Method for recycling PVDF dust formed in spraying process

By mixing PVDF dust with thickener and water during the spraying process, and filtration and iron removal treatment, the problem of low recycling rate of PVDF dust is solved, and the preparation of high-purity recycling slurry is realized, reducing production costs and dust Health risks and maintain the performance of the diaphragm bonding layer.

CN119019710APending Publication Date: 2024-11-26JIANGSU SENIOR NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113366.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the spraying process of lithium-ion batteries, PVDF dust is difficult to recycle, resulting in high production costs and affecting human health.

Method used

By mixing PVDF dust with thickener and water, filtering and iron removal treatment, a high-purity recovery slurry is prepared to improve the dispersion and utilization of PVDF particles in water.

Benefits of technology

It improves the utilization rate of PVDF slurry, reduces production costs, and reduces the impact of dust on human health, while ensuring the performance of the diaphragm bonding layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019710A_ABST
    Figure CN119019710A_ABST
Patent Text Reader

Abstract

The invention provides a method for recycling PVDF dust formed in the spraying process, and belongs to the technical field of battery material recycling. The method for recycling the PVDF dust formed in the spraying process comprises the following steps: providing the PVDF dust formed in the spraying process; wherein the PVDF surface in the PVDF dust is provided with an adhesive, and the mass ratio of the PVDF to the adhesive is 9: (0.5-2); pVDF dust, a thickening agent and water are mixed, and a mixed solution is obtained; carrying out filtering treatment and iron removal treatment on the mixed solution to obtain a slurry precursor; according to the method, PVDF dust formed in the spraying process can be recycled, so that the utilization rate of the PVDF slurry is increased, the production cost is reduced, and meanwhile, the influence of the dust on human health can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery material recycling, and in particular to a method for recycling PVDF dust generated during a spraying process. Background Art

[0002] PVDF (polyvinylidene fluoride) often acts as a binder in lithium-ion batteries. At present, it has been widely used in the bonding coating of battery separators to bond the separators and pole pieces. Specifically, in the process of using PVDF raw materials to prepare spray separators, water is usually used as a solvent, and then PVDF powder and polyacrylonitrile copolymer (an adhesive) are dissolved in water to form a slurry, and then the prepared slurry is sprayed on the surface of the separator to obtain a separator with a bonding coating. During the spraying process, a part of the slurry is not bonded to the surface of the separator after atomization, but enters the oven together with the separator and is dried into dust, and then remains near the machine; in addition, some particles that have been combined with the surface of the separator will fall off due to unstable bonding, which will also cause them to remain near the machine. Therefore, after the production line has been running for a period of time, a large amount of PVDF dust will remain near the corresponding machine, and this type of dust can easily flow in the air duct with the air flow. Therefore, there is an urgent need to develop a recycling process to recycle the PVDF dust generated during the spraying process, thereby improving the utilization rate of PVDF slurry, reducing production costs, and at the same time, reducing the impact of dust on human health. Summary of the invention

[0003] The purpose of the present application is to provide a method for recycling PVDF dust formed during the spraying process, which can recycle the PVDF dust formed during the spraying process, thereby improving the utilization rate of PVDF slurry, reducing production costs, and at the same time, reducing the impact of dust on human health.

[0004] The embodiment of the present application is implemented as follows:

[0005] The embodiment of the present application provides a method for recycling PVDF dust formed in a spraying process, comprising the following steps: providing PVDF dust formed in a spraying process; the PVDF surface in the PVDF dust has an adhesive, and the mass ratio of PVDF to the adhesive is 9:(0.5-2); mixing the PVDF dust, a thickener and water to obtain a mixed solution; filtering and deironing the mixed solution to obtain a slurry precursor; and mixing the slurry precursor, the adhesive and water to obtain a recycled slurry.

[0006] In the above technical scheme, on the one hand, the water solubility of PVDF particles themselves is poor; on the other hand, the solvent used in the process of preparing the spray slurry in the early stage is generally water. In order to reduce the pollution to PVDF particles during the recycling process, other non-aqueous solvents cannot be added, so water is also needed as a dispersing solvent in the recycling process. Therefore, how to solve the dispersibility problem of PVDF particles in water during the recycling process is particularly important. In this application, in the process of configuring the mixed solution, a thickener is added to improve the problem of poor dispersibility of PVDF particles of a specific composition (i.e., composed of PVDF and adhesives of a specific mass ratio) in water, so that PVDF particles can be better dispersed in water, so that various impurities mixed in PVDF particles are fully exposed, so that high-purity PVDF particles can be obtained after filtering and iron removal treatment. , At the same time, it can also reduce the risk of PVDF particles being intercepted as impurities due to agglomeration in the filtering treatment stage, thereby improving the recycling rate; Finally, the slurry precursor after impurity removal is mixed with adhesives and water to obtain a recovered slurry that can be used for machine spraying. The specific recycling process can recycle the PVDF dust generated during the spraying process, thereby improving the utilization rate of the PVDF slurry, reducing production costs, and at the same time reducing the impact of dust on human health.

[0007] In some alternative embodiments, the thickening agent comprises sodium carboxymethylcellulose.

[0008] Optionally, the viscosity of sodium carboxymethyl cellulose is 10 to 20 mPa·s.

[0009] Optionally, the degree of substitution of sodium carboxymethyl cellulose is 0.8-1.0.

[0010] In the above technical solution, sodium carboxymethyl cellulose is a macromolecule with good water solubility and a certain spatial skeleton structure. It is used as a thickener to allow PVDF particles to enter the internal space of sodium carboxymethyl cellulose, so that the PVDF particles can be better dispersed in water with the help of sodium carboxymethyl cellulose with good water solubility, so that various impurities mixed in the PVDF particles can be more fully exposed, so that after filtering and iron removal, PVDF particles with higher purity can be obtained. At the same time, the risk of PVDF particles being intercepted as impurities during the filtering stage due to agglomeration can be further reduced, thereby further improving the recovery rate of PVDF dust. In addition, although sodium carboxymethyl cellulose is an added substance, the performance of the bonding layer subsequently formed on the surface of the diaphragm will not be affected.

[0011] Furthermore, limiting the viscosity and degree of substitution of sodium carboxymethyl cellulose within specific ranges can better assist the dispersion of PVDF particles in water, and at the same time, can also make the subsequently obtained recycled slurry have a suitable viscosity, thereby improving the performance of the corresponding coating.

[0012] In some optional embodiments, in the step of preparing the mixed solution, the PVDF dust is 10 to 40 parts, the thickener is 0.1 to 1 part and the water is 30 to 89 parts, calculated by weight.

[0013] In the above technical scheme, the amount of each component is limited within a specific range so that the multiple components have a more suitable mass ratio, which is more conducive to the full dissolution and uniform dispersion of PVDF particles in water, so as to improve the overall stability of the mixed system. At the same time, it can also make the subsequent recycled slurry have a suitable viscosity, thereby improving the performance of the corresponding coating.

[0014] In some optional embodiments, the steps of preparing the mixed solution include: firstly mixing the thickener and water to obtain a mixed solution intermediate; and then mixing the PVDF dust and the mixed solution intermediate to obtain a mixed solution.

[0015] Optionally, in the process of first mixing the thickener and water, the processing speed is 500 to 3000 rpm and the processing time is 40 to 80 minutes.

[0016] Optionally, during the process of mixing the PVDF dust and the mixed solution intermediate, the processing rotation speed is 1500 to 3000 rpm and the processing time is 20 to 40 minutes.

[0017] In the above technical solution, after the thickener is mixed with water, PVDF dust is added to the mixed system, which helps to better disperse the PVDF particles in the water.

[0018] Furthermore, by limiting the processing speed and time in the two-stage mixing process to specific ranges, better dispersion effect can be achieved.

[0019] In some optional embodiments, in the filtering step, a vibrating screen is used for filtering.

[0020] Optionally, the specification of the vibrating screen is 50-100 meshes.

[0021] In the above technical solution, a vibrating filter screen is used in the filtering step to assist the mixed solution to flow, thereby improving the impurity removal efficiency and effect.

[0022] Furthermore, limiting the specifications of the vibrating screen to a specific range helps to better separate the PVDF particles from impurities.

[0023] In some optional embodiments, in the iron removal step, multiple magnetic rods connected in series are used for iron removal.

[0024] Optionally, the specification of a single magnetic rod is 8000-12000 GS.

[0025] In the above technical solution, multiple magnetic rods connected in series are used for iron removal, which can achieve a better iron removal effect. At the same time, the method of removing iron by magnetic rods is also relatively easy to implement.

[0026] Furthermore, limiting the specifications of a single magnetic bar within a specific range helps to further improve the iron removal effect.

[0027] In some optional embodiments, in the step of preparing the recycled slurry, the slurry precursor is 40-60 parts, the adhesive is 8-15 parts and the water is 40-70 parts, calculated by weight.

[0028] In the above technical scheme, the dosage of each component is limited within a specific range so that the multiple components in the recovered slurry have a more suitable dosage ratio. On the one hand, it can make the prepared recovered slurry have a suitable viscosity, thereby facilitating the subsequent coating process; on the other hand, it can make the bonding layer subsequently formed on the surface of the diaphragm have the advantages of strong bonding force and stable performance.

[0029] In some optional embodiments, the preparation steps of the recycled slurry include: first mixing an adhesive and water to obtain a slurry intermediate; and then mixing a slurry precursor and the slurry intermediate to obtain a recycled slurry.

[0030] Optionally, during the process of mixing the adhesive and water, the processing speed is 600 to 1000 rpm and the processing time is 20 to 40 minutes.

[0031] Optionally, during the process of mixing the slurry precursor and the slurry intermediate, the processing speed is 1500 to 3000 rpm and the processing time is 100 to 140 minutes.

[0032] In the above technical solution, the adhesive is mixed with water and then the slurry precursor is added to the mixed system, which helps to better disperse the PVDF particles in the slurry precursor in the water.

[0033] Furthermore, by limiting the processing speed and time in the two-stage mixing process to specific ranges, better dispersion effect can be achieved.

[0034] In some optional embodiments, the method for recycling PVDF dust formed in the spraying process also includes: directly using the recovered slurry for spraying on a machine; or, mixing the recovered slurry and the spraying slurry to form a mixture and then spraying on a machine.

[0035] In the above technical solution, the prepared recycled slurry can be used alone or mixed with the spraying slurry during the spraying stage, and there are many feasible implementation methods, which facilitates the promotion and application of the technical solution provided in the embodiment of the present application.

[0036] In some optional embodiments, the mass ratio of the recovered slurry to the spraying slurry is (0.1-1):1.

[0037] In the above technical solution, when the recycled slurry and the spraying slurry are mixed for use, the mass ratio of the two is limited to a specific range, so that the bonding layer subsequently formed on the surface of the diaphragm has the advantage of relatively stable performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 A process flow chart of a method for recycling PVDF dust formed during a spraying process provided in an embodiment of the present application;

[0040] Figure 2 This is a microscopic image of the bonding layer of the spray-coated diaphragm corresponding to Example 1 of the present application;

[0041] Figure 3 This is a microscopic image of the bonding layer of the spray-coated diaphragm corresponding to Example 2 of the present application;

[0042] Figure 4 This is a microscopic image of the bonding layer of the spray-coated diaphragm corresponding to Comparative Example 1 of the present application;

[0043] Figure 5 This is a microscopic image of the bonding layer of the spray-coated diaphragm corresponding to Comparative Example 1 of the present application;

[0044] Figure 6 This is a physical picture of the settled particles in the recovered slurry corresponding to Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0046] It should be noted that “and / or” in this application, such as “Feature 1 and / or Feature 2”, refers to the three situations of “Feature 1” alone, “Feature 2” alone, or “Feature 1” plus “Feature 2”.

[0047] In addition, in the description of the present application, unless otherwise specified, the meaning of "multiple" in "one or more" refers to two or more; the range of "value a ~ value b" includes the two end values ​​"a" and "b", and the "unit" in "value a ~ value b + unit of measurement" represents the "unit of measurement" of both "value a" and "value b".

[0048] The following is a detailed description of the method for recycling PVDF dust formed during the spraying process in an embodiment of the present application.

[0049] The embodiment of the present application provides a method for recycling PVDF dust formed in a spraying process, comprising the following steps: providing PVDF dust formed in a spraying process; the PVDF surface in the PVDF dust has an adhesive, and the mass ratio of PVDF to the adhesive is 9:(0.5-2); mixing the PVDF dust, a thickener and water to obtain a mixed solution; filtering and deironing the mixed solution to obtain a slurry precursor; and mixing the slurry precursor, the adhesive and water to obtain a recycled slurry.

[0050] In this application, on the one hand, the water solubility of PVDF particles themselves is poor; on the other hand, the solvent used in the early stage of preparing the spray slurry is generally water. In order to reduce the pollution to PVDF particles during the recycling process, other non-aqueous solvents cannot be added, so water is also needed as a dispersing solvent in the recycling process. Therefore, how to solve the dispersibility problem of PVDF particles in water during the recycling process is particularly important. In this application, in the process of configuring the mixed solution, a thickener is added to improve the problem of poor dispersibility of PVDF particles of a specific composition (i.e., composed of PVDF and adhesives of a specific mass ratio) in water, so that PVDF particles can be better dispersed in water, so that various impurities mixed in PVDF particles are fully exposed, so that high-purity PVDF particles can be obtained after filtering and iron removal treatment. , At the same time, it can also reduce the risk of PVDF particles being intercepted as impurities due to agglomeration in the filtering treatment stage, thereby improving the recycling rate; Finally, the slurry precursor after impurity removal is mixed with adhesives and water to obtain a recovered slurry that can be used for machine spraying. The specific recycling process can recycle the PVDF dust generated during the spraying process, thereby improving the utilization rate of the PVDF slurry, reducing production costs, and at the same time reducing the impact of dust on human health.

[0051] It should be noted that there is no limitation on the method of removing the PVDF dust generated during the spraying process. For example, a dust collecting device may be directly used to collect the PVDF dust near the machine.

[0052] It should be noted that after the mass fraction of the adhesive is determined, it is usually added in the form of a liquid with a solid content of 15%.

[0053] It should be noted that the order of the filtration treatment and the iron removal treatment is not limited. For example, the filtration treatment may be performed first and then the iron removal treatment, or the iron removal treatment may be performed first and then the filtration treatment.

[0054] It should be noted that the filtration treatment stage is mainly used to remove some broken films, fibers and hair in the PVDF dust; the iron removal treatment stage is mainly used to remove some metal debris in the PVDF dust.

[0055] It is understandable that the thickener should not only be able to assist the PVDF particles to be evenly dispersed in water, but also the use of the thickener should have a sufficiently small effect on the performance of the bonding layer subsequently formed on the surface of the diaphragm.

[0056] As an example, the thickening agent includes sodium carboxymethylcellulose.

[0057] In this embodiment, sodium carboxymethyl cellulose is a macromolecule with good water solubility and a certain spatial skeleton structure. It is used as a thickener to allow PVDF particles to enter the internal space of sodium carboxymethyl cellulose, so that the PVDF particles can be better dispersed in water with the help of sodium carboxymethyl cellulose with good water solubility, so that various impurities mixed in the PVDF particles can be more fully exposed, so that after filtering and iron removal, PVDF particles with higher purity can be obtained. At the same time, the risk of PVDF particles being intercepted as impurities during the filtering treatment stage due to agglomeration can be further reduced, thereby further improving the recovery rate of PVDF dust. In addition, although sodium carboxymethyl cellulose is used as a thickener, the performance of the bonding layer subsequently formed on the surface of the diaphragm will not be affected.

[0058] As an example, the viscosity of sodium carboxymethyl cellulose is 10 to 20 mPa·s, for example, but not limited to, any one of 10 mPa·s, 12 mPa·s, 14 mPa·s, 16 mPa·s, 18 mPa·s and 20 mPa·s, or a range between any two of them; wherein the viscosity refers to the viscosity of sodium carboxymethyl cellulose alone when it is configured into an aqueous solution with a mass concentration of 1%.

[0059] As an example, the degree of substitution of sodium carboxymethyl cellulose is 0.8-1.0, for example but not limited to any one of 0.8, 0.85, 0.9, 0.95 and 1, or a range between any two of them.

[0060] In this embodiment, the viscosity and degree of substitution of sodium carboxymethyl cellulose are further limited within specific ranges, which can better assist the dispersion of PVDF particles in water. At the same time, it can also make the subsequently obtained recycled slurry have a suitable viscosity, thereby improving the performance of the corresponding coating.

[0061] As an example, in the preparation step of the mixed solution, by weight, 10 to 40 parts of PVDF dust, 0.1 to 1 part of thickener and 30 to 89 parts of water are used.

[0062] In this embodiment, the amount of each component is limited to a specific range so that the multiple components have a more suitable mass ratio, which is more conducive to the full dissolution and uniform dispersion of PVDF particles in water, so as to improve the overall stability of the mixed system. At the same time, it can also make the subsequently obtained recycled slurry have a suitable viscosity, thereby improving the performance of the corresponding coating.

[0063] As an example, the steps of preparing the mixed solution include: firstly mixing a thickener and water to obtain a mixed solution intermediate; and then mixing PVDF dust and the mixed solution intermediate to obtain a mixed solution.

[0064] In this embodiment, the thickener is mixed with water and then PVDF dust is added to the mixed system, which helps to better disperse the PVDF particles in the water.

[0065] In other possible implementations, the thickener and PVDF dust may be added into water for mixing.

[0066] As an example, in the process of mixing the thickener and water, the processing speed is 500-3000 rpm, for example but not limited to the processing speed of any one of 500 rpm, 1000 rpm, 1500 rpm, 2000 rpm, 2500 rpm and 3000 rpm or a range between any two of them; the processing time is 40-80 min, for example but not limited to the processing time of any one of 40 min, 50 min, 60 min, 70 min and 80 min or a range between any two of them.

[0067] As an example, in the process of mixing the PVDF dust and the mixed solution intermediate, the processing speed is 1500-3000rpm, for example but not limited to the processing speed of any one of 1500rpm, 2000rpm, 2500rpm and 3000rpm or the range value between any two; the processing time is 20-40min, for example but not limited to the processing time of any one of 20min, 25min, 30min, 35min and 40min or the range value between any two.

[0068] In this embodiment, the processing speed and time in the two-stage mixing process are further limited to specific ranges, so that a better dispersion effect can be achieved.

[0069] As an example, in the filtering step, a vibrating screen is used for filtering.

[0070] In this embodiment, a vibrating filter screen is used in the filtering step to assist the mixed solution in flowing, thereby improving the impurity removal efficiency and effect.

[0071] As an example, the specification of the vibrating screen is 50-100 meshes, for example but not limited to any one of 50 meshes, 60 meshes, 70 meshes, 80 meshes, 90 meshes and 100 meshes or a range between any two of them.

[0072] In this embodiment, the specifications of the vibrating screen are further limited within a specific range, which helps to better separate the PVDF particles and impurities.

[0073] As an example, in the step of iron removal, multiple magnetic rods connected in series are used for iron removal.

[0074] In this embodiment, multiple magnetic rods connected in series are used for iron removal, which can achieve a better iron removal effect. At the same time, the method of removing iron by magnetic rods is also relatively easy to implement.

[0075] As an example, the specification of a single magnetic rod is 8000-12000 GS, such as but not limited to any one of 8000 GS, 9000 GS, 10000 GS, 11000 GS and 12000 GS or a range between any two of the specifications.

[0076] In this embodiment, the specification of a single magnetic rod is further limited within a specific range, which helps to further improve the iron removal effect.

[0077] It should be noted that the time for iron removal treatment is not limited and can be adjusted according to actual needs, for example, 10 to 30 minutes.

[0078] As an example, in the preparation step of the recycled slurry, the slurry precursor is 40 to 60 parts, the adhesive is 8 to 15 parts and the water is 40 to 70 parts, calculated by weight.

[0079] In this embodiment, the dosage of each component is limited within a specific range so that the multiple components in the recovered slurry have a more suitable dosage ratio. On the one hand, the prepared recovered slurry can have a suitable viscosity, thereby facilitating the subsequent coating process; on the other hand, the bonding layer subsequently formed on the surface of the diaphragm has the advantages of strong bonding force and stable performance.

[0080] It should be noted that the type of adhesive is not limited and can be selected according to conventional methods in the art, for example, it can be a polyacrylonitrile copolymer.

[0081] As an example, the preparation steps of the recycled slurry include: first mixing an adhesive and water to obtain a slurry intermediate; then mixing a slurry precursor and the slurry intermediate to obtain a recycled slurry.

[0082] In this embodiment, the adhesive is mixed with water and then the slurry precursor is added to the mixed system, which helps to better disperse the PVDF particles in the slurry precursor in the water.

[0083] As an example, in the process of mixing the adhesive and water, the processing speed is 600-1000rpm, for example but not limited to the processing speed of any one point value of 600rpm, 700rpm, 800rpm, 900rpm and 1000rpm or the range value between any two; the processing time is 20-40min, for example but not limited to the processing time of any one point value of 20min, 25min, 30min, 35min and 40min or the range value between any two.

[0084] As an example, in the process of mixing the slurry precursor and the slurry intermediate, the processing speed is 1500-3000 rpm, for example but not limited to the processing speed of any one of 1500 rpm, 2000 rpm, 2500 rpm and 3000 rpm or the range value between any two; the processing time is 100-140 min, for example but not limited to the processing time of any one of 100 min, 110 min, 120 min, 130 min and 140 min or the range value between any two.

[0085] In this embodiment, the processing speed and time in the two-stage mixing process are further limited to specific ranges, so that a better dispersion effect can be achieved.

[0086] As an example, the method for recycling PVDF dust formed in the spraying process also includes: directly using the recycled slurry for spraying; or mixing the recycled slurry with the spraying slurry to form a mixture and then spraying it on the machine.

[0087] In this embodiment, the prepared recycled slurry can be used alone or mixed with the spraying slurry during the spraying stage, and there are many feasible implementation methods, which facilitates the promotion and application of the technical solution provided in the embodiment of the present application.

[0088] It should be noted that the slurry for spraying refers to the slurry directly prepared by using PVDF raw materials according to normal processes, and this application does not provide additional explanation on the preparation process of the slurry for spraying.

[0089] As an example, the mass ratio of the recovered slurry to the spraying slurry is (0.1-1):1, for example but not limited to the mass ratio of any one of 0.1:1, 0.2:1, 0.4:1, 0.6:1, 0.8:1 and 1:1 or a range between any two of them.

[0090] In this embodiment, when the recovered slurry and the spraying slurry are mixed for use, the mass ratio of the two is limited to a specific range, so that the bonding layer subsequently formed on the surface of the diaphragm has the advantage of relatively stable performance.

[0091] It should be noted that, in the process of recycling the PVDF dust formed during the spraying process, the processes or steps not specifically described or limited can be arranged according to the conventional selection in the art.

[0092] As an example, the process flow chart of the method for recycling PVDF dust formed during the spraying process is shown in FIG. Figure 1 .

[0093] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0094] Example 1

[0095] The present application embodiment provides a method for recycling PVDF dust generated during a spraying process, comprising the following steps:

[0096] Provide PVDF dust formed during the spraying process, wherein the mass ratio of PVDF to adhesive is 9:1; 0.25 parts of sodium carboxymethyl cellulose (thickener, viscosity of 15mPa·s, degree of substitution of 0.9) and 36.25 parts of water are mixed by mass to obtain a mixed solution intermediate; 15 parts of PVDF dust are added to the mixed solution intermediate and mixed to obtain a mixed solution. In the process of mixing the thickener and water, the processing speed is 2000rpm and the processing time is 60min; in the process of mixing the PVDF dust and the mixed solution intermediate, the processing speed is 2000rpm and the processing time is 30min.

[0097] The mixed solution was passed through an 80-mesh vibrating screen to remove impurities in the mixed solution; then, two 10,000 GS magnetic bars were connected in series to remove iron from the collected filtrate for 20 minutes to obtain a slurry precursor.

[0098] According to the mass fraction, 11.1 parts of (polyacrylonitrile copolymer) adhesive and 56.4 parts of water are mixed to obtain a slurry intermediate; then 51.5 parts of slurry precursor (i.e., all slurry precursors) are added to the slurry intermediate and mixed to obtain a recycled slurry. In the process of mixing the adhesive and water, the processing speed is 800 rpm and the processing time is 30 minutes; in the process of mixing the slurry precursor and the slurry intermediate, the processing speed is 2000 rpm and the processing time is 120 minutes.

[0099] The prepared recycled slurry is directly sprayed onto the surface of the diaphragm to form a diaphragm with a bonding layer.

[0100] Example 2

[0101] This embodiment of the present application provides a method for recycling PVDF dust generated during the spraying process, which differs from Embodiment 1 only in that:

[0102] After the recycled slurry is prepared, the method further includes preparing a slurry for spraying. Specifically, 11.1 parts of (polyacrylonitrile copolymer) adhesive and 92.9 parts of water are mixed by weight to obtain a slurry intermediate; and 15 parts of PVDF raw material powder are added to the slurry intermediate and mixed to obtain a slurry for spraying. In the process of mixing the adhesive and water, the processing speed is 800 rpm and the processing time is 30 minutes; in the process of mixing the PVDF raw material powder and the slurry intermediate, the processing speed is 2000 rpm and the processing time is 120 minutes.

[0103] The recovered slurry is then mixed with the spraying slurry in a mass ratio of 1:1 to obtain a mixture, and the mixture is then sprayed onto the surface of the diaphragm to form a diaphragm with a bonding layer.

[0104] Comparative Example 1

[0105] The comparative example of the present application provides a method for recycling PVDF dust formed in the spraying process, which is different from Example 1 only in that no thickener is used in the process of preparing the recycled slurry.

[0106] Comparative Example 1

[0107] The comparative example of the present application provides a method for preparing a slurry for spraying, comprising the following steps:

[0108] According to the mass fraction, 11.1 parts of (polyacrylonitrile copolymer) adhesive and 92.9 parts of water were mixed to obtain a slurry intermediate; 15 parts of PVDF raw material powder were added to the slurry intermediate and mixed to obtain a slurry for spraying. In the process of mixing the adhesive and water, the processing speed was 800 rpm and the processing time was 30 minutes; in the process of mixing the PVDF raw material powder and the slurry intermediate, the processing speed was 2000 rpm and the processing time was 120 minutes.

[0109] It should be noted that the mass proportion of PVDF particles in the slurry before spraying in Control Example 1 and Example 1 is the same.

[0110] Test Example 1

[0111] Basic performance test of slurry

[0112] Test method:

[0113] The slurries before spraying prepared in Examples 1 to 2, Comparative Example 1 and Reference Example 1 were numbered respectively, and then the particle size D50 and D99, solid content and viscosity of each slurry were tested.

[0114] Table 1 Performance statistics of each slurry

[0115] Sample D50(μm) D99(μm) Solid content (%) Viscosity(cPs) Example 1 8.078 92.207 13.29 87.5 Example 2 5.872 76.502 14.1 85.7 Comparative Example 1 15.936 113.5 8.5 63 Comparative Example 1 3.824 61.024 14.02 81.7

[0116] Test Example 2

[0117] Basic performance test of the product

[0118] Test method:

[0119] The separators with adhesive layers prepared in Examples 1 to 2, Comparative Example 1 and Reference Example 1 were numbered respectively, and then the thickness, surface density, air permeability and hot pressing bonding strength of each adhesive layer were tested.

[0120] Table 2 Performance statistics of each product

[0121] Sample Thickness(μm) <![CDATA[Areal density (g / m 2 )]]> Air permeability(s) Hot press bonding strength (N / m) Example 1 23.2 10.56 185.2 3.87 Example 2 22.25 10.71 175.5 2.76 Comparative Example 1 23 10.51 183.2 1.93 Comparative Example 1 22.15 10.69 173.3 2.55

[0122] Test Example 3

[0123] Microscopic morphology characterization of products

[0124] Test method:

[0125] The membranes with adhesive layers prepared in Examples 1 to 2, Comparative Example 1, and Control Example 1 were numbered respectively, and then the microscopic images of each adhesive layer were tested using a microscope, wherein the eyepiece magnification was 60 times, the objective lens magnification was 1.25 times, and the total magnification was 75 times.

[0126] In summary, refer to Tables 1 to 3 and Figure 2 to Figure 5 , it can be seen from the test results of Examples 1 to 2 and Comparative Example 1 that the recycling process provided by the embodiments of the present application can realize the recycling of PVDF dust formed during the spraying process, and the performance of the spray diaphragm prepared by the embodiment of the present application is basically consistent with that of the spray diaphragm prepared by the existing process, so as to improve the utilization rate of PVDF slurry in the process of preparing the spray diaphragm, reduce production costs, and at the same time, reduce the impact of dust on human health. In addition, under the same mass proportion, that is, the mass proportion of PVDF particles in the slurry before spraying is the same, compared with the slurry corresponding to the raw material PVDF particles, the slurry corresponding to the recycled PVDF particles has a higher viscosity, and the corresponding bonding layer also has a higher bonding force, which may be due to the adhesive remaining on the surface of the recycled PVDF particles.

[0127] It can be seen from the test results of Example 1 and Comparative Example 1 that the use of a thickener to assist the dispersion of PVDF particles in water during the recycling process helps the PVDF particles to be better dispersed in water, thereby fully exposing various impurities mixed in the PVDF particles, so that high-purity PVDF particles can be obtained after filtration and iron removal treatment. At the same time, the risk of PVDF particles being intercepted as impurities during the filtration treatment stage due to agglomeration can be reduced, thereby improving the recycling rate. Therefore, the particle size at each stage in Example 1 is smaller than that in Comparative Example 1, but the solid content, viscosity and hot pressing bonding force in Example 1 are greater than those in Comparative Example 1. In addition, the inventors also found that if a thickener is not used, the prepared recycled slurry still has a more serious particle sedimentation phenomenon, which can be found in detail. Figure 6 .

[0128] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A method for recycling PVDF dust generated during a spraying process, characterized in that: The following steps are involved: Providing PVDF dust formed during the spraying process; wherein the surface of the PVDF in the PVDF dust has an adhesive, and the mass ratio of PVDF to the adhesive is 9:(0.5-2); Mixing the PVDF dust, thickener and water to obtain a mixed solution; filtering and removing iron from the mixed solution to obtain a slurry precursor; and The slurry precursor, adhesive and water are mixed to obtain a recycled slurry.

2. The method for recycling PVDF dust generated during the spraying process according to claim 1, characterized in that: The thickener includes sodium carboxymethyl cellulose; Optionally, the viscosity of the sodium carboxymethyl cellulose is 10 to 20 mPa·s; Optionally, the degree of substitution of the sodium carboxymethyl cellulose is 0.8 to 1.

0.

3. The method for recycling PVDF dust generated during the spraying process according to claim 1, characterized in that: In the step of preparing the mixed solution, the PVDF dust is 10 to 40 parts, the thickener is 0.1 to 1 part and the water is 30 to 89 parts by weight.

4. The method for recycling PVDF dust generated during the spraying process according to claim 3, characterized in that: The steps of preparing the mixed solution include: Firstly, the thickener and water are mixed to obtain a mixed solution intermediate; then, the PVDF dust and the mixed solution intermediate are mixed to obtain the mixed solution; Optionally, in the process of first mixing the thickener and water, the processing speed is 500 to 3000 rpm and the processing time is 40 to 80 minutes; Optionally, in the process of mixing the PVDF dust and the mixed solution intermediate, the processing rotation speed is 1500-3000 rpm and the processing time is 20-40 min.

5. The method for recycling PVDF dust generated during spraying according to any one of claims 1 to 4, characterized in that: In the filtering step, a vibrating screen is used for filtering; Optionally, the vibrating screen has a size of 50 to 100 meshes.

6. The method for recycling PVDF dust generated during spraying according to any one of claims 1 to 4, characterized in that: In the step of iron removal, a plurality of magnetic rods connected in series are used for iron removal; Optionally, the specification of a single magnetic rod is 8000-12000GS.

7. The method for recycling PVDF dust generated during spraying according to any one of claims 1 to 4, characterized in that: In the step of preparing the recycled slurry, the slurry precursor is 40 to 60 parts, the adhesive is 8 to 15 parts and water is 40 to 70 parts, calculated by weight.

8. The method for recycling PVDF dust generated during the spraying process according to claim 7, characterized in that: The steps of preparing the recovered slurry include: Firstly, the adhesive and water are mixed to obtain a slurry intermediate; then, the slurry precursor and the slurry intermediate are mixed to obtain the recycled slurry; Optionally, in the process of mixing the adhesive and water, the processing speed is 600-1000 rpm and the processing time is 20-40 min; Optionally, in the process of mixing the slurry precursor and the slurry intermediate, the processing speed is 1500-3000 rpm and the processing time is 100-140 min.

9. The method for recycling PVDF dust generated during spraying according to any one of claims 1 to 4, characterized in that: Also includes: The step of directly using the recycled slurry to carry out spraying on a machine; or the step of mixing the recycled slurry with spraying slurry to form a mixture and then carrying out spraying on a machine.

10. The method for recycling PVDF dust generated during the spraying process according to claim 9, characterized in that: The mass ratio of the recovered slurry to the spraying slurry is (0.1-1):1.