the vacuum degree of the vacuum conditions is 1000-2000 Pa, and the stirring speed is controlled to be 50-500 rpm.

[0022] Further preferably, in step S2, the temperature is controlled to be 120-130° C. for the reaction for 1-4 hours, the reaction is continued for 11-23 hours under vacuum conditions, the vacuum degree of the vacuum conditions is 1000-1500 Pa, and the stirring speed is controlled to be 150-250 rpm.

[0023] Preferably, in step S1, the inert gas is nitrogen, the nitrogen is introduced for 1 to 8 hours, and the flow rate of nitrogen is 10 to 50 ml / min; more preferably, the nitrogen is introduced for 4 to 6 hours, and the flow rate of nitrogen is 10 to 30 ml / min.

[0024] Preferably, the oligomer pre-PGS has the following characteristics: (1) Intrinsic viscosity is 0.07~0.32dL / g; (2) Acid value is 0.05~0.18g / g; (3) The number average molecular weight is 600~3500g / mol, and the polydispersity coefficient is 2.1~7.3; (4) The hydroxyl content is 15%~50%.

[0025] Preferably, in step S2, the inert gas is nitrogen, the nitrogen is introduced for 1 to 4 hours, and the flow rate of nitrogen is 10 to 50 ml / min; more preferably, the nitrogen is introduced for 2 to 3 hours, and the flow rate of nitrogen is 10 to 30 ml / min.

[0026] Preferably, in step S2, the oligomer pre-PGS and itaconic acid are mixed in proportion, and after the temperature and stirring speed are controlled to react, the catalyst is added and the mixture is uniformly mixed, which is marked by the absence of stratification in the mixture.

[0027] The application also claims the use of a novel degradable bio-based polyester elastomer in tissue engineering, drug delivery, wound dressing or bioelectronics.

[0028] PGS is a three-dimensional mesh elastomer prepared by melt polycondensation of bio-based monomers glycerol and sebacic acid. Compared with other biodegradable polymer materials, PGS can be degraded and absorbed in the body, and can promote cell proliferation and adhesion. Since its introduction, it has been proven to be used in many biomedical applications. Its uses mainly include supporting, enhancing or replacing damaged tissues to achieve or accelerate tissue regeneration and promote tissue recovery of physiological functions; the main application areas include: tissue engineering, drug delivery, wound dressings and bioelectronics. PGS has highly adjustable mechanical properties compatible with a variety of biological tissues (especially cardiac tissues), and can be used to construct cell scaffolds that promote the regeneration of cardiomyocytes and induce cardiac tissue repair. At the same time, it can carry drugs to achieve controlled release of drugs and active macromolecules that are anti-inflammatory and promote myocardial repair. PGS derivatives are also widely used as conductive grafts for nerve function recovery. They have ideal mechanical strength and degradation, can assist the growth of new nerves, and promote myelin gene expression and neurotrophin secretion of stem cells. PGS scaffolds can support cell attachment, proliferation and collagen deposition, and have the potential to be used in soft tissue engineering such as skin, blood vessels and ligaments. PGS can also be used to construct implantable electronic devices. Its biocompatibility and surface degradation mechanism can well ensure the operation of the device in the human body. It can sensitively capture and adapt to large deformations of human tissues. Its biodegradability avoids the harm to the human body caused by secondary removal. It is more in line with the movement of human tissues than traditional electronic devices, and exhibits low cytotoxicity and supports the adhesion and proliferation of neurons.

[0029] Preferably, the raw materials and catalysts in the examples of the present application are purchased through commercial channels, the sebacic acid and glycerol used are from Maclean Co., Ltd., and itaconic acid and catalyst are purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0030] Due to the application of the above technical solution, the present invention has the following beneficial effects compared with the prior art: 1. The novel biodegradable bio-based polyester elastomer prepared by the present invention can effectively design the molecular structure, including the hydroxyl content, molecular weight and its distribution, and cross-linking degree in the molecular chain, so as to optimize and customize the thermodynamic properties, mechanical properties, hydrophilicity and degradation properties of the elastomer; 2. The novel biodegradable bio-based polyester elastomer prepared by the present invention can effectively improve the cross-linking conditions of polyglyceryl sebacate, provide guidance for cross-linking modification, and the introduction of itaconic acid can also give polyglyceryl sebacate antibacterial properties; 3. The present invention adopts the melt polycondensation method, which does not require solvents, uses a small amount of catalyst, is low in price, has simple and safe experimental operations, has low requirements for equipment, and the product is formed in one step without the need for subsequent treatment and processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, some of the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be made based on these drawings without paying any creative work.

[0032] Figure 1 is the total reflection Fourier infrared analysis spectrum of the novel degradable bio-based polyester elastomer of Example 1 of the present invention; Figure 2 is a differential scanning calorimetry DSC curve diagram of the novel degradable bio-based polyester elastomer of Example 1 of the present invention; Figure 3 is an X-ray diffraction analysis spectrum of the novel degradable bio-based polyester elastomer of Example 1 of the present invention; Figure 4 is a stress-strain curve diagram of the novel degradable bio-based polyester elastomer in Example 1 of the present invention; Figure 5 This is a water contact angle picture of the novel degradable bio-based polyester elastomer of Example 1 of the present invention; Figure 6 This is a degradation curve diagram of the novel degradable bio-based polyester elastomer according to Example 1 of the present invention. DETAILED DESCRIPTION

[0033] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, a specific implementation scheme is now described in detail.

[0034] The present invention is further described below in conjunction with the examples, but the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not indicated are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0035] Example 1 See attached Figure 1-6 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.69 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. The temperature was gradually raised to 140°C under the protection of a nitrogen atmosphere, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-1 prepolymer with a molecular weight of 630 g / mol; S2. Preparation of itaconic acid cross-linked polyglycerol sebacate bioelastomer: add 0.1 mol of pre-PGS-1 prepolymer obtained in step S1 and 0.1 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat to 130°C under the protection of a nitrogen atmosphere, react for 3 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 21 hours to obtain the final product PGSIA-1.

[0036] Example 2 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.5 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. The temperature was gradually raised to 150°C under the protection of a nitrogen atmosphere, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-2 prepolymer with a molecular weight of 1950 g / mol; S2. Preparation of itaconic acid cross-linked polysebacic acid glycerol bioelastomer: add 0.1 mol of pre-PGS-2 prepolymer obtained in step S1 and 0.05 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat up to 130°C under the protection of a nitrogen atmosphere, react for 2 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 22 hours to obtain the final product PGSIA-2.

[0037] Example 3 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.5 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. The temperature was gradually raised to 160°C under the protection of a nitrogen atmosphere, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-3 prepolymer with a molecular weight of 3500 g / mol; S2. Preparation of itaconic acid cross-linked polyglycerol sebacate bioelastomer: add 0.1 mol of pre-PGS-3 prepolymer obtained in step S1 and 0.05 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat to 130°C under the protection of a nitrogen atmosphere, react for 1 hour, add 5% by mass of the catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 23 hours to obtain the final product PGSIA-3.

[0038] Example 4 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.375 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. The temperature was gradually raised to 140°C under the protection of a nitrogen atmosphere, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-4 prepolymer with a molecular weight of 610 g / mol; S2. Preparation of itaconic acid cross-linked polyglycerol sebacate bioelastomer: add 0.1 mol of pre-PGS-4 prepolymer obtained in step S1 and 0.075 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat to 130°C under the protection of a nitrogen atmosphere, react for 3 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 21 hours to obtain the final product PGSIA-4.

[0039] Example 5 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 1 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. The temperature was gradually raised to 140°C under the protection of a nitrogen atmosphere, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-5 prepolymer with a molecular weight of 680 g / mol; S2. Preparation of itaconic acid cross-linked polyglycerol sebacate bioelastomer: add 0.1 mol of pre-PGS-5 prepolymer obtained in step S1 and 0.03 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat to 130°C under the protection of a nitrogen atmosphere, react for 3 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 21 hours to obtain the final product PGSIA-5.

[0040] Example 6 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.5 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. Under the protection of a nitrogen atmosphere, the temperature was gradually raised to 140°C, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-6 prepolymer with a molecular weight of 1500 g / mol; S2. Preparation of itaconic acid cross-linked polyglycerol sebacate bioelastomer: add 0.1 mol of pre-PGS-6 prepolymer obtained in step S1 and 0.025 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat up to 130°C under the protection of a nitrogen atmosphere, react for 3 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 21 hours to obtain the final product PGSIA-6.

[0041] Example 7 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.5 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. Under the protection of a nitrogen atmosphere, the temperature was gradually raised to 140°C, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-7 prepolymer with a molecular weight of 1500 g / mol; S2. Preparation of itaconic acid cross-linked polyglycerol sebacate bioelastomer: add 0.1 mol of pre-PGS-7 prepolymer obtained in step S1 and 0.05 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat to 130°C under the protection of a nitrogen atmosphere, react for 3 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 21 hours to obtain the final product PGSIA-7.

[0042] Example 8 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.5 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. Under the protection of a nitrogen atmosphere, the temperature was gradually raised to 140°C, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-8 prepolymer with a molecular weight of 1500 g / mol; S2. Preparation of itaconic acid cross-linked polysebacic acid glycerol bioelastomer: add 0.1 mol of pre-PGS-8 prepolymer obtained in step S1 and 0.075 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat to 130°C under the protection of a nitrogen atmosphere, react for 3 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 21 hours to obtain the final product PGSIA-8.

[0043] Example 9 This embodiment provides a method for preparing a novel biodegradable bio-based polyester elastomer, comprising the following steps: S1. Esterification reaction to generate oligomers: 0.5 mol of glycerol and 0.5 mol of sebacic acid were added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask was placed in an oil bath pot with magnetic stirring. Under the protection of a nitrogen atmosphere, the temperature was gradually raised to 140°C, and the reaction was carried out for 4 hours. After that, the vacuum degree of the reaction system was reduced to 200 Pa, and the reaction was continued for 8 hours to obtain a pre-PGS-9 prepolymer with a molecular weight of 1500 g / mol; S2. Preparation of itaconic acid cross-linked polysebacic acid glyceride bioelastomer: add 0.1 mol of pre-PGS-9 prepolymer obtained in step S1 and 0.1 mol of itaconic acid into a three-necked flask connected to a nitrogen inlet and a condensing device, then place the flask in an oil bath with a magnetic stirrer, gradually heat to 130°C under the protection of a nitrogen atmosphere, react for 3 hours, add 5% by mass of a catalyst diisopropyl peroxide (DPO), mix well and transfer to a polytetrafluoroethylene mold, place in an oven at 130°C, adjust the vacuum degree to 1300 Pa, and continue the reaction for 21 hours to obtain the final product PGSIA-9.

[0044] Comparative Example 1 This comparative example is carried out on the basis of the above-mentioned Example 6, and the similarities with the above-mentioned Example are not repeated here.

[0045] In this embodiment, after the prepolymer is synthesized according to the process of Example 6, the prepolymer is placed in a vacuum oven at a temperature of 130° C. and a vacuum degree of 200 Pa to continue reacting for 21 hours to obtain thermally cross-linked PGS.

[0046] Comparative Example 2 This comparative example is carried out on the basis of the above-mentioned Example 9, and the similarities with the above-mentioned Example are not repeated here.

[0047] In this embodiment, 0.5 mol of glycerol and 0.5 mol of sebacic acid are first added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask is placed in an oil bath with a magnetic stirrer. The temperature is gradually raised to 140°C under the protection of a nitrogen atmosphere, and the reaction is carried out for 4 hours. The vacuum degree of the reaction system is then reduced to 200 Pa, and the reaction is continued for 4 hours to obtain a pre-PGS prepolymer with a number average molecular weight of 400 g / mol; a cross-linking reaction is subsequently carried out under the same conditions. The product after the reaction is in a viscous state and cannot be processed and formed.

[0048] Comparative Example 3 This comparative example is carried out on the basis of the above-mentioned Example 9, and the similarities with the above-mentioned Example are not repeated here.

[0049] In this embodiment, 0.5 mol of glycerol and 0.5 mol of sebacic acid are first added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask is placed in an oil bath with a magnetic stirrer. The temperature is gradually raised to 140°C under the protection of a nitrogen atmosphere, and the reaction is carried out for 4 hours. The vacuum degree of the reaction system is then reduced to 200 Pa, and the reaction is continued for 20 hours to obtain a pre-PGS prepolymer with a number average molecular weight of 4000 g / mol; a cross-linking reaction is subsequently carried out under the same conditions, but due to the excessive viscosity of the system, the reaction of itaconic acid and the prepolymer is insufficient, the bubble removal is difficult, the cross-linking effect is significantly deteriorated, and the product performance cannot meet the application.

[0050] Comparative Example 4 This comparative example is carried out on the basis of the above-mentioned Example 7, and the similarities with the above-mentioned Example are not repeated here.

[0051] In this embodiment, after the prepolymer is synthesized according to the process of Example 7, 0.1 mol of the prepolymer and 0.05 mol of itaconic acid are added to a three-necked flask connected to a nitrogen inlet and a condensing device, and then the flask is placed in an oil bath pot with a magnetic stirrer. The temperature is gradually raised to 130° C. under the protection of a nitrogen atmosphere. After reacting for 3 hours, the mixture is transferred to a polytetrafluoroethylene mold, placed in an oven at 130° C., the vacuum degree is adjusted to 1300 Pa, and the reaction is continued for 24 hours to obtain the final product PGSIA-10.

[0052] The products obtained in the above embodiments and comparative examples were tested, and the test results are shown in Table 1.

[0053] Table 1

[0054] It can be concluded from Examples 1, 2 and 3 that prepolymers with different molecular weights and the same hydroxyl content can be obtained by changing the process conditions of the synthesis. As the molecular weight of the prepolymer increases, the mechanical properties of itaconic acid cross-linked polyglyceryl sebacate gradually increase, the hydrophilicity gradually decreases, and the degradation rate gradually slows down.

[0055] It can be seen from Examples 1, 4 and 5 that prepolymers with different hydroxyl contents and the same molecular weight can be obtained by changing the process conditions of the synthesis. As the hydroxyl content of the prepolymer increases, the mechanical properties of itaconic acid cross-linked polyglyceryl sebacate gradually improve, the hydrophilicity gradually increases, and the degradation rate gradually slows down.

[0056] Through Examples 6, 7, 8, and 9, it can be concluded that by maintaining the consistency of the prepolymer structure and changing the content of itaconic acid, the performance of PGSIA can be adjusted. As the content of itaconic acid increases, the mechanical properties of itaconic acid-cross-linked polyglyceryl sebacate gradually improve, the hydrophilicity gradually increases, and the degradation rate gradually slows down.

[0057] It can be concluded from Examples 1-9 and Comparative Example 1 that the addition of itaconic acid significantly improves the cross-linking structure of PGS, and enhances the mechanical properties and antibacterial properties of PGS.

[0058] It can be concluded from Examples 1, 2, 3 and Comparative Examples 2 and 3 that the prepolymer within the molecular weight range of the present scheme (number average molecular weight of 600-3500 g / mol) can effectively form a cross-linked network after cross-linking with itaconic acid, and has adjustable excellent mechanical properties, hydrophilic properties and degradation properties. A prepolymer with a molecular weight that is too high or too low is not conducive to the cross-linking reaction and the improvement of the structure.

[0059] It can be concluded from Example 7 and Comparative Example 4 that the addition of a catalyst can accelerate the cross-linking reaction, improve the mechanical properties of PGSIA, and promote the cross-linking of double bonds.

[0060] By comparing the performance test results of the embodiments with those of the comparative examples, it can be seen that the novel degradable bio-based polyester elastomer prepared by the present invention has a designable molecular structure, and the mechanical properties, hydrophilic properties, degradation properties and antibacterial properties of the elastomer can be regulated by adjusting the molecular weight of the prepolymer and the amount of the cross-linking agent, thereby meeting application requirements.

[0061] In the above, the product testing and characterization methods used in Examples 1-9 and Comparative Examples 1-4 of the present invention are as follows: Test method for intrinsic viscosity: The intrinsic viscosity of polyester elastomer is measured using the automatic viscometer NCY-4 produced by Shanghai Starda Co., Ltd. The solvent used in the measurement is a phenol / 1,1,2,2-tetrachloroethane mixed solution with a mass ratio of 1:1, and the Ubbelohde viscometer with an inner diameter of 0.84 mm is used. The test is carried out in a constant temperature water bath at a temperature of (25±0.05)°C.

[0062] Molecular weight test method: The molecular weight of the sample was determined by an American Waters 1515 gel permeation chromatograph, the chromatographic column was Agilent PL gel 5 μm MIXED-C, the mobile phase was N, N-dimethylformamide, the flow rate was 1 mL / min, and the polystyrene standard was used.

[0063] Melting temperature and crystallization temperature test method: The thermal properties of copolyester were studied using the American TAQ2000 differential scanning calorimeter. In a nitrogen environment, 5-10 mg of the sample was heated to 100°C at a rate of 10°C / min and kept constant for 10 minutes. Then, the sample was cooled to -50°C at a rate of 10°C / min, and finally the sample was heated to 100°C at a rate of 10°C / min, and the glass transition temperature (Tg) was recorded.

[0064] Mechanical properties test method: Use a universal testing machine to test the tensile properties of the material. Cut the material into dumbbell-shaped specimens, perform a tensile test at a speed of 50mm / min, and test each sample at least five times.

[0065] Hydrophilicity test method: Use German Datephysics OCA40 to measure the static water contact angle of the material. Use a microsyringe to titrate 3ml of deionized water on the sample surface, take a picture of the morphology of the water drop on the sample surface at 15s, measure the water contact angle on both sides of the water drop and calculate the average value. Take five points for each sample and calculate the average value.

[0066] Antibacterial rate test method: Dilute E.coli (ATCC25922) in sterile broth and place in a centrifuge tube, and place in a 37℃ constant temperature incubator for overnight culture, and observe the turbidity of the bacterial solution. Use a sterilized pipette tip to take 100ul of bacterial solution in a 96-well plate, test the OD value at 600nm, and then dilute the bacterial solution at 1:1000 for use. After high-temperature sterilization of PGSIA, sterilize it under ultraviolet light overnight, take PGSIA of the same mass and size and place it in a centrifuge tube containing an equal amount of bacterial solution, and place it in a 37℃ constant temperature incubator for 24 hours.

[0067] The antibacterial rate is calculated by formula 1: ; Among them, N0 represents the OD600 value of the bacterial solution without adding PGSIA, and N1 represents the OD600 value of the bacterial solution after adding PGSIA.

[0068] In summary, the novel biodegradable bio-based polyester elastomer prepared by the present invention has a strong designability of molecular structure. By regulating the hydroxyl content, molecular weight and distribution in the prepolymer pre-PGS molecular chain, or regulating the degree of crosslinking, the thermodynamic properties, mechanical properties, hydrophilicity and degradation properties of the elastomer can be optimized and customized. On the other hand, the method for preparing a novel biodegradable bio-based polyester elastomer proposed by the present invention provides a new idea for the crosslinking modification of polysebacic acid glycerol ester, and the introduction of itaconic acid can also give polysebacic acid glycerol ester antibacterial properties; the melt polycondensation method adopted does not require solvents, the catalyst used in the crosslinking modification process is low in price and small in amount, the experimental operation is simple and safe, and the requirements for equipment are low, and the product is formed in one step without subsequent processing.

[0069] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A novel biodegradable bio-based polyester elastomer, characterized in that: Glycerol, sebacic acid and itaconic acid are used as reaction monomers, and the following structural units are included: (Ⅰ); Wherein, n is an integer from 1 to 6; R1 is selected from or or The residues of R2 is selected from or of residues.

2. A method for preparing the novel biodegradable bio-based polyester elastomer according to claim 1, characterized in that: The steps include: S1. Esterification reaction to generate oligomers: under the protection of inert gas, glycerol and sebacic acid are placed in a container in proportion, the temperature and stirring speed are controlled to react, and then the vacuum degree of the system is reduced to continue the reaction to obtain the oligomer pre-PGS; S2. Preparation of itaconic acid cross-linked polyglyceryl sebacate bioelastomer: Under the protection of inert gas, the oligomer pre-PGS obtained in step S1 and itaconic acid are mixed in proportion, the temperature and stirring speed are controlled to react, a catalyst is added and mixed evenly, and the reaction is continued under vacuum conditions to obtain itaconic acid cross-linked polyglyceryl sebacate bioelastomer PGSIA.

3. The method for preparing a novel biodegradable bio-based polyester elastomer according to claim 2, characterized in that: In step S1, the glycerol and the sebacic acid are placed in a container at a molar ratio of 0.5 to 1.

33.

4. The method for preparing a novel biodegradable bio-based polyester elastomer according to claim 2, characterized in that: In step S2, the itaconic acid and the oligomer pre-PGS are mixed at a molar ratio of 0.25 to 1.

5. The method for preparing a novel biodegradable bio-based polyester elastomer according to claim 2, characterized in that: The catalyst in step S2 is an organic peroxide initiator, and the peroxide initiator is selected from at least one of dicumyl peroxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

6. The method for preparing a novel biodegradable bio-based polyester elastomer according to claim 2, characterized in that: The mass of the catalyst in step S2 is 3% to 7% of the total mass of the oligomer pre-PGS and the itaconic acid.

7. The method for preparing a novel biodegradable bio-based polyester elastomer according to claim 2, characterized in that: In step S1, the temperature is controlled at 120-160° C. for reaction for 4-8 hours, and then the vacuum degree of the system is reduced to 50-250 Pa and the reaction is continued for 8-16 hours. The stirring speed is controlled at 100-900 rpm.

8. The method for preparing a novel biodegradable bio-based polyester elastomer according to claim 2, characterized in that: In step S2, the temperature is controlled to be 110-140°C for reaction for 1-4 hours, and then the reaction is continued for 11-23 hours under vacuum conditions, the vacuum degree of the vacuum conditions is 1000-2000 Pa, and the stirring speed is controlled to be 50-500 rpm.

9. The novel biodegradable bio-based polyester elastomer according to claim 1, characterized in that: The Young's modulus of the novel biodegradable bio-based polyester elastomer is 0.95~24.94MPa, the tensile strength is 0.48~7.82MPa, and the antibacterial property is improved to 53.76%.

10. Application of the novel bio-based polyester elastomer prepared by the novel bio-based polyester elastomer according to any one of claims 1 and 9 or the method for preparing the novel bio-based polyester elastomer according to any one of claims 2 to 8 in tissue engineering, drug delivery, wound dressing or bioelectronics.

Citation Information

Patent Citations

  • Ultrasonic microwave synthesis method for poly(butanediol itaconate-co-butanediol sebate)copolyester

    CN105601894A

  • Application of poly(glycerol disebacate)

    CN106620827A

  • Isocyanate crosslinked polyethylene glycol-polyglycerol sebacate bio-elastomer as well as preparation method and application thereof

    CN110078880A

  • Bio-based biodegradable polyester and synthesis method thereof

    CN110078907A

  • Method for preparing biodegradable polyester elastomer

    US20200247945A1