Organic sulfide, graphene-organic sulfide composite material, active positive electrode material and preparation method and application thereof
Through the use of organic sulfide and graphene-organic sulfide composite materials, the problems of high solubility, easy cracking and poor conductivity of the positive electrode material of lithium sulfur battery are solved, and the high specific capacity, cycle stability and rate performance are improved. .
Patent Information
- Application Number
- CN202411134650.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-19
AI Technical Summary
Lithium sulfur batteries have high solubility, easy rupture and differentiation, poor conductivity, resulting in specific capacity attenuation, poor cycle stability and poor rate performance.
Using organic sulfide and graphene-organic sulfide composite materials, it is prepared by substitution reaction of 1,2,3,4,5,6-hexasulfide benzene and sulfur in a solvent to form a polysulfur chain structure with S-S bonds. Combined with carbon-based host materials to provide physical barriers and chemosorption, enhancing conductivity and reaction kinetics.
It effectively suppresses the dissolution and volume changes of the charge and discharge intermediate, and improves the specific capacity, cycle stability and rate performance of lithium-sulfur batteries.
Smart Images

Figure CN119019688A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of positive electrode materials for lithium-sulfur batteries, and in particular to an organic sulfide, a graphene-organic sulfide composite material, an active positive electrode material, and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of light weight, high energy density and zero memory effect, and are widely used in portable electronic devices, transportation and large-scale energy storage. Traditional lithium-ion batteries use inorganic intercalation type positive electrode materials, such as lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4) and lithium iron phosphate (LiFePO4), and the negative electrode uses graphite and lithium titanate (Li4Ti5O 12 ), etc., the further improvement of the theoretical specific capacity of these electrode materials has reached a bottleneck period, and the heavy metal elements therein are also facing severe resource and environmental problems, which is not conducive to their large-scale sustainable development in the future.
[0003] Lithium-sulfur batteries consist of a conversion-type sulfur positive electrode and a lithium negative electrode. The positive electrode sulfur undergoes a reversible redox reaction with multi-step electron transfer during the charge and discharge process. A series of lithium polysulfide intermediates (LiPSs) are generated during the redox process, and finally Li2S product is generated with a capacity of 1672 mAh g -1 High theoretical specific capacity, and has the advantages of abundant resources, low cost and low environmental pollution; the lithium negative electrode undergoes Reaction process, with 3860mAh g -1 High theoretical specific capacity. The average output voltage of lithium-sulfur batteries is about 2.1V, with a capacity of 2600Wh kg -1 Therefore, lithium-sulfur batteries are expected to become an important direction for the large-scale development of high-energy-density batteries in the future.
[0004] A variety of lithium-sulfur batteries have been developed and show excellent electrochemical performance, but their further development and large-scale commercialization also face a series of challenges. First, the lithium polysulfide intermediates LiPSs produced by the sulfur positive electrode during the charge and discharge process have high solubility in the electrolyte. During the cycle, the positive electrode active material is continuously lost. The LiPSs dissolved in the electrolyte will pass through the diaphragm to the negative electrode side and undergo a series of side reactions on the negative electrode surface, resulting in self-discharge of the battery, specific capacity decay and poor cycle stability. Secondly, the positive electrode material S8 and its discharge product Li2S have a large density difference. During the charge and discharge process, the electrode will undergo severe volume changes, resulting in the rupture and differentiation of the electrode material and the reduction of the battery cycle life. In addition, the insoluble S8 and Li2S have poor conductivity, and the conversion reaction kinetics of polysulfides are poor. These factors seriously affect the reaction kinetics of the battery and limit its rate performance.
[0005] Based on this, there is an urgent need to develop a sulfur cathode host material. Summary of the invention
[0006] The present application provides an organic sulfide, a graphene-organic sulfide composite material, an active positive electrode material, and a preparation method and application thereof, aiming to solve the problems of specific capacity attenuation, poor cycle stability, and poor rate performance of existing lithium-sulfur batteries caused by high solubility, easy rupture and differentiation, and poor conductivity of the positive electrode material.
[0007] In order to achieve the above objectives, the present application adopts the following technical solutions.
[0008] In a first aspect of the present application, an organic sulfide is provided, having a chemical structure shown in formula (1):
[0009]
[0010] Here, n is the number of sulfur atoms, 2≤n≤8.
[0011] In some embodiments, it is prepared by a substitution reaction between 1,2,3,4,5,6-hexamercaptobenzene and sulfur in a solvent;
[0012] The mass ratio of the 1,2,3,4,5,6-hexamercaptobenzene to sulfur is 1:(1.5-6).
[0013] In some embodiments, the solvent includes at least one of carbon disulfide, toluene, or ethylene glycol.
[0014] In some embodiments, the reaction temperature is 20-50°C and the reaction time is 12-48h.
[0015] In a second aspect of the present application, a graphene-organosulfide composite material is provided, comprising a carbon-based host material and an active component adsorbed on the surface of the carbon-based host material;
[0016] The active ingredient includes the above-mentioned organic sulfide.
[0017] In some embodiments, the carbon-based host material includes at least one of graphene, carbon nanotubes, nitrogen-doped graphene, Ketjen black, MoS2-modified nitrogen-doped graphene, or CoS2-modified graphene.
[0018] The third aspect of the present application provides a method for preparing the above-mentioned graphene-organic sulfide composite material, comprising:
[0019] 1,2,3,4,5,6-hexamercaptobenzene, sulfur and carbon-based host materials are dispersed in a solvent, reacted at 20-50° C. under an inert atmosphere for 12-48 hours, and after the reaction, the solid phase is collected and dried to obtain a graphene-organic sulfide composite material.
[0020] In another aspect of the present application, an active positive electrode material is provided, comprising the above-mentioned organic sulfide, or the above-mentioned graphene-organic sulfide composite material.
[0021] Another aspect of the present application provides use of the above-mentioned active positive electrode material in a lithium-sulfur battery.
[0022] In another aspect of the present application, a lithium-sulfur battery is provided, wherein the positive electrode thereof comprises the above-mentioned active positive electrode material.
[0023] Compared with the prior art, the beneficial effects of this application are:
[0024] The organic sulfide and graphene-organic sulfide composite material of the present application have specific structures and functions. They are composed of 1,2,3,4,5,6-hexamercaptobenzene and polysulfide chains alternately. The two units are connected by SS bonds. A large number of redox-active polysulfide chains are chemically fixed on the aromatic skeleton of 1,2,3,4,5,6-hexamercaptobenzene through SS bonds. The carbon-based host material and 1,2,3,4,5,6-hexamercaptobenzene synergistically provide physical barriers, chemical adsorption and stable chemical bonds, which effectively inhibit the shuttling and dissolution of polysulfide intermediates in charge and discharge. At the same time, the carbon-based host material modified with metal compounds and doped with heteroatoms has the effect of enhancing conductivity and rapid catalytic conversion reactions, and can also alleviate the volume change of the organic sulfide or graphene-organic sulfide composite material during the charge and discharge process, further improving its stability and reaction kinetics, thereby achieving high specific capacity, high cycle stability and high rate performance of lithium-sulfur batteries.
[0025] The organic sulfide and graphene-organic sulfide composite material of the present application contain redox-active polysulfide bonds connected by aromatic rings, and are particularly suitable for positive electrode active materials of lithium-sulfur batteries. The lithium-sulfur battery containing the positive electrode active material has higher specific capacity, higher cycle stability and higher rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 This is the infrared spectrum of the organic sulfide prepared in Example 1;
[0028] Figure 2 This is a thermogravimetric analysis test diagram of the organic sulfide prepared in Example 1;
[0029] Figure 3 This is the infrared spectrum of the graphene-organic sulfide composite material prepared in Example 3;
[0030] Figure 4 This is a charge and discharge cycle test diagram of the lithium-sulfur battery 1;
[0031] Figure 5 is a capacity-voltage curve diagram of the lithium-sulfur battery 2;
[0032] Figure 6 This is a charge and discharge cycle test diagram of lithium-sulfur battery 2;
[0033] Figure 7 This is a charge and discharge cycle test diagram of the lithium-sulfur battery 3;
[0034] Figure 8 This is the charge and discharge cycle test diagram of lithium-sulfur battery D1. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0036] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0037] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0038] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0039] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0040] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0041] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.
[0042] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0043] In a first aspect, the present application provides an organic sulfide having a chemical structure shown in formula (1):
[0044]
[0045] Here, n is the number of sulfur atoms, 2≤n≤8.
[0046] The organic sulfide represented by formula (1) is composed of 1,2,3,4,5,6-hexamercaptobenzene and polysulfide chains alternately, and the two units are connected by SS bonds. The six thiol groups on each 1,2,3,4,5,6-hexamercaptobenzene can be replaced by polysulfide chains, and the number of polysulfide substitutions is 1, 2, 3, 4, 5 or 6. Each polysulfide chain includes 2-8 sulfur atoms. The polysulfide chains fixed by SS bonds are chemically fixed on the aromatic skeleton of 1,2,3,4,5,6-hexamercaptobenzene, and the dissolution and shuttling of polysulfide intermediates are effectively inhibited, which improves the stability of the material and further enhances the cycle performance of the battery.
[0047] The organic sulfide of the present application is prepared by a substitution reaction between 1,2,3,4,5,6-hexamercaptobenzene and a series of measured sulfur in a solvent. The reaction is preferably carried out under anaerobic conditions, the reaction temperature is 20-50°C, preferably 20-30°C, and the reaction time is 12-48h, preferably 18-36h.
[0048] In the present application, the mass ratio of 1,2,3,4,5,6-hexamercaptobenzene to sulfur is preferably 1:(1.5-6); and the solvent preferably includes at least one of carbon disulfide, toluene or ethylene glycol.
[0049] In a second aspect, the present application provides a graphene-organic sulfide composite material, comprising a carbon-based host material and an active ingredient adsorbed on the surface of the carbon-based host material; the active ingredient comprises the above-mentioned organic sulfide; the carbon-based host material comprises at least one of graphene, carbon nanotubes, nitrogen-doped graphene, Ketjen black, MoS2-modified nitrogen-doped graphene or CoS2-modified graphene.
[0050] In the present application, the method for preparing the graphene-organic sulfide composite material comprises:
[0051] 1,2,3,4,5,6-hexamercaptobenzene, sulfur and carbon-based host materials are weighed in a mass ratio of 1:(1.5-6):(0.2-2), added to a round-bottom flask, and an inert gas is introduced into the reaction system; a solvent is added to the system, and the reaction is carried out by constant temperature stirring; after the reaction is completed, the reaction system is allowed to stand, the supernatant is discarded, the lower solid precipitate is collected, and the product is obtained by vacuum heating and drying, namely, a graphene-organic sulfide composite material. Among them, the inert gas is preferably argon.
[0052] The present application provides an active positive electrode material, comprising the above-mentioned organic sulfide, or the above-mentioned graphene-organic sulfide composite material.
[0053] The active positive electrode material of the present application, i.e., the organic sulfide and the composite material thereof, has a stable structure, i.e., the structure shown in formula (1), which contains redox-active polysulfide bonds connected by aromatic rings, and is suitable for lithium-sulfur batteries, and is particularly suitable for positive electrode active materials of lithium-sulfur batteries. The active positive electrode material of the present application can be applied to lithium-sulfur batteries, and the lithium-sulfur battery containing the active positive electrode material has a higher specific capacity, higher cycle stability and higher rate performance.
[0054] The active positive electrode material graphene-organosulfide composite material of the present application, when the organic sulfide is composited with a carbon-based host material, the active material is dispersed on the surface of the porous conductive carbon material, and the porous conductive carbon material acts as a physical barrier to inhibit the dissolution and shuttling of polysulfides, and at the same time can alleviate the volume change of the electrode during the charge and discharge process, further improving the cycle stability of the material. In addition, the material also has enhanced conductivity and improved kinetics, which is beneficial to improve its rate performance. Among them, when the organic sulfide is composited with a heteroatom-doped carbon-based host material modified by a metal compound, the host material simultaneously provides a physical barrier and chemical adsorption of polysulfides, and the metal compound is beneficial to catalyze the conversion reaction of polysulfides, synergistically improving the reaction kinetics and cycle stability of the material.
[0055] The present application also provides a lithium-sulfur battery, the positive electrode of which includes the above-mentioned active positive electrode material. The lithium-sulfur battery prepared using the organic sulfide and the composite material of the present application has a higher mass specific capacity, better cycle stability and rate performance.
[0056] In the present application, the lithium-sulfur battery can be prepared by conventional techniques in the art.
[0057] Specifically, the preparation method of the lithium-sulfur battery includes: grinding and mixing an organic sulfide or graphene-organic sulfide composite material with a conductive additive and a binder in N-methylpyrrolidone (NMP) to form a slurry, applying the slurry on the surface of a carbon-coated aluminum foil current collector, heating and drying to form a positive electrode film, cutting the positive electrode film into a circle to form a positive electrode sheet; separating the positive electrode sheet and the negative lithium foil by a separator, adding an electrolyte, and assembling to obtain a button-type lithium-sulfur battery. The mass ratio of the organic sulfide or graphene-organic sulfide composite material, the conductive additive and the binder is (40-80):(50-10):10.
[0058] The conductive additive may be selected from at least one of SuperP, Ketjen black or carbon nanotubes; the electrolyte is a solution obtained by dissolving a lithium salt in an organic solvent, and the electrolyte salt concentration is 0.5-2.0 mol / L, preferably 1.0 mol / L. The lithium salt is selected from one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or lithium hexafluorophosphate (LiPF6) salts or a mixed salt prepared by mixing several of them in any proportion; the organic solvent is selected from one of 1,3-dioxolane (DOL), ethylene glycol dimethyl ether (DME), ethylene carbonate (EC) or dimethyl carbonate (DMC) or a mixed solvent prepared by mixing several of them in any proportion.
[0059] The present application is further described below by way of examples.
[0060] Example 1
[0061] This embodiment provides a method for preparing an organic sulfide, comprising:
[0062] 50 mg of 1,2,3,4,5,6-hexamercaptobenzene and 200 mg of sulfur powder were added to a 50 mL round-bottom flask in sequence, and then 20 mL of carbon disulfide was added. The mixture was stirred at 25 °C for 24 hours. After the reaction was completed, the reaction system was allowed to stand, the supernatant was removed and the solid precipitated product was retained. The product was vacuum dried at 60 °C for 6 hours to obtain an organic sulfur compound 1.
[0063] Example 2
[0064] This embodiment provides a method for preparing an organic sulfide, comprising:
[0065] 50 mg of 1,2,3,4,5,6-hexamercaptobenzene and 150 mg of sulfur powder were added to a 25 mL round-bottom flask in sequence, and the reaction system was protected by argon. 10 mL of toluene was added and stirred at 50 °C for 12 hours. After the reaction was completed, the reaction system was allowed to stand, and the supernatant was removed after the liquid was separated. The solid precipitated product was collected and vacuum dried at 60 °C for 12 hours to obtain organic sulfur compound 2.
[0066] Example 3
[0067] This embodiment provides a method for preparing a graphene-organic sulfide composite material, comprising:
[0068] 50 mg of 1,2,3,4,5,6-hexamercaptobenzene, 200 mg of sulfur powder and 50 mg of MoS2-modified nitrogen-doped graphene host material were added into a 50 mL round-bottom flask in sequence, the reaction system was placed under argon protection, 20 mL of carbon disulfide solvent was added, and the mixture was stirred at 25 °C for 24 hours. After the reaction was completed, the reaction system was allowed to stand, and the supernatant was removed after the liquid was separated, the solid precipitated product was collected, and the product was vacuum dried at 60 °C for 12 hours to obtain the organic sulfur compound composite material 3.
[0069] Example 4
[0070] This embodiment provides a method for preparing a graphene-organic sulfide composite material, comprising:
[0071] 75 mg of 1,2,3,4,5,6-hexamercaptobenzene, 200 mg of sulfur powder and 25 mg of MoS2-modified graphene host material were added to a 50 mL round-bottom flask in sequence, and the reaction system was protected by argon. 20 mL of carbon disulfide was added and stirred at 25 °C for 24 hours. After the reaction was completed, the reaction system was allowed to stand, and the supernatant was removed after the liquid was separated, and the solid precipitated product was collected. The product was vacuum dried at 60 °C for 12 hours to obtain an organic sulfur compound composite material 4.
[0072] Example 5
[0073] This embodiment provides a method for preparing a graphene-organic sulfide composite material, comprising:
[0074] 50 mg of 1,2,3,4,5,6-hexamercaptobenzene, 200 mg of sulfur powder and 50 mg of CoS2-modified graphene host material were added to a 50 mL round-bottom flask in sequence, and the reaction system was protected by argon. 20 mL of carbon disulfide was added and stirred at 30 °C for 18 hours. After the reaction was completed, the reaction system was allowed to stand, and the supernatant was removed after the liquid was separated, and the solid precipitated product was collected. The product was vacuum dried at 60 °C for 8 hours to obtain an organic sulfur compound composite material 5.
[0075] The performance and structure of the organic sulfide prepared in Example 1 were characterized by infrared spectroscopy and thermogravimetric analysis.
[0076] Among them, the infrared spectrum is as follows Figure 1 As shown, from Figure 1 It can be seen that at 468cm -1 The infrared characteristic peak of SS appears at , indicating that 1,2,3,4,5,6-hexamercaptobenzene undergoes a substitution reaction with sulfur to produce SS connecting bonds.
[0077] Thermogravimetric analysis test results are as follows Figure 2 As shown. Figure 2 It can be seen that the organosulfur polymer exhibits a mass retention rate of more than 96% at 200°C and has high thermal stability.
[0078] The graphene-organic sulfide composite material prepared in Example 3 was tested by infrared spectroscopy, and the results are as follows: Figure 3 As shown. Figure 3 It can be seen that the graphene-organic sulfide composite material has a peak at 468 cm -1 The infrared peak with SS bond indicates that 1,2,3,4,5,6-hexamercaptobenzene undergoes substitution reaction with sulfur to form a polymer containing SS connecting bonds.
[0079] Example 6
[0080] This embodiment provides a lithium-sulfur battery, wherein the positive electrode active material is the organic sulfide prepared in Example 1. The preparation method thereof comprises:
[0081] The organic sulfide prepared in Example 1 was used as the positive electrode active material, Ketjen black was used as the conductive additive, and PVDF was used as the binder to prepare a slurry, wherein the mass ratio of the positive electrode active material, Ketjen black, and PVDF was 7:2:1. The slurry was coated on the surface of the carbon-coated aluminum foil current collector, and after drying at 60°C, a positive electrode film was obtained, which was cut to obtain a positive electrode disc.
[0082] Metal lithium foil was used as the negative electrode, Celgard2325 was used as the separator, LiTFSI was used as the electrolyte, DME and DOL were mixed in a volume ratio of 1:1 as the solvent, and an electrolyte with a molar concentration of 1M was prepared. An additive LiNO3 was added to the electrolyte with a concentration of 1wt%. A button-type (Cion-type 2025) lithium-sulfur battery was assembled in an argon-filled glove box, which was recorded as lithium-sulfur battery 1.
[0083] Example 7
[0084] This embodiment provides a lithium-sulfur battery, wherein the positive electrode active material is the graphene-organic sulfide composite material prepared in Example 3. The preparation method thereof comprises:
[0085] The graphene-organic sulfide composite material prepared in Example 3 was used as the positive electrode active material, Ketjen black was used as the conductive additive, and PVDF was used as the binder to prepare a slurry, wherein the mass ratio of the positive electrode active material, Ketjen black, and PVDF was 7:2:1. The slurry was coated on the surface of the carbon-coated aluminum foil current collector, and after drying at 60°C, a positive electrode film was obtained, which was cut to obtain a positive electrode disc.
[0086] Metal lithium foil was used as the negative electrode, Celgard2325 was used as the separator, LiTFSI was used as the electrolyte, DME and DOL were mixed in a volume ratio of 1:1 as the solvent, and the electrolyte with a molar concentration of 1M was prepared. The additive LiNO3 was added to the electrolyte with a concentration of 1wt%. A button-type (Cion-type 2025) lithium-sulfur battery was assembled in a glove box filled with argon gas, which was recorded as lithium-sulfur battery 2.
[0087] Example 8
[0088] This embodiment provides a lithium-sulfur battery, wherein the positive electrode active material is the graphene-organic sulfide composite material prepared in Example 3. The preparation method thereof comprises:
[0089] The graphene-organic sulfide composite material prepared in Example 3 was used as the positive electrode active material, Ketjen black was used as the conductive additive, and PVDF was used as the binder to prepare a slurry, wherein the mass ratio of the positive electrode active material, Ketjen black, and PVDF was 7:2:1. The slurry was coated on the surface of the carbon-coated aluminum foil current collector, and after drying at 60°C, a positive electrode film was obtained, which was cut to obtain a positive electrode disc.
[0090] Metal lithium foil was used as the negative electrode and Celgard2325 as the separator; the electrolyte used was an in-situ polymerized gel electrolyte, and the electrolyte precursor was a 1M LiTFSI + 0.5M LiFSI DOL solution. A button-type (Cion-type 2025) lithium-sulfur battery was assembled in an argon-filled glove box. After the battery was assembled, it was heated at 60°C. DOL underwent a ring-opening polymerization reaction under the initiation of LiFSI, and a gel polymer electrolyte was generated in situ. The resulting lithium-sulfur battery was recorded as lithium-sulfur battery 3.
[0091] Comparative Example 1
[0092] This comparative example provides a conventional lithium-sulfur battery, whose positive electrode active material is sulfur. Its preparation method includes:
[0093] Sulfur was used as the positive electrode active material, Ketjen black was used as the conductive additive, and PVDF was used as the binder to prepare a slurry, wherein the mass ratio of the positive electrode active material, Ketjen black, and PVDF was 7:2:1. The slurry was coated on the surface of the carbon-coated aluminum foil current collector, and after drying at 60°C, a positive electrode film was obtained, which was cut to obtain a positive electrode disc.
[0094] Metal lithium foil was used as the negative electrode and Celgard2325 as the separator; LiTFSI was used as the electrolyte, DME and DOL were mixed in a volume ratio of 1:1 as the solvent, and the electrolyte with a molar concentration of 1M was prepared. The additive LiNO3 was added to the electrolyte with a concentration of 1wt%. A button-type (Cion-type 2025) lithium-sulfur battery was assembled in a glove box filled with argon gas, which was recorded as lithium-sulfur battery D1.
[0095] Electrochemical performance tests were performed on the lithium-sulfur batteries 1-3 prepared in Examples 1-3 and the lithium-sulfur battery D1 prepared in Comparative Example 1, respectively.
[0096] The test results of lithium-sulfur battery 1 are as follows Figure 4 As shown. Figure 4 It can be seen that in the test voltage window range of 1.7-2.8V (vsLi / Li + ) within 1672mAg -1 At the current density (1.0C), the battery’s discharge capacity is 516.7 mAh g -1 , showing higher specific capacity and improved capacity utilization, while also exhibiting higher cycle stability.
[0097] The test results of lithium-sulfur battery 2 are as follows Figure 5 and Figure 6 As shown. Figure 5 It can be seen that in the test voltage window range of 1.7-2.8V (vs Li / Li + ) within 83.6mA g -1 At the current density (0.05C), the discharge capacity of the battery can reach 1573.8mAhg -1 .Depend on Figure 6 It can be seen that at 1672mAg -1 At the current density (1.0C), its first cycle discharge capacity can reach 844.5mAh g -1 In the 500-cycle charge and discharge cycle test, the average capacity retention rate per cycle can reach 99.94%, showing good charge and discharge cycle stability.
[0098] The test results of lithium-sulfur battery 3 are as follows Figure 7 As shown. Figure 7 It can be seen that in the test voltage window range of 1.7-2.8V (vsLi / Li + ) within 167.2mAg -1 At the current density (0.1C), the first cycle discharge capacity can reach 1341.5mAh g -1 .
[0099] The test results of the lithium-sulfur battery D1 prepared in Comparative Example 1 are as follows: Figure 8 As shown. Figure 8 It can be seen that in the test voltage window range of 1.7-2.8V (vs Li / Li + ) within 1672mAg -1 At current density (1.0C), lithium-sulfur battery D1 showed 322.3mAhg -1 The initial discharge capacity is 120.6 mAh g after 500 cycles. -1 , the capacity utilization is low and the cycle stability is poor.
[0100] The above test results show that the organic sulfide and graphene-organic sulfide composite materials of the present application are used as positive electrode active materials for lithium-sulfur batteries, and various lithium-sulfur batteries containing the positive electrode active materials have higher specific capacity, higher cycle stability and higher rate performance. In particular, the graphene-organic sulfide composite materials are used as positive electrode active materials for lithium-sulfur batteries, and the test voltage window range is 1.7-2.8V (vs Li / Li + ) within 83.6mA g -1 At the current density (0.05C), the discharge capacity of the battery can reach 1573.8mAh g -1 , has a very high discharge specific capacity; its -1 At the current density (1.0C), its first cycle discharge capacity can reach 844.5mAh g -1 In the 500-cycle charge and discharge cycle test, the average capacity retention rate per cycle can reach 99.94%, and the charge and discharge cycle stability is very high.
[0101] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.
Claims
1. An organic sulfide, characterized in that It has the chemical structure shown in formula (1): Here, n is the number of sulfur atoms, 2≤n≤8.
2. The organic sulfide according to claim 1, characterized in that It is prepared by a substitution reaction between 1,2,3,4,5,6-hexamercaptobenzene and sulfur in a solvent; The mass ratio of the 1,2,3,4,5,6-hexamercaptobenzene to sulfur is 1:(1.5-6).
3. The organic sulfide according to claim 2, characterized in that The solvent includes at least one of carbon disulfide, toluene or ethylene glycol.
4. The organic sulfide according to claim 2, characterized in that The reaction temperature is 20-50°C and the reaction time is 12-48h.
5. A graphene-organic sulfide composite material, characterized in that: It includes a carbon-based host material and an active component adsorbed on the surface of the carbon-based host material; The active ingredient comprises the organic sulfide according to claim 1.
6. The graphene-organosulfide composite material according to claim 5, characterized in that: The carbon-based host material includes at least one of graphene, carbon nanotubes, nitrogen-doped graphene, Ketjen black, MoS2-modified nitrogen-doped graphene or CoS2-modified graphene.
7. The method for preparing the graphene-organosulfide composite material according to claim 5, characterized in that: include: 1,2,3,4,5,6-hexamercaptobenzene, sulfur and carbon-based host materials are dispersed in a solvent, reacted at 20-50° C. under an inert atmosphere for 12-48 hours, and after the reaction, the solid phase is collected and dried to obtain a graphene-organic sulfide composite material.
8. An active positive electrode material, characterized in that The method comprises the organic sulfide according to any one of claims 1 to 4, or the graphene-organic sulfide composite material according to any one of claims 5 to 6.
9. Use of the active positive electrode material according to claim 8 in a lithium-sulfur battery.
10. A lithium-sulfur battery, characterized in that: The positive electrode thereof comprises the active positive electrode material as claimed in claim 8.
Citation Information
Patent Citations
Polysulfide anode material for lithium-sulfur battery, preparation method and application
CN110218324A
Graphene-hexasulfydryl benzene copper electrode material and preparation method and application thereof
CN112490441A
Polymeric sulfur material and application thereof in preparation of lithium-sulfur battery
CN114854018A
Preparation method and application of high-sulfur-loading high-conductivity vulcanized polyacrylonitrile
CN115160465A
Cited By
Composite sulfur positive electrode material and preparation method and application thereof
CN119864402A
Carbon body for positive electrode of lithium-sulfur battery and manufacturing method therefor
WO2026117008A1