Foaming type wear-resistant impact-resistant protective coating and preparation method thereof

Through the cross-linking reaction of two-component polyurethane coatings and nano-silicon nitride and nitrile rubber additives, the problem of insufficient wear and impact resistance of automotive chassis coatings is solved, and better protection effect is achieved.

CN119019924AInactive Publication Date: 2024-11-26YANCHENG TIANYI SEALING MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411104557.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing automotive chassis protective coatings are prone to fall off in harsh environments, and lack wear and impact resistance, making them unable to effectively protect chassis parts.

Method used

Using the preparation method of two-component polyurethane coating, nano silicon nitride and nitrile rubber are added as wear-resistant and impact-resistant additives through the cross-linking reaction between the prepolymer component and the curing agent component, to improve the wear-resistant and impact-resistant of the coating. performance.

Benefits of technology

It significantly improves the wear and impact resistance of the coating, enhances the protection ability of the coated object, and ensures a good cushioning effect during external extrusion and collision.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019924A_ABST
    Figure CN119019924A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, in particular to a foamed wear-resistant impact-resistant protective coating and a preparation method thereof. The foaming type wear-resistant impact-resistant protective coating is a double-component polyurethane coating and comprises a prepolymer group and a curing agent component, and the prepolymer component is an isocyanate group-terminated polyurethane prepolymer generated by reaction of diisocyanate and polyether polyol; wherein the curing agent component comprises a diamine curing agent, a wear-resistant and impact-resistant auxiliary agent and a foaming agent, the diamine curing agent reacts with isocyanate groups in the polyurethane prepolymer through amino groups to generate ureido, and cross-linking curing among molecules of the polyurethane prepolymer is achieved; due to the addition of the foaming agent, the polyurethane coating can be foamed, so that the buffering effect of a coated object when the coated object is extruded and collided by the outside is improved; the wear-resistant and impact-resistant auxiliary agent can be connected to polyurethane molecules through stable chemical bonds and has good compatibility with polyurethane, and the wear resistance and impact resistance of the coating are high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a foaming type wear-resistant and impact-resistant protective coating and a preparation method thereof. Background Art

[0002] Due to its special location and structure, the chassis of a car is susceptible to external damage such as corrosion and impact from foreign objects when the car is used under harsh road conditions, which in turn damages the parts located in the chassis. Therefore, it is generally necessary to perform protective treatment on the chassis of the car, which includes using protective coatings to form a protective layer on the chassis to prevent erosion from the external environment.

[0003] Chinese patent application CN108300064A discloses an anti-rust coating for automobile chassis, which is made of acrylic emulsion, xanthan gum, defoamer, film-forming aid, barium sulfate, modified zinc phosphate, surfactant, isotridecyloxypropylamine, nano-alumina, talcum powder, tributyl phosphate, oxidized starch, sepiolite powder, and chlorinated paraffin. It has good anti-rust and anti-corrosion properties. However, when the chassis is scratched or collided by the outside world, the coating is easy to fall off, and the collision is easy to cause deformation of the chassis and damage to parts. The wear resistance and impact resistance of the coating need to be improved. Liu Sheng et al. published "Research on Physical Foaming Anti-Stone Impact Car Underbody Coating", which prepares the coating by adding foaming microspheres into thermoplastic polymer resin. The foaming microspheres are heat-expandable closed microcapsule particles. When the external environment rises to a certain temperature, the contents of the microcapsules in the coating film are vaporized by the heat, and the volume expands. The microcapsule shell is softened by the heat and expands accordingly. When the external environment temperature begins to drop, the contents stop vaporizing and expanding, and the volume of the microcapsules stops growing. When cooling, the thermoplastic shell hardens again, thereby maintaining the volume after heating. The coating has good impact resistance, but the wear resistance of the coating needs to be improved. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a foaming wear-resistant and impact-resistant protective coating and a preparation method thereof, so as to solve the problem that the wear resistance and impact resistance of protective coatings for automobile chassis in the prior art need to be improved.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a foaming wear-resistant and impact-resistant protective coating comprises the following steps:

[0007] Step 1, preparing a prepolymer component and a curing agent component;

[0008] The preparation of the prepolymer component comprises the following steps:

[0009] Add a catalyst dropwise to the polyether polyol, stir, heat to a set temperature, add diisocyanate, react, and obtain a prepolymer component;

[0010] The preparation of the curing agent component comprises the following steps:

[0011] (1) adding sodium dodecyl sulfate to deionized water, stirring until dissolved, adding nano silicon nitride, ultrasonically dispersing, and then dropping γ-methacryloxypropyl to react. After the reaction is completed, filtering, washing, and drying to obtain alkenyl-modified nano silicon nitride;

[0012] (2) adding olefin-modified nano silicon nitride, dibenzoyl peroxide and amino-terminated liquid nitrile rubber to ethyl acetate for reaction, cooling to room temperature after the reaction is completed, precipitating, filtering, washing and drying to obtain a wear-resistant and impact-resistant additive;

[0013] (3) mixing 3,3-dichloro-4,4-diaminodiphenylmethane, a wear-resistant and impact-resistant additive, a foaming agent, a foam stabilizer, and a solvent to obtain a curing agent component;

[0014] Step 2: Mix the prepolymer component and the curing agent component, stir, and obtain a foaming wear-resistant and impact-resistant protective coating.

[0015] Preferably, in the step 1, when preparing the prepolymer component: the molar ratio of polyether polyol to diisocyanate is 1:(1.5-2.0), the amount of catalyst used accounts for 0.6%-1% of the total mass of polyether polyol and diisocyanate, and the reaction conditions are stirring the reaction at a set temperature for 2.5-3.5 hours.

[0016] Preferably, in the step 1, when preparing the prepolymer component: the temperature is set at 75-85°C.

[0017] Preferably, in the step 1, when preparing the prepolymer component:

[0018] Polyether polyols include polyoxypropylene glycol;

[0019] The catalyst includes stannous isooctanoate;

[0020] The diisocyanate includes 4,4'-diphenylmethane diisocyanate.

[0021] Preferably, in step 1, when preparing the curing agent component: the mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl and deionized water is (2-6):140:(11-15):(550-750), and the reaction conditions are stirring the reaction at a temperature of 65-75°C for 6-8h.

[0022] Preferably, in the step 1, when preparing the curing agent component: the mass ratio of olefin-modified nano silicon nitride, dibenzoyl peroxide, amino-terminated liquid nitrile rubber, and ethyl acetate is (80-120):(6-10):350:(1000-1750), and the reaction conditions are in a nitrogen atmosphere at a temperature of 65-75°C for 6-10 hours.

[0023] Preferably, in step 1, when preparing the curing agent component: the mass ratio of 3,3'-dichloro-4,4'-diaminodiphenylmethane, wear-resistant and impact-resistant additive, foaming agent, foam stabilizer, and solvent is (20-30):(30-40):(25-35):(5-10):(80-120).

[0024] Preferably, the blowing agent comprises ethylene dichloride;

[0025] The foam stabilizer includes polysiloxane;

[0026] The solvent includes ethanol.

[0027] Preferably, in step 2, the mass ratio of the prepolymer component to the curing agent component is 100:(50-60).

[0028] Preferably, in step 2, the stirring speed is 1000 r / min and the stirring time is 20-30 s.

[0029] Preferably, the prepolymer component and the curing agent component of the foamable wear-resistant and impact-resistant protective coating are stored separately, and are mixed and stirred in proportion before use.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The foamable wear-resistant and impact-resistant protective coating prepared by the present invention is a two-component polyurethane coating, wherein the prepolymer component is an isocyanate-terminated polyurethane prepolymer generated by the reaction of diisocyanate and polyether polyol through isocyanate group (-NCO) and hydroxyl group (-OH) under the action of a catalyst; the curing agent component includes a diamine curing agent 3,3-dichloro-4,4-diaminodiphenylmethane, a wear-resistant and impact-resistant auxiliary agent, and a foaming agent. When the prepolymer component and the curing agent component are mixed, the amino group on the 3,3-dichloro-4,4-diaminodiphenylmethane molecule reacts with the isocyanate group in the polyurethane prepolymer to generate a urea group, thereby realizing cross-linking and curing between the polyurethane prepolymer molecules; the addition of the foaming agent can make the polyurethane coating foam, thereby improving the buffering effect of the coated object when it is squeezed and collided by the outside world, thereby realizing the protective effect on the coated object;

[0032] The addition of wear-resistant and impact-resistant additives can improve the wear resistance and impact resistance of the coating, and further improve the protection of the coating to the coated object; the wear-resistant and impact-resistant additives are made of nano silicon nitride and nitrile rubber, the addition of nano silicon nitride can effectively improve the wear resistance of the coating, and the addition of nitrile rubber can effectively improve the toughness of the coating, thereby improving the impact resistance of the coating; nano silicon nitride reacts with γ-methacryloxypropyl to obtain alkenyl-modified nano silicon nitride, and the carbon-carbon double bond (-C=C-) on the alkenyl-modified nano silicon nitride molecule reacts with the α-C on the amino-terminated liquid nitrile rubber molecular chain under the action of a peroxidation initiator. Through addition reaction, nano silicon nitride is grafted onto the amino-terminated liquid nitrile rubber molecules. As the nitrile rubber molecular chains and the polyurethane molecular chains are entangled with each other, the compatibility and dispersion uniformity of nano silicon nitride in the polyurethane coating are improved, and the wear resistance can be improved. The amino group at the end of the amino-terminated liquid nitrile rubber molecular chain can react with the isocyanate group in the polyurethane prepolymer to generate a urea group, so that the wear-resistant and impact-resistant additive participates in the curing and cross-linking of the polyurethane prepolymer, and the wear-resistant and impact-resistant additive is connected to the polyurethane molecule with a stable chemical bond, thereby improving the compatibility between the wear-resistant and impact-resistant additive and the polyurethane, and further improving the wear resistance and impact resistance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The present invention is a flow chart of the preparation process of the foaming wear-resistant and impact-resistant protective coating;

[0034] Figure 2 It is a line chart of the impact resistance test results of the foaming wear-resistant and impact-resistant protective coatings prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention;

[0035] Figure 3 The present invention is a line graph of the wear resistance test results of the foamed wear-resistant and impact-resistant protective coatings prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] This embodiment discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0039] Step 1, preparing a prepolymer component and a curing agent component;

[0040] The preparation of the prepolymer component comprises the following steps:

[0041] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 75°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:1.5, the amount of stannous isooctanoate as a catalyst accounts for 0.6% of the total mass of polyether polyol and diisocyanate, react for 3.5 hours at a stirring speed of 250 r / min and a temperature of 75°C to obtain a prepolymer component;

[0042] The preparation of the curing agent component comprises the following steps:

[0043] (1) adding sodium dodecyl sulfate to deionized water, stirring at a stirring speed of 500 r / min until dissolved, adding nano silicon nitride, ultrasonically dispersing at a frequency of 50 kHz for 30 min, and then dropping γ-methacryloxypropyl at a stirring speed of 250 r / min, wherein the mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl and deionized water is 2:140:11:550, reacting at a stirring speed of 250 r / min and a temperature of 65° C. for 8 h. After the reaction is completed, filtering, washing with deionized water for 3 times, and drying in a vacuum drying oven at 60° C. for 10 h, to obtain olefin-modified nano silicon nitride;

[0044] (2) adding olefin-modified nano silicon nitride, dibenzoyl peroxide and amino-terminated liquid nitrile rubber to ethyl acetate, wherein the mass ratio of olefin-modified nano silicon nitride, dibenzoyl peroxide, amino-terminated liquid nitrile rubber and ethyl acetate is 80:6:350:1000, reacting for 10 hours at 65° C. in a nitrogen atmosphere, cooling to room temperature after the reaction, adding methanol twice the mass of ethyl acetate for precipitation, filtering, washing with ethanol three times, and drying in a vacuum drying oven at 60° C. for 10 hours to obtain a wear-resistant and impact-resistant additive;

[0045] (3) 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, a foaming agent, fluorodichloroethane, a foam stabilizer, and ethanol were stirred at a stirring speed of 250 r / min for 1 h, wherein the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, fluorodichloroethane, polysiloxane, and ethanol was 20:30:25:5:80, to obtain a curing agent component;

[0046] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:50 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0047] Example 2

[0048] This embodiment discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0049] Step 1, preparing a prepolymer component and a curing agent component;

[0050] The preparation of the prepolymer component comprises the following steps:

[0051] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 85°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:2, the amount of stannous isooctanoate as a catalyst accounts for 0.7% of the total mass of polyether polyol and diisocyanate, react at a stirring speed of 250 r / min and a temperature of 85°C for 2.5 hours to obtain a prepolymer component;

[0052] The preparation of the curing agent component comprises the following steps:

[0053] (1) adding sodium dodecyl sulfate to deionized water, stirring at a stirring speed of 500 r / min until dissolved, adding nano silicon nitride, ultrasonically dispersing at a frequency of 50 kHz for 30 min, and then dropping γ-methacryloxypropyl at a stirring speed of 250 r / min, wherein the mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl and deionized water is 6:140:15:750, reacting at a stirring speed of 250 r / min and a temperature of 75° C. for 6 h. After the reaction is completed, filtering, washing with deionized water for 3 times, and drying in a vacuum drying oven at 60° C. for 10 h, to obtain olefin-modified nano silicon nitride;

[0054] (2) adding olefin-modified nano silicon nitride, dibenzoyl peroxide and amino-terminated liquid nitrile rubber to ethyl acetate, wherein the mass ratio of olefin-modified nano silicon nitride, dibenzoyl peroxide, amino-terminated liquid nitrile rubber and ethyl acetate is 120:10:350:1750, reacting for 6 hours at 75°C in a nitrogen atmosphere, cooling to room temperature after the reaction, adding methanol twice the mass of ethyl acetate for precipitation, filtering, washing with ethanol three times, and drying in a vacuum drying oven at 60°C for 10 hours to obtain a wear-resistant and impact-resistant additive;

[0055] (3) 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additive, a foaming agent, fluorodichloroethane, a foam stabilizer, and ethanol were stirred at a stirring speed of 250 r / min for 1 h, wherein the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additive, fluorodichloroethane, polysiloxane, and ethanol was 30:40:35:10:120, to obtain a curing agent component;

[0056] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:60 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0057] Example 3

[0058] This embodiment discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0059] Step 1, preparing a prepolymer component and a curing agent component;

[0060] The preparation of the prepolymer component comprises the following steps:

[0061] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 80°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:1.6, the amount of stannous isooctanoate as a catalyst accounts for 0.7% of the total mass of polyether polyol and diisocyanate, react for 3 hours at a stirring speed of 250 r / min and a temperature of 80°C to obtain a prepolymer component;

[0062] The preparation of the curing agent component comprises the following steps:

[0063] (1) adding sodium dodecyl sulfate to deionized water, stirring at a stirring speed of 500 r / min until dissolved, adding nano silicon nitride, ultrasonically dispersing at a frequency of 50 kHz for 30 min, and then dropping γ-methacryloxypropyl at a stirring speed of 250 r / min, the mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl, and deionized water is 3:140:12:600, and reacting at a stirring speed of 250 r / min and a temperature of 70° C. for 7 h. After the reaction is completed, filtering, washing with deionized water 3 times, and drying in a vacuum drying oven at 60° C. for 10 h to obtain olefin-modified nano silicon nitride;

[0064] (2) adding olefin-modified nano silicon nitride, dibenzoyl peroxide and amino-terminated liquid nitrile rubber to ethyl acetate, wherein the mass ratio of olefin-modified nano silicon nitride, dibenzoyl peroxide, amino-terminated liquid nitrile rubber and ethyl acetate is 90:7:350:1200, reacting for 8 hours at 70° C. in a nitrogen atmosphere, cooling to room temperature after the reaction, adding methanol twice the mass of ethyl acetate for precipitation, filtering, washing with ethanol for 3 times, and drying in a vacuum drying oven at 60° C. for 10 hours to obtain a wear-resistant and impact-resistant additive;

[0065] (3) 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, a foaming agent, fluorodichloroethane, a foam stabilizer, and ethanol were stirred at a stirring speed of 250 r / min for 1 h, and the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, fluorodichloroethane, polysiloxane, and ethanol was 23:42:28:6.5:90 to obtain a curing agent component;

[0066] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:52.5 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0067] Example 4

[0068] This embodiment discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0069] Step 1, preparing a prepolymer component and a curing agent component;

[0070] The preparation of the prepolymer component comprises the following steps:

[0071] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 80°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:1.75, the amount of stannous isooctanoate as a catalyst accounts for 0.8% of the total mass of polyether polyol and diisocyanate, react for 3 hours at a stirring speed of 250 r / min and a temperature of 80°C to obtain a prepolymer component;

[0072] The preparation of the curing agent component comprises the following steps:

[0073] (1) adding sodium dodecyl sulfate to deionized water, stirring at a stirring speed of 500 r / min until dissolved, adding nano silicon nitride, ultrasonically dispersing at a frequency of 50 kHz for 30 min, and then dropping γ-methacryloxypropyl at a stirring speed of 250 r / min, wherein the mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl and deionized water is 4:140:13:650, reacting at a stirring speed of 250 r / min and a temperature of 70° C. for 7 h. After the reaction is completed, filtering, washing with deionized water for 3 times, and drying in a vacuum drying oven at 60° C. for 10 h, to obtain olefin-modified nano silicon nitride;

[0074] (2) adding olefin-modified nano silicon nitride, dibenzoyl peroxide and amino-terminated liquid nitrile rubber to ethyl acetate, wherein the mass ratio of olefin-modified nano silicon nitride, dibenzoyl peroxide, amino-terminated liquid nitrile rubber and ethyl acetate is 100:8:350:1350, reacting for 8 hours at 70°C in a nitrogen atmosphere, cooling to room temperature after the reaction, adding methanol twice the mass of ethyl acetate for precipitation, filtering, washing with ethanol for 3 times, and drying in a vacuum drying oven at 60°C for 10 hours to obtain a wear-resistant and impact-resistant additive;

[0075] (3) 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, a foaming agent, fluorodichloroethane, a foam stabilizer, and ethanol were stirred at a stirring speed of 250 r / min for 1 h, and the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, fluorodichloroethane, polysiloxane, and ethanol was 25:45:30:7.5:100 to obtain a curing agent component;

[0076] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:55 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0077] Example 5

[0078] This embodiment discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0079] Step 1, preparing a prepolymer component and a curing agent component;

[0080] The preparation of the prepolymer component comprises the following steps:

[0081] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 80°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:1.9, the amount of stannous isooctanoate as a catalyst accounts for 0.9% of the total mass of polyether polyol and diisocyanate, react for 3 hours at a stirring speed of 250 r / min and a temperature of 80°C to obtain a prepolymer component;

[0082] The preparation of the curing agent component comprises the following steps:

[0083] (1) adding sodium dodecyl sulfate to deionized water, stirring at a stirring speed of 500 r / min until dissolved, adding nano silicon nitride, ultrasonically dispersing at a frequency of 50 kHz for 30 min, and then dropping γ-methacryloxypropyl at a stirring speed of 250 r / min. The mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl and deionized water is 5:140:14:700. The mixture is reacted at a stirring speed of 250 r / min and a temperature of 70° C. for 7 h. After the reaction is completed, filtering, washing with deionized water for 3 times, and drying in a vacuum drying oven at 60° C. for 10 h to obtain olefin-modified nano silicon nitride;

[0084] (2) adding olefin-modified nano silicon nitride, dibenzoyl peroxide and amino-terminated liquid nitrile rubber to ethyl acetate, wherein the mass ratio of olefin-modified nano silicon nitride, dibenzoyl peroxide, amino-terminated liquid nitrile rubber and ethyl acetate is 110:9:350:1500, reacting for 8 hours at 70°C in a nitrogen atmosphere, cooling to room temperature after the reaction, adding methanol twice the mass of ethyl acetate for precipitation, filtering, washing with ethanol for 3 times, and drying in a vacuum drying oven at 60°C for 10 hours to obtain a wear-resistant and impact-resistant additive;

[0085] (3) 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, a foaming agent, fluorodichloroethane, a foam stabilizer, and ethanol were stirred at a stirring speed of 250 r / min for 1 h, wherein the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, abrasion-resistant and impact-resistant additives, fluorodichloroethane, polysiloxane, and ethanol was 28:47:33:9:110, to obtain a curing agent component;

[0086] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:58 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0087] Comparative Example 1

[0088] This comparative example discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0089] Step 1, preparing a prepolymer component and a curing agent component;

[0090] The preparation of the prepolymer component comprises the following steps:

[0091] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 75°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:1.5, the amount of stannous isooctanoate as a catalyst accounts for 0.6% of the total mass of polyether polyol and diisocyanate, react for 3.5 hours at a stirring speed of 250 r / min and a temperature of 75°C to obtain a prepolymer component;

[0092] The preparation of the curing agent component comprises the following steps:

[0093] (1) adding sodium dodecyl sulfate to deionized water, stirring at a stirring speed of 500 r / min until dissolved, adding nano silicon nitride, ultrasonically dispersing at a frequency of 50 kHz for 30 min, and then dropping γ-methacryloxypropyl at a stirring speed of 250 r / min, wherein the mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl and deionized water is 2:140:11:550, reacting at a stirring speed of 250 r / min and a temperature of 65° C. for 8 h. After the reaction is completed, filtering, washing with deionized water for 3 times, and drying in a vacuum drying oven at 60° C. for 10 h, to obtain olefin-modified nano silicon nitride;

[0094] (2) 3,3-dichloro-4,4-diaminodiphenylmethane, amino-terminated liquid nitrile rubber, olefin-modified nano silicon nitride, foaming agent fluorodichloroethane, foam stabilizer polysiloxane, and ethanol were stirred at a stirring speed of 250 r / min for 1 h, and the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, amino-terminated liquid nitrile rubber, olefin-modified nano silicon nitride, fluorodichloroethane, polysiloxane, and ethanol was 20:24.4:5.6:25:5:80 to obtain a curing agent component;

[0095] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:50 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0096] Comparative Example 2

[0097] This comparative example discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0098] Step 1, preparing a prepolymer component and a curing agent component;

[0099] The preparation of the prepolymer component comprises the following steps:

[0100] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 75°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:1.5, the amount of stannous isooctanoate as a catalyst accounts for 0.6% of the total mass of polyether polyol and diisocyanate, react for 3.5 hours at a stirring speed of 250 r / min and a temperature of 75°C to obtain a prepolymer component;

[0101] The preparation of the curing agent component comprises the following steps:

[0102] 3,3-dichloro-4,4-diaminodiphenylmethane, amino-terminated liquid nitrile rubber, nano silicon nitride, monofluorodichloroethane, a foaming agent, polysiloxane, and ethanol were stirred at a stirring speed of 250 r / min for 1 hour, and the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, amino-terminated liquid nitrile rubber, nano silicon nitride, monofluorodichloroethane, polysiloxane, and ethanol was 20:24.4:5.2:25:5:80.4 to obtain a curing agent component;

[0103] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:50 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0104] Comparative Example 3

[0105] This comparative example discloses a method for preparing a foaming wear-resistant and impact-resistant protective coating, comprising the following steps:

[0106] Step 1, preparing a prepolymer component and a curing agent component;

[0107] The preparation of the prepolymer component comprises the following steps:

[0108] Add stannous isooctanoate as a catalyst to polyoxypropylene glycol, stir for 30 minutes at a stirring speed of 250 r / min, heat to 75°C, add 4,4'-diphenylmethane diisocyanate, the molar ratio of polyoxypropylene glycol to 4,4'-diphenylmethane diisocyanate is 1:1.5, the amount of stannous isooctanoate as a catalyst accounts for 0.6% of the total mass of polyether polyol and diisocyanate, react for 3.5 hours at a stirring speed of 250 r / min and a temperature of 75°C to obtain a prepolymer component;

[0109] The preparation of the curing agent component comprises the following steps:

[0110] 3,3-dichloro-4,4-diaminodiphenylmethane, liquid nitrile rubber, nano silicon nitride, monofluorodichloroethane, foaming agent, polysiloxane, and ethanol were stirred at a stirring speed of 250 r / min for 1 hour, and the mass ratio of 3,3-dichloro-4,4-diaminodiphenylmethane, liquid nitrile rubber, nano silicon nitride, monofluorodichloroethane, polysiloxane, and ethanol was 20:24.4:5.2:25:5:80.4, to obtain a curing agent component;

[0111] Step 2: Mix the prepolymer component and the curing agent component in a mass ratio of 100:50 to obtain a foaming wear-resistant and impact-resistant protective coating.

[0112] In the above embodiments and comparative examples, polyoxypropylene glycol was purchased from Shanghai McLean Biochemical Technology Co., Ltd., with a number average molecular weight of 600; stannous isooctanoate was purchased from Yantai Sunshine Plastic Co., Ltd., with appearance properties: liquid, model: T9; nano silicon nitride was purchased from Shanghai Yaotian New Material Technology Co., Ltd., with article number: YT-BY-4-1, and particle size: 20 nm; amino-terminated liquid nitrile rubber was purchased from Shanghai Citailong Industrial Co., Ltd., with a number average molecular weight of 3500; polysiloxane was purchased from Shandong Dayi Chemical Co., Ltd., with article number: DY-ET101B; liquid nitrile rubber was purchased from Shanghai Duokang Industrial Co., Ltd., with model: LNBR40, acrylonitrile content: 30-34%, and molecular weight: 1000-2000.

[0113] Test example

[0114] The coatings prepared in Examples 1-5 and Comparative Examples 1-3 were tested for performance:

[0115] (1) Impact resistance test: The prepolymer component and the curing agent component of the coating were mixed according to the mass ratio, sprayed on the mold, and cured at 80°C for 48 hours to obtain a sample with a size of 100 mm×30 mm×15 mm. The impact toughness of the sample was measured using an XJ-300A impact testing machine. The test results are shown in Table 1:

[0116] Table 1

[0117]

[0118] As shown in Table 1, after the coating obtained by the present invention is foamed and molded, it has excellent impact resistance and can play a good protective role. Wear-resistant and impact-resistant additives are made from nano silicon nitride and nitrile rubber, wherein the addition of nitrile rubber can effectively improve the toughness of the coating, thereby improving the impact resistance of the coating; the amino group at the end of the amino-terminated liquid nitrile rubber molecular chain reacts with the isocyanate group in the polyurethane prepolymer to generate a urea group, so that the nitrile rubber participates in the curing and crosslinking of the polyurethane prepolymer, and the nitrile rubber is connected to the polyurethane molecule with a stable chemical bond, and the compatibility between the nitrile rubber and the polyurethane is improved, thereby improving the impact resistance of the coating. Compared with Example 1, in Comparative Examples 1 and 2, the nitrile rubber is an amino-terminated liquid nitrile rubber, which can be connected to the polyurethane molecule, and the compatibility between the nitrile rubber and the polyurethane is improved, and the impact resistance is not significantly changed compared to Example 1; in Comparative Example 3, the nitrile rubber is not connected to the polyurethane molecule, and the compatibility between the nitrile rubber and the polyurethane is reduced, and the impact resistance is significantly reduced compared to Example 1.

[0119] (2) Wear resistance test: The test method refers to the standard GB / T9867-2008 "Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrasion machine method)". The prepolymer component and the curing agent component of the coating are mixed according to the mass ratio, sprayed on the mold, cured at 80°C for 48 hours, cut to obtain a sample with a diameter of 16 mm and a height of 10 mm, and the average relative volume wear of the sample is measured. The test results are shown in Table 2:

[0120] Table 2

[0121]

[0122] As shown in Table 2, the coating prepared by the present invention has excellent wear resistance after foaming and can play a good protective role. The wear-resistant and impact-resistant additive is prepared from nano silicon nitride and nitrile rubber, wherein the addition of nano silicon nitride can effectively improve the wear resistance of the coating; the olefin-modified nano silicon nitride obtained by the reaction of nano silicon nitride and γ-methacryloxypropyl is grafted onto the terminal amino liquid nitrile rubber molecule through an addition reaction, and the amino group at the end of the terminal amino liquid nitrile rubber molecular chain reacts with the isocyanate group in the polyurethane prepolymer to generate a urea group, and the nano silicon nitride is connected to the polyurethane molecule with a stable chemical bond, thereby improving the compatibility and dispersion uniformity of the nano silicon nitride in the polyurethane coating, and then improving the wear resistance of the coating. Compared with Example 1, in Comparative Example 1, although the nano silicon nitride is olefin-modified, it is not connected to the polyurethane molecule, and its compatibility and dispersion uniformity in the polyurethane coating are reduced, and the wear resistance is reduced; in Comparative Examples 2 and 3, the nano silicon nitride is not olefin-modified, and its compatibility and dispersion uniformity in the polyurethane coating are worse, and the wear resistance is further reduced.

[0123] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a foaming wear-resistant and impact-resistant protective coating, characterized in that: The following steps are involved: Step 1, preparing a prepolymer component and a curing agent component; The preparation of the prepolymer component comprises the following steps: Add a catalyst dropwise to the polyether polyol, stir, heat to a set temperature, add diisocyanate, react, and obtain a prepolymer component; Wherein, the preparation of the curing agent component comprises the following steps: (1) adding sodium dodecyl sulfate to deionized water, stirring until dissolved, adding nano silicon nitride, ultrasonically dispersing, and then dropping γ-methacryloxypropyl to react. After the reaction is completed, filtering, washing, and drying to obtain alkenyl-modified nano silicon nitride; (2) adding olefin-modified nano silicon nitride, dibenzoyl peroxide and amino-terminated liquid nitrile rubber to ethyl acetate for reaction, cooling to room temperature after the reaction is completed, precipitating, filtering, washing and drying to obtain a wear-resistant and impact-resistant additive; (3) mixing 3,3-dichloro-4,4-diaminodiphenylmethane, a wear-resistant and impact-resistant additive, a foaming agent, a foam stabilizer, and a solvent to obtain a curing agent component; Step 2: Mix the prepolymer component and the curing agent component, stir, and obtain a foaming wear-resistant and impact-resistant protective coating.

2. The method for preparing a foamable wear-resistant and impact-resistant protective coating according to claim 1, characterized in that: In the step 1, when preparing the prepolymer component: the molar ratio of polyether polyol to diisocyanate is 1:(1.5-2.0), the amount of catalyst used accounts for 0.6%-1% of the total mass of polyether polyol and diisocyanate, and the reaction conditions are stirring the reaction at a set temperature for 2.5-3.5 hours.

3. The method for preparing a foamable wear-resistant and impact-resistant protective coating according to claim 2, characterized in that: The set temperature is 75-85°C.

4. The method for preparing a foamable wear-resistant and impact-resistant protective coating according to claim 1, characterized in that: In the step 1, when preparing the prepolymer component: Polyether polyols include polyoxypropylene glycol; The catalyst includes stannous isooctanoate; The diisocyanate includes 4,4'-diphenylmethane diisocyanate.

5. The method for preparing a foaming wear-resistant and impact-resistant protective coating according to claim 1, characterized in that: In the step 1, when preparing the curing agent component: the mass ratio of sodium dodecyl sulfate, nano silicon nitride, γ-methacryloxypropyl, and deionized water is (2-6):140:(11-15):(550-750), and the reaction conditions are 65-75° C. for 6-8 hours.

6. The method for preparing a foamable wear-resistant and impact-resistant protective coating according to claim 1, characterized in that: In the step 1, when preparing the curing agent component: the mass ratio of olefin-modified nano silicon nitride, dibenzoyl peroxide, amino-terminated liquid nitrile rubber, and ethyl acetate is (80-120):(6-10):350:(3000-5000), and the reaction conditions are in a nitrogen atmosphere at a temperature of 65-75° C. for 6-10 hours.

7. The method for preparing a foamable wear-resistant and impact-resistant protective coating according to claim 1, characterized in that: In the step 1, when preparing the curing agent component: the mass ratio of 3,3'-dichloro-4,4'-diaminodiphenylmethane, wear-resistant and impact-resistant additive, foaming agent, foam stabilizer, and solvent is (20-30):(30-40):(25-35):(5-10):(80-120).

8. The method for preparing a foamable wear-resistant and impact-resistant protective coating according to claim 7, characterized in that: The blowing agent includes monofluorodichloroethane; The foam stabilizer includes polysiloxane; The solvent includes ethanol.

9. The method for preparing a foamable wear-resistant and impact-resistant protective coating according to claim 1, characterized in that: In the step 2, the mass ratio of the prepolymer component to the curing agent component is 100:(50-60).

10. A foaming wear-resistant and impact-resistant protective coating prepared by the method for preparing a foaming wear-resistant and impact-resistant protective coating as described in any one of claims 1 to 9.