Yellow-green switchable electrochromic film and preparation method thereof

CN119019719APending Publication Date: 2024-11-26ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411141032.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

Smart Images

  • Figure CN119019719A_ABST
    Figure CN119019719A_ABST
Patent Text Reader

Abstract

The invention provides a yellow-green switchable electrochromic film and a preparation method thereof, and belongs to the technical field of optical materials. Two ternary random copolymers FEP and FTP are prepared through arylation polycondensation, can be switched between yellow and green under the action of external voltage, have high optical contrast in the wavelength range of 460 nm, and are short in coloring time and fading time; after 1000 cycles under the step voltage of 0V and 1V, the optical contrast at 460 nm can still keep 69% or more of the original contrast, and the electrochromic material is two kinds of electrochromic materials which are excellent in property and can be switched between yellow and green; and the electrochromic camouflage net device prepared on the basis of the two electrochromic materials shows different colors and camouflage effects under different voltages, so that the purpose of camouflage in different environments can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical materials, and in particular to an electrochromic film capable of switching between yellow and green and a preparation method thereof. Background Art

[0002] Camouflage net is a camouflage device with two different camouflage patterns, which can adapt to different backgrounds in two or three seasons in most parts of my country. However, it lacks the ability to actively change color, which limits its potential application. Faced with complex and changeable combat environments, it is often necessary to use a variety of camouflage nets to achieve the best camouflage effect. Electrochromism refers to the phenomenon that the color of a material changes reversibly under the action of an applied electric field. At present, the yellow-green switching electrochromic material system is relatively complete, but there are few high-performance, wide-adjustment range yellow-green switching electrochromic polymer materials. Based on this, providing an electrochromic material with low driving voltage and high cycle stability is of great significance in the field of camouflage equipment. Summary of the invention

[0003] The object of the present invention is to provide an electrochromic film capable of switching between yellow and green and a preparation method thereof, so as to solve the technical problems of high driving voltage and poor cycle stability of existing electrochromic materials.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing a yellow-green switchable electrochromic film, comprising the following steps:

[0006] 1) reacting 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin, a thiophene compound, anhydrous potassium carbonate, pivalic acid, and Pd(OAc)2 in anhydrous dimethylacetamide to obtain a reaction mixture;

[0007] 2) mixing the reaction mixture obtained in step 1) with methanol, and sequentially filtering, washing, extracting and evaporating to obtain a product;

[0008] 3) mixing the product obtained in step 2) with chloroform and coating the mixture to obtain an electrochromic film capable of switching between yellow and green;

[0009] The structural formulas of the 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine and 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin are shown in Formula I and Formula II respectively:

[0010] Formula I: Formula II:

[0011] In Formula I and Formula II,

[0012] Furthermore, in step 1), the thiophene compound includes 3,4-ethylenedioxythiophene or 3-methylthiophene.

[0013] Further, in step 1), when the thiophene compound is 3,4-ethylenedioxythiophene, the mass ratio of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin and 3,4-ethylenedioxythiophene is 1.8:2.4:1;

[0014] The mass ratio of anhydrous potassium carbonate to 3,4-ethylenedioxythiophene is 1.2 to 2:1;

[0015] The mass ratio of pivalic acid to 3,4-ethylenedioxythiophene is 0.3-0.6:1;

[0016] The mass ratio of Pd(OAc)2 to 3,4-ethylenedioxythiophene is 0.3-0.6:1;

[0017] The added volume of the anhydrous dimethylacetamide is 50 to 80 mL / g based on the mass of 3,4-ethylenedioxythiophene.

[0018] Further, in step 1), when the thiophene compound is 3-methylthiophene, the mass ratio of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin and 3-methylthiophene is 2.3:3:1;

[0019] The mass ratio of anhydrous potassium carbonate to 3-methylthiophene is 1.5-2.5:1;

[0020] The mass ratio of pivalic acid to 3-methylthiophene is 1.5 to 3:1;

[0021] The mass ratio of Pd(OAc)2 to 3-methylthiophene is 1.5 to 3:1;

[0022] The added volume of the anhydrous dimethylacetamide is 80 to 120 mL / g based on the mass of 3-methylthiophene.

[0023] Furthermore, in step 1), the reaction temperature is 120-150° C., and the reaction time is 16-20 h.

[0024] Furthermore, in step 2), the extraction is an organic solvent extraction method, the order of the organic solvents is methanol, acetone, petroleum ether and chloroform, and the amount of the organic solvent is 200-300 mL;

[0025] The products include FEP or FTP.

[0026] Furthermore, in step 3), the ratio of the product to chloroform is 8-12 mg:1 mL.

[0027] Furthermore, in step 3), the coating includes spray coating or spin coating.

[0028] The invention provides an electrochromic film capable of switching between yellow and green and prepared by the above-mentioned preparation method.

[0029] Furthermore, the thickness of the electrochromic film is 50 nm to 5 μm.

[0030] Beneficial effects of the present invention:

[0031] The electrochromic film capable of switching from yellow to green of the present invention: FEP (I) exhibits yellow in a neutral state (0V) and exhibits a green state in an oxidized state (0.7V), and the optical contrast ratio in a wavelength range of 460nm is 26%, the coloring time is 0.93s, and the fading time is 2.19s. After 1000 cycles under a step voltage of 0V and 1V, the optical contrast ratio at 460nm can still maintain 83.7% of the original contrast ratio; FTP (II) exhibits yellow in a neutral state (0V) and exhibits a green state in an oxidized state (0.9V), and the optical contrast ratio in a wavelength range of 440nm is 18%, the coloring time is 0.83s, and the fading time is 2.95s. After 1000 cycles under a step voltage of 0V and 1V, the optical contrast ratio at 440nm can still maintain 69.2% of the original contrast ratio. The two electrochromic materials capable of switching from yellow to green have excellent properties. In addition, the electrochromic camouflage net device assembled based on these two yellow-green switchable electrochromic materials can be used in the field of military camouflage. The color of the film can be changed by applying different voltages to achieve the purpose of camouflage on different battlefields. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The synthetic route map for FEP and FTP;

[0033] Figure 2 The cyclic voltammetry curves of the yellow-green switchable electrochromic film prepared in Example 1 at different scanning speeds;

[0034] Figure 3 Cyclic voltammetry curves of the yellow-green switchable electrochromic film prepared in Example 2 at different scanning speeds;

[0035] Figure 4 The UV-visible absorption spectra of the yellow-green switchable electrochromic film prepared in Example 1 at different voltages;

[0036] Figure 5 The UV-visible absorption spectra of the yellow-green switchable electrochromic film prepared in Example 2 at different voltages;

[0037] Figure 6 This is a relationship diagram between the wavelength range and response time of the yellow-green switchable electrochromic film prepared in Example 1;

[0038] Figure 7 This is a relationship diagram between the wavelength range and response time of the yellow-green switchable electrochromic film prepared in Example 2;

[0039] Figure 8 This is a relationship diagram between the wavelength range and stability of the yellow-green switchable electrochromic film prepared in Example 1;

[0040] Fig. 9 This is a relationship diagram between the wavelength range and stability of the yellow-green switchable electrochromic film prepared in Example 2;

[0041] Fig.10 The color coordinate diagram of the yellow-green switchable electrochromic film prepared in Example 1 at different voltages (the right end point of the broken line is the starting point);

[0042] Fig.11 The color coordinate diagram of the yellow-green switchable electrochromic film prepared in Example 2 at different voltages (the right end point of the broken line is the starting point);

[0043] Fig.12 This is a graph showing the brightness change of the yellow-green switchable electrochromic film prepared in Example 1 at different voltages;

[0044] Fig.13 This is a graph showing the brightness change of the yellow-green switchable electrochromic film prepared in Example 2 at different voltages;

[0045] Fig.14 This is a schematic diagram of a hollow mask in Example 5, where the black square is the hollow part;

[0046] Fig.15 This is a photo of the yellow-green switchable electrochromic camouflage net assembled in Example 5;

[0047] Fig.16 These are photos of the yellow-green switchable electrochromic camouflage net assembled in Example 5 under different voltages. DETAILED DESCRIPTION

[0048] The present invention provides a method for preparing a yellow-green switchable electrochromic film, comprising the following steps:

[0049] 1) reacting 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin, a thiophene compound, anhydrous potassium carbonate, pivalic acid, and Pd(OAc)2 in anhydrous dimethylacetamide to obtain a reaction mixture;

[0050] 2) mixing the reaction mixture obtained in step 1) with methanol, and sequentially filtering, washing, extracting and evaporating to obtain a product;

[0051] 3) mixing the product obtained in step 2) with chloroform and coating the mixture to obtain an electrochromic film capable of switching between yellow and green;

[0052] The structural formulas of the 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine and 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin are shown in Formula I and Formula II respectively:

[0053] Formula I: Formula II:

[0054] In Formula I and Formula II,

[0055] In the present invention, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin is synthesized according to the document J Polym Sci. 2021; 59: 2771-2782.

[0056] In the present invention, in step 1), the thiophene compound includes 3,4-ethylenedioxythiophene or 3-methylthiophene, preferably 3,4-ethylenedioxythiophene.

[0057] In the present invention, in step 1), when the thiophene compound is 3,4-ethylenedioxythiophene, the mass ratio of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin and 3,4-ethylenedioxythiophene is 1.5-2.7:1-2.5:1, preferably 1.8:1.6-2.4:1, and more preferably 1.8:2:1;

[0058] The mass ratio of anhydrous potassium carbonate to 3,4-ethylenedioxythiophene is 1.2 to 2:1, preferably 1.2:1;

[0059] The mass ratio of pivalic acid to 3,4-ethylenedioxythiophene is 0.3-0.6:1, preferably 0.5:1;

[0060] The mass ratio of Pd(OAc)2 to 3,4-ethylenedioxythiophene is 0.3-0.6:1, preferably 0.5:1;

[0061] The added volume of the anhydrous dimethylacetamide is 50 to 80 mL / g, preferably 60 to 70 mL / g, and more preferably 70 mL / g, based on the mass of 3,4-ethylenedioxythiophene.

[0062] In the present invention, in step 1), when the thiophene compound is 3-methylthiophene, the mass ratio of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin and 3-methylthiophene is 2-2.5:2.5-3.5:1, preferably 2.2-2.4:2.7-3.2:1, and more preferably 2.3:3:1;

[0063] The mass ratio of anhydrous potassium carbonate to 3-methylthiophene is 1.5-2.5:1, preferably 2:1;

[0064] The mass ratio of pivalic acid to 3-methylthiophene is 1.5 to 3:1, preferably 1.5 to 2:1, and more preferably 1.7:1;

[0065] The mass ratio of Pd(OAc)2 to 3-methylthiophene is 1.5 to 3:1, preferably 1.7 to 2.8:1, more preferably 2 to 2.5:1, and more preferably 2.3:1;

[0066] The added volume of the anhydrous dimethylacetamide is 80 to 120 mL / g, preferably 90 to 110 mL / g, and more preferably 100 mL / g, based on the mass of 3-methylthiophene.

[0067] In the present invention, in step 1), the reaction temperature is 120-150° C., preferably 130-140° C., more preferably 135° C., and the reaction time is 16-20 h, preferably 17-19 h, more preferably 18 h.

[0068] In the present invention, in step 2), the extraction is an organic solvent extraction method, the order of the organic solvents is preferably methanol, acetone, petroleum ether and chloroform, and the amount of the organic solvent is 200-300 mL, preferably 220-280 mL, and more preferably 250 mL;

[0069] The product comprises FEP or FTP, preferably FEP.

[0070] In the present invention, the structural formulas of FEP and FTP are shown in Formula III and Formula IV:

[0071] Formula III:

[0072] Formula IV:

[0073] In the present invention, in step 3), the usage ratio of the product to chloroform is 8-12 mg:1 mL, preferably 10 mg:1 mL.

[0074] In the present invention, in step 3), the coating liquid used for coating is prepared by dissolving FEP and / or FTP in an organic solvent, preferably FEP and FTP.

[0075] In the present invention, the organic solvent includes dichloromethane, chloroform or tetrahydrofuran, preferably dichloromethane or chloroform, and more preferably chloroform.

[0076] In the present invention, the coated substrate is preferably ITO glass, FTO conductive glass, or ITO-PET conductive film.

[0077] In the present invention, when the coating liquid is mixed and coated by FEP and FTP, the mass ratio of FEP to FTP is 1:1-5, preferably 1:2-4, and more preferably 1:3.

[0078] In the present invention, in step 3), the coating comprises spray coating or spin coating, preferably spray coating.

[0079] In the present invention, when spin coating is used for coating, the concentration of the coating solution for spin coating is 5 to 20 mg / mL, preferably 10 to 18 mg / mL, and more preferably 15 mg / mL;

[0080] The rotation speed of the spin coating is 500 to 3000 r / min, preferably 1000 to 2500 r / min, more preferably 1500 to 2000 r / min, and more preferably 1800 r / min;

[0081] The spin coating time is 5 s to 10 min, preferably 30 s to 8 min, more preferably 1 min to 5 min, and even more preferably 3 min.

[0082] In the present invention, when spray coating is used, the concentration of the spray coating liquid is 3 to 15 mg / mL, preferably 5 to 12 mg / mL, more preferably 8 to 10 mg / mL, and more preferably 9 mg / mL;

[0083] The angle between the spray gun and the substrate is 15 to 90°, preferably 30 to 70°, more preferably 45 to 60°, and more preferably 50°;

[0084] The flow rate of the spray gun is 3 to 10 L / min, preferably 5 to 8 L / min, and more preferably 7 L / min;

[0085] The diameter of the spray gun is 1 to 5 mm, preferably 2 to 4 mm, and more preferably 3 mm.

[0086] The invention provides an electrochromic film capable of switching between yellow and green and prepared by the above-mentioned preparation method.

[0087] In the present invention, the thickness of the electrochromic film is 50 nm to 5 μm, preferably 100 nm to 3 μm, more preferably 200 nm to 2 μm, and even more preferably 1 μm.

[0088] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0089] Example 1

[0090] 3,7-Dibromo-10-(2-ethylhexyl)-10H-phenothiazine (235 mg, 0.5 mmol), 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin (300 mg, 0.5 mmol), 3,4-ethylenedioxythiophene (142 mg, 1 mmol), anhydrous potassium carbonate (172.5 mg, 1.25 mmol), pivalic acid (42.6 mg, 0.41 mmol) and Pd(O Ac)2 (71 mg, 0.31 mmol) were sequentially added into a 35 mL Schlenk tube, and under nitrogen protection, 10 mL of anhydrous dimethylacetamide was added, and the mixture was reacted at 130°C for 18 h, and then cooled to room temperature; the obtained reaction mixture was mixed with 500 mL of methanol and filtered, and the filter cake was washed with methanol, and then the filter cake was wrapped with filter paper, and extracted with 250 mL each of methanol, acetone, petroleum ether and chloroform in sequence using a Soxhlet extractor, and finally the part extracted with chloroform was rotary evaporated to remove the solvent to obtain FEP;

[0091] 10 mg of FEP and 1 mL of chloroform were ultrasonically mixed at a frequency of 50 kHz for 10 min, and then spin-coated on the conductive surface of an ITO glass with a specification of 25*40 mm at a rotation speed of 1000 r / min for 20 s to obtain a yellow-green switchable electrochromic film with a thickness of 716.9 nm.

[0092] 1. Electrochemical testing

[0093] The electrochemical test was performed using a Chenhua 660 electrochemical workstation with the following parameters set: CV mode, scan rates of 50mv / s, 100mv / s, 200mv / s, 300mv / s, 500mv / s, and the highest and lowest scan voltages of 1V and 0V, respectively. Figure 2 As shown, the initial oxidation potential of the electrochromic film is 0.17 V, and there is a pair of obvious redox peaks, which proves that the electrochemical behavior of FEP is good.

[0094] 2. Electrochromic performance test

[0095] The electrochromic performance test was carried out using a Chenhua 660 electrochemical workstation coupled with a UV-visible spectrophotometer. Figure 4 As shown in the figure: in the process of applying different voltages, the peak of its absorption curve in the visible light range changes, proving that FEP switches color from yellow-brown to light grass green under the stimulation of voltage. Figure 6 As shown: the optical contrast of FEP at 460nm wavelength is 26%, the coloring time is 0.83s, and the fading time is 2.19s. Figure 8As shown: after 1000 cycles under a step voltage of 0V and 1V, the optical contrast at 460nm can still maintain 83.7% of the original contrast.

[0096] 3. Color and brightness measurement

[0097] The color coordinates of FEP were measured by using Chenhua 660 electrochemical workstation and CM-3600D-spectrophotometer. Fig.10 and Fig.12 As shown: as the applied voltage of FEP gradually increases from 0V to 1V, the a* value and b* value of the film gradually change from high to low, and the color of the film gradually switches from yellowish brown to light grass green; the brightness only changes from 66 to 80, proving that FEP has an obvious tendency from yellow to green color during the color change process, and there is no obvious change in light and dark.

[0098] Example 2

[0099] 3,7-Dibromo-10-(2-ethylhexyl)-10H-phenothiazine (235 mg, 0.5 mmol), 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin (300 mg, 0.5 mmol), 3-methylthiophene (98 mg, 1 mmol), anhydrous potassium carbonate (172.5 mg, 1.25 mmol), pivalic acid (196 mg, 1.91 mmol) and Pd(OAc) were added. 2 (196 mg, 0.87 mmol) was sequentially added into a 35 mL Schlenk tube, and under nitrogen protection, 10 mL of anhydrous dimethylacetamide was added, and the mixture was reacted at 130 °C for 18 h, and then cooled to room temperature; the obtained reaction mixture was mixed with 500 mL of methanol and filtered, and the filter cake was washed with methanol, and then the filter cake was wrapped with filter paper, and extracted with 250 mL each of methanol, acetone, petroleum ether and chloroform using a Soxhlet extractor, and finally the part extracted with chloroform was rotary evaporated to remove the solvent to obtain FTP;

[0100] 10 mg of FTP and 1 mL of chloroform were ultrasonically mixed at a frequency of 50 kHz for 10 min, and then spin-coated on the conductive surface of an ITO glass with a specification of 25*40 mm at a speed of 1000 r / min for 20 s to obtain a yellow-green switchable electrochromic film with a thickness of 301.9 nm.

[0101] 1. Electrochemical testing

[0102] The electrochemical test was performed using a Chenhua 660 electrochemical workstation with the following parameters set: CV mode, scan rates of 50mv / s, 100mv / s, 200mv / s, 300mv / s, 500mv / s, and the highest and lowest scan voltages of 1V and 0V, respectively. Figure 3 As shown, the initial oxidation potential of the electrochromic film is 0.73 V, and there is a pair of obvious redox peaks, which proves that the electrochemical behavior of FTP is good.

[0103] 2. Electrochromic performance test

[0104] The electrochromic performance test was carried out using a Chenhua 660 electrochemical workstation coupled with a UV-visible spectrophotometer. Figure 5 As shown in the figure, during the process of applying different voltages, the peak of its absorption curve in the visible light range changes, proving that FTP switches color from light yellow to grass green under the stimulation of voltage. Figure 7 As shown: the optical contrast of FTP at 440nm wavelength is 18%, the coloring time is 0.83s, and the fading time is 2.95. Fig. 9 As shown: after 1000 cycles under a step voltage of 0V and 1V, the optical contrast at 460nm can still maintain 69% of the original contrast.

[0105] 3. Color and brightness measurement

[0106] The color coordinates of FTP were determined by using Chenhua 660 electrochemical workstation and CM-3600D-spectrophotometer. Fig.11 and Fig.13 As shown: as the applied voltage gradually increases from 0V to 1V, the a* and b* values ​​of the FTP film gradually change from high to low, and the color of the film gradually switches from light yellow to grass green; the brightness only changes from 68 to 72, proving that FTP has an obvious yellow to green color tendency during the color change process, and there is no obvious change in light and dark.

[0107] Example 3

[0108] 150 mg of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 100 mg of 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin, 100 mg of 3,4-ethylenedioxythiophene, 110 mg of anhydrous potassium carbonate, 300 mg of pivalic acid and 300 mg of Pd(OAc)2 were added sequentially to 35 mL of In a Schlenk tube, under nitrogen protection, 8 mL of anhydrous dimethylacetamide was added, and the mixture was reacted at 120°C for 16 h, and then cooled to room temperature; the obtained reaction mixture was mixed with 500 mL of methanol and filtered, and the filter cake was washed with methanol, and then the filter cake was wrapped with filter paper, and extracted with 200 mL each of methanol, acetone, petroleum ether and chloroform in sequence using a Soxhlet extractor, and finally the part extracted with chloroform was rotary evaporated to remove the solvent to obtain FEP;

[0109] 12 mg of FEP and 1 mL of chloroform were ultrasonically mixed at a frequency of 50 kHz for 10 min, and then spin-coated on the conductive surface of an ITO glass with a specification of 25*40 mm at a speed of 1000 r / min for 20 s to obtain a yellow-green switchable electrochromic film with a thickness of 428 nm.

[0110] Example 4

[0111] 250 mg of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 350 mg of 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin, 100 mg of 3,4-ethylenedioxythiophene, 200 mg of anhydrous potassium carbonate, 150 mg of pivalic acid and 150 mg of Pd(OAc)2 were added to 35 mL of In a Schlenk tube, 12 mL of anhydrous dimethylacetamide was added under nitrogen protection, and the mixture was reacted at 150°C for 20 h, followed by cooling to room temperature; the obtained reaction mixture was mixed with 500 mL of methanol and filtered, and the filter cake was washed with methanol, and then the filter cake was wrapped with filter paper, and extracted with 300 mL each of methanol, acetone, petroleum ether and chloroform in sequence using a Soxhlet extractor, and finally the part extracted with chloroform was rotary evaporated to remove the solvent to obtain FEP;

[0112] 50 mg of FEP and 10 mL of chloroform were ultrasonically mixed at a frequency of 50 kHz for 10 min, and then spin-coated on the conductive surface of an ITO glass with a specification of 25*40 mm at a rotation speed of 3000 r / min for 1 min to obtain an electrochromic film that can switch from yellow to green.

[0113] Example 5

[0114] 50 mg of the FEP obtained in Example 1 was mixed with 10 mL of chloroform solution to obtain a FEP solution; 50 mg of the FTP obtained in Example 2 was mixed with 10 mL of chloroform solution to obtain a FTP solution; 25 mg each of the FEP obtained in Example 1 and the FTP obtained in Example 2 were mixed with 10 mL of chloroform to obtain a FEP-FTP mixed solution.

[0115] Use as Fig.14 The hollow mask shown in the figure has the black square as the hollow part. The FEP solution, FTP solution and FEP-FTP mixed solution are sprayed on the conductive surface of the ITO glass for 1 min using a spray gun (the angle between the spray gun and the ITO glass is 80°, the flow rate of the spray gun is 5.2 L / min, and the diameter of the spray gun is 3 mm) to obtain an electrochromic film that can switch from yellow to green, and an electrochromic camouflage net device is assembled using this, as shown in FIG. Fig.15 Shown is an electrochromic camouflage net that can switch from yellow to green.

[0116] It can be seen from the above embodiments that the present invention provides an electrochromic film capable of switching between yellow and green and a preparation method thereof. Fig.16 These are photos of the electrochromic camouflage net assembled in Example 5 at different voltages. It can be seen from the figure that the electrochromic film capable of switching between yellow and green of the present invention has a low driving voltage, excellent cycle stability, and a high optical contrast before and after color change, and is an electrochromic material with excellent performance.

[0117] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an electrochromic film capable of switching between yellow and green. It is characterized in that The following steps are involved: 1) 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin, thiophene compound, anhydrous potassium carbonate, pivalic acid, Pd(OAc) 2 reacting in anhydrous dimethylacetamide to obtain a reaction mixture; 2) mixing the reaction mixture obtained in step 1) with methanol, and sequentially filtering, washing, extracting and evaporating to obtain a product; 3) mixing the product obtained in step 2) with chloroform and coating the mixture to obtain an electrochromic film capable of switching between yellow and green; The structural formulas of the 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine and 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin are shown in Formula I and Formula II respectively: In Formula I and Formula II, 2. The method for preparing a yellow-green switchable electrochromic film according to claim 1, It is characterized in that In step 1), the thiophene compound includes 3,4-ethylenedioxythiophene or 3-methylthiophene.

3. The method for preparing a yellow-green switchable electrochromic film according to claim 2, It is characterized in that In step 1), when the thiophene compound is 3,4-ethylenedioxythiophene, the mass ratio of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin and 3,4-ethylenedioxythiophene is 1.5-2.7:1-2.5:1; The mass ratio of anhydrous potassium carbonate to 3,4-ethylenedioxythiophene is 1.2 to 2:1; The mass ratio of pivalic acid to 3,4-ethylenedioxythiophene is 0.3-0.6:1; The Pd(OAc) 2 The mass ratio of ethylenedioxythiophene to 3,4-ethylenedioxythiophene is 0.3 to 0.6:1; The added volume of the anhydrous dimethylacetamide is 50 to 80 mL / g based on the mass of 3,4-ethylenedioxythiophene.

4. A method for preparing a yellow-green switchable electrochromic film according to claim 2 or 3, It is characterized in that In step 1), when the thiophene compound is 3-methylthiophene, the mass ratio of 3,7-dibromo-10-(2-ethylhexyl)-10H-phenothiazine, 6,8-dibromo-3,3-bis(((2-ethylhexyl)oxy)methyl)-3,4-dihydro-2H-thieno[3,4-B][1,4]dioxepin and 3-methylthiophene is 2-2.5:2.5-3.5:1; The mass ratio of anhydrous potassium carbonate to 3-methylthiophene is 1.5-2.5:1; The mass ratio of pivalic acid to 3-methylthiophene is 1.5 to 3:1; The Pd(OAc) 2 The mass ratio of 3-methylthiophene to 1.5 to 3:1; The added volume of the anhydrous dimethylacetamide is 80 to 120 mL / g based on the mass of 3-methylthiophene.

5. The method for preparing a yellow-green switchable electrochromic film according to claim 1, It is characterized in that In step 1), the reaction temperature is 120-150° C., and the reaction time is 16-20 hours.

6. The method for preparing a yellow-green switchable electrochromic film according to claim 1, It is characterized in that In step 2), the extraction is an organic solvent extraction method, the order of the organic solvents is methanol, acetone, petroleum ether and chloroform, and the amount of the organic solvent is 200-300 mL; The products include FEP or FTP.

7. A method for preparing a yellow-green switchable electrochromic film according to claim 1 or 6, It is characterized in that In step 3), the ratio of the product to chloroform is 8-12 mg:1 mL.

8. The method for preparing a yellow-green switchable electrochromic film according to claim 7, It is characterized in that In step 3), the coating includes spray coating or spin coating.

9. The electrochromic film capable of switching between yellow and green obtained by the preparation method according to any one of claims 1 to 8.

10. The yellow-green switchable electrochromic film according to claim 9, It is characterized in that The thickness of the electrochromic film is 50nm-5μm.