Accurate control method for content of nitrogen element in high-strength steel
By controlling the linear relationship between nitrogen filling pressure and melt pool temperature, the problem of difficult to accurately control the nitrogen content in high-temperature alloys is solved, the smelting efficiency is improved and the risk of inclusions is reduced, and the efficient production of high-strength steel is achieved.
Patent Information
- Application Number
- CN202410732566.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-11-26
AI Technical Summary
During the smelting of high-temperature alloys, the nitrogen content is difficult to accurately control. Traditional methods require frequent adjustment of the melt pool temperature and nitrogen filling pressure, resulting in low smelting efficiency and increasing the risk of inclusions.
By controlling the minimum nitrogen filling pressure and the maximum melt pool temperature, using the linear relationship p=0.02546*T-30.81527, the precise control of nitrogen content is achieved, including the nitrogen filling pressure and temperature adjustment during the alloying and casting periods, ensuring that the nitrogen element is in Within the range of 0.02~0.08wt.%.
It improves the smelting efficiency, reduces the content of foreign inclusions, achieves rapid and effective control of nitrogen content, and ensures the finished product quality of high-strength steel.
Smart Images

Figure CN119020550A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature alloy smelting, and in particular to a method for accurately controlling the nitrogen content in high-strength steel. Background Art
[0002] 1Cr12Ni2WMoVNbN is a martensitic heat-resistant stainless steel with high thermal strength and good marine corrosion resistance. It is suitable for compressor disks, blades and other materials working below 650℃. Due to the addition of Nb and N, and the high content of Mo and Ni, it has good hardenability and high strength, mainly relying on phase transformation strengthening. The addition of austenitizing stabilizing elements Ni, Mn, and Co can reduce the austenite zone, reduce the δ-ferrite content, and improve the material quality of large forgings. As a strong austenite-forming element (the ability of nitrogen to form austenite is about 30 times that of nickel), replacing nickel with nitrogen to obtain stable austenite not only greatly reduces costs, but also significantly improves the strength and corrosion resistance of stainless steel due to the significant solid solution strengthening effect of nitrogen and its effect on pitting corrosion.
[0003] The main difficulties of this alloy are: (1) the N content is difficult to control accurately, and escape will occur during the smelting process, and nitrogen protection is required; (2) the steel ingot is prone to cracking when cooled from high temperature, and slow cooling and timely stress relief annealing are required. During the smelting process, the temperature of the molten steel and the vapor pressure of the molten pool liquid surface have a decisive effect on the solubility of nitrogen in the molten pool. When the vapor pressure increases, the temperature of the corresponding molten steel will decrease, and then the temperature needs to be adjusted to ensure that the alloy has good fluidity. When the molten pool temperature increases, the solubility of nitrogen in the corresponding molten steel decreases, and nitrogen filling protection is required to increase the solubility of nitrogen. Therefore, the traditional method of controlling the nitrogen content in the vacuum induction melting process has the problem of repeatedly adjusting the molten pool temperature and nitrogen filling pressure, which reduces the melting efficiency, and the long-term melting increases the risk of refractory materials bringing inclusions to the molten steel. This paper proposes a method for controlling the nitrogen content in high-strength steel, which can quickly and effectively control the molten pool temperature and nitrogen filling pressure, improve the melting efficiency, and reduce the content of foreign inclusions. Summary of the invention
[0004] The object of the present invention is to provide a method for accurately controlling the nitrogen content in high-strength steel to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for accurately controlling the nitrogen content in high-strength steel, which controls the nitrogen content by controlling the minimum nitrogen filling pressure and the maximum molten pool temperature, comprising the following steps:
[0006] Step 1: Nitrogen filling during alloying period:
[0007] 1Cr12Ni2WMoVNbN high-strength steel requires nitrogen element control range: N (0.02 ~ 0.08), the target value is 0.06wt.%. Chromium nitride is added during vacuum induction melting alloying, and nitrogen is charged before adding chromium nitride;
[0008] Step 2: Adjust the temperature during alloying according to the nitrogen filling pressure:
[0009] After nitrogen filling, adjust the temperature according to the nitrogen filling pressure, and then take samples to test the nitrogen content. Because chromium nitride will burn, the nitrogen content can be accurately controlled by subsequent addition;
[0010] Step 3: Adjust pouring temperature and nitrogen filling pressure during pouring:
[0011] At the end of vacuum induction melting, in order to ensure the fluidity of molten steel during the pouring process, a high superheat is generally selected as the pouring temperature. At this time, the nitrogen filling pressure needs to be adjusted accordingly to maintain the nitrogen content.
[0012] Preferably, the correlation between the molten pool temperature (T, K) and the nitrogen filling pressure (p, KPa) is a linear relationship, and the linear equation is: p=0.02546*T-30.81527.
[0013] Preferably, the composition range of the 1Cr12Ni2WMoVNbN satisfies (wt.%): C (0.13-0.18), Cr (11.00-12.50), Ni (1.70-2.10), W (0.65-1.00), Mo (1.35-1.65), V (0.18-0.30), N (0.02-0.08), Nb (0.20-0.30), Mn≤0.50, Si≤0.50, S≤0.015, P≤0.030, Al≤0.02
[0014] Preferably, nitrogen is charged to 15-20 KPa before adding chromium nitride in step 1.
[0015] Preferably, in step 2, the temperature is adjusted to 1530-1650° C. according to the nitrogen filling pressure.
[0016] Preferably, in step 2 and step 3, a suitable nitrogen filling pressure is matched according to the molten pool temperature to achieve dynamic control of the nitrogen element.
[0017] Compared with the prior art, the beneficial effect of the present invention is that the nitrogen content can be controlled by controlling the minimum nitrogen filling pressure and the maximum molten pool temperature, and the correlation between the molten pool temperature (T, K) and the nitrogen filling pressure (p, KPa) is determined to be a linear relationship, and the linear equation is: p = 0.02546*T-30.81527. Finally, during the vacuum induction melting alloying period and the pouring period, the appropriate nitrogen filling pressure can be matched according to the molten pool temperature to achieve dynamic control of the nitrogen element. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is the correlation between the molten pool temperature (T, K) and the nitrogen filling pressure (p, KPa). DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] See also Figure 1 The present invention provides a technical solution: a method for accurately controlling the nitrogen content in high-strength steel, which can ultimately control the nitrogen content in the high-strength steel within the standard requirement range by matching the pressure of the protective atmosphere nitrogen and the melting temperature during the melting process.
[0021] Step 1, nitrogen filling during alloying:
[0022] 1Cr12Ni2WMoVNbN high-strength steel requires nitrogen element control range: N (0.02 ~ 0.08), the target value is set to 0.06wt.%. Add appropriate amount of chromium nitride during vacuum induction melting alloying period, and fill nitrogen to 15 ~ 20KPa before adding chromium nitride;
[0023] Step 2: Adjust the temperature during alloying according to the nitrogen filling pressure:
[0024] After nitrogen filling, adjust the temperature to 1530-1650℃ according to the nitrogen filling pressure, and then take samples to test the nitrogen content. Because chromium nitride will burn, the nitrogen content can be accurately controlled by subsequent addition;
[0025] Step 3: Reasonably adjust the pouring temperature and nitrogen filling pressure during the pouring period:
[0026] At the end of vacuum induction melting, in order to ensure the fluidity of the molten steel during the pouring process, a higher superheat is selected as the pouring temperature. At this time, the nitrogen filling pressure needs to be reasonably adjusted to maintain the nitrogen content in the molten steel.
[0027] It should be noted that the technical solution adopted by the present invention is to determine the correlation between the molten pool temperature and the nitrogen filling pressure on the surface of the molten steel, find the maximum melting temperature required under a constant nitrogen filling pressure, or the minimum nitrogen filling pressure under a constant melting temperature, and finally achieve efficient controllable N content in the steel under the matching of the two parameters.
[0028] Furthermore, the high-strength steel is 1Cr12Ni2WMoVNbN, and its composition range satisfies (wt.%): C (0.13-0.18), Cr (11.00-12.50), Ni (1.70-2.10), W (0.65-1.00), Mo (1.35-1.65), V (0.18-0.30), N (0.02-0.08), Nb (0.20-0.30), Mn≤0.50, Si≤0.50, S≤0.015, P≤0.030, Al≤0.02, and the target value of N content in the steel is controlled at 0.06wt.% according to the standard requirements. The melting point of the high-strength steel is 1488°C, and the full melting temperature is 1520-1570°C. According to the smelting experience of high-strength steel, the temperature of the molten pool during the refining and pouring periods after full melting should be controlled at 1560-1650℃.
[0029] Furthermore, the determined correlation between the molten pool temperature (T, K) and the nitrogen filling pressure (p, KPa) is a linear relationship, and the linear equation is: p=0.02546*T-30.81527.
[0030] It should be noted that the control of the gaseous element N content in the steel of the present invention is mainly related to the molten pool temperature and the surface vapor pressure. According to the gas dissolution theory, the higher the vapor pressure of the gaseous element N, the higher the soluble N content in the molten pool, while the higher the molten pool temperature, the lower its solubility. Therefore, the two parameters of the molten pool temperature and the nitrogen filling pressure play a decisive role in the control of the gaseous element N content, and influence each other during the smelting process.
[0031] Furthermore, in the above linear relationship, if the nitrogen filling pressure is determined, the calculated temperature is the highest temperature of the molten pool. If the molten pool temperature is determined, the calculated temperature is the minimum nitrogen filling pressure.
[0032] Embodiment 1:
[0033] Step 1, adding an appropriate amount of chromium nitride during the vacuum induction melting alloying period, and nitrogen filling to 15KPa before adding chromium nitride;
[0034] Step 2: During the alloying period, the temperature of the molten pool is adjusted to not exceed 1530°C, at which time the maximum solubility of nitrogen in the molten pool is 0.06wt.%;
[0035] Step 3: During the pouring period, if the pouring temperature is set to 1600-1610°C, the nitrogen filling pressure must be increased to at least 17KPa to maintain the nitrogen content in the molten pool.
[0036] Embodiment 2:
[0037] Step 1, adding an appropriate amount of chromium nitride during the vacuum induction melting alloying period, and filling nitrogen to 16KPa before adding chromium nitride;
[0038] Step 2: During the alloying period, the temperature of the molten pool is adjusted to not exceed 1560°C, at which time the maximum solubility of nitrogen in the molten pool is 0.06wt.%;
[0039] Step 3: During the pouring period, if the pouring temperature is set to 1600-1610°C, the nitrogen filling pressure must be increased to at least 17KPa to maintain the nitrogen content in the molten pool.
[0040] Embodiment 3:
[0041] Step 1, adding an appropriate amount of chromium nitride during the vacuum induction melting alloying period, and nitrogen filling to 17KPa before adding chromium nitride;
[0042] Step 2: During the alloying period, the temperature of the molten pool is adjusted to not exceed 1600°C, at which time the maximum solubility of nitrogen in the molten pool is 0.06wt.%;
[0043] Step 3: During the pouring period, if the pouring temperature is set to 1640-1650°C, the nitrogen filling pressure must be increased to at least 18KPa to maintain the nitrogen content in the molten pool.
[0044] Embodiment 4:
[0045] Step 1, adding an appropriate amount of chromium nitride during the vacuum induction melting alloying period, and filling nitrogen to 18KPa before adding chromium nitride;
[0046] Step 2: During the alloying period, the temperature of the molten pool is adjusted to not exceed 1650°C, at which time the maximum solubility of nitrogen in the molten pool is 0.06wt.%;
[0047] Step 3: During the pouring period, if the pouring temperature reaches 1610-1620°C, the nitrogen filling pressure can be adjusted to ≥17KPa to maintain the nitrogen content in the molten pool.
[0048] In the above embodiment, the nitrogen content can be accurately and efficiently controlled by controlling the minimum nitrogen filling pressure and the maximum molten pool temperature. The correlation between the molten pool temperature (T, K) and the nitrogen filling pressure (p, KPa) is determined to be a linear relationship, and the linear equation is: p = 0.02546*T-30.81527, as shown in FIG. Figure 1 shown.
[0049] This technical solution can accurately control the nitrogen content in 1Cr12Ni2WMoVNbN high-strength steel during vacuum induction melting. Its practical method and theoretical reasoning can be used to accurately control the nitrogen content in other high-strength steels (steels with similar composition).
[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for accurately controlling the nitrogen content in high-strength steel, which controls the nitrogen content by controlling the minimum nitrogen filling pressure and the maximum molten pool temperature, characterized in that: The following steps are involved: Step 1: Nitrogen filling during alloying period: 1Cr12Ni2WMoVNbN high-strength steel requires nitrogen element control range: N (0.02 ~ 0.08), the target value is 0.06wt.%. Chromium nitride is added during vacuum induction melting alloying, and nitrogen is charged before adding chromium nitride; Step 2: Adjust the temperature during alloying according to the nitrogen filling pressure: After nitrogen filling, adjust the temperature according to the nitrogen filling pressure, and then take samples to test the nitrogen content. Because chromium nitride will burn, the nitrogen content can be accurately controlled by subsequent addition; Step 3: Adjust pouring temperature and nitrogen filling pressure during pouring: At the end of vacuum induction melting, in order to ensure the fluidity of molten steel during the pouring process, a high superheat is generally selected as the pouring temperature. At this time, the nitrogen filling pressure needs to be adjusted accordingly to maintain the nitrogen content.
2. The method for accurately controlling the nitrogen content in high-strength steel according to claim 1, characterized in that: The correlation between the molten pool temperature (T, K) and the nitrogen filling pressure (p, KPa) is a linear relationship, and the linear equation is: p=0.02546*T-30.81527.
3. The method for accurately controlling the nitrogen content in high-strength steel according to claim 1, characterized in that: The composition range of the 1Cr12Ni2WMoVNbN satisfies (wt.%): C (0.13-0.18), Cr (11.00-12.50), Ni (1.70-2.10), W (0.65-1.00), Mo (1.35-1.65), V (0.18-0.30), N (0.02-0.08), Nb (0.20-0.30), Mn≤0.50, Si≤0.50, S≤0.015, P≤0.030, and Al≤0.
02.
4. The method for accurately controlling the nitrogen content in high-strength steel according to claim 1, characterized in that: In the step 1, nitrogen is charged to 15-20 KPa before adding chromium nitride.
5. The method for accurately controlling the nitrogen content in high-strength steel according to claim 1, characterized in that: In step 2, the temperature is adjusted to 1530-1650° C. according to the nitrogen filling pressure.
6. The method for accurately controlling the nitrogen content in high-strength steel according to claim 1, characterized in that: In step 2 and step 3, the appropriate nitrogen filling pressure is matched according to the molten pool temperature to achieve dynamic control of the nitrogen element.