High-pressure melt spinning production process

By spraying surface tension improver at the outlet of the spinneret during melt spinning, the problem of surface tension of fine fluids affecting fiber stretching is solved, and the effect of reducing fracture rate and saving raw materials is achieved.

CN119020874APending Publication Date: 2024-11-26YIBIN QUANLIAN NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411114749.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During melt spinning, the surface tension of the fine fluid will affect the tensile and fracture strength of the fibers. Surfactants and silicone oil are often used in the prior art, but the performance of these agents is affected at high temperatures and need to be mixed into In melt raw materials, resulting in waste and performance changes.

Method used

Directly spray the surface tension improver at the outlet of the spinneret to reduce the concentration of liquid on the surface of the fine fluid, improve tensile performance, avoid the influence of high temperatures, and save the improver.

Benefits of technology

Effectively reduce the breakage rate of fine fluids, improve the tensile performance of fibers, ensure that the performance of surface tension improvers is not affected by high temperatures, and save raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020874A_ABST
    Figure CN119020874A_ABST
Patent Text Reader

Abstract

The invention discloses a high-pressure melt spinning production process, and belongs to the technical field of spinning. Comprising the following steps: S1, preparing a melt raw material: melting a polymer raw material at a high temperature to prepare a polymer melt; s2, continuously and uniformly extruding the polymer melt into a spinning nozzle; s3, fine fluid preparation, wherein fine fluid is pressed out through fine holes in the spinning nozzle; s4, surface tension improvement: spraying a surface tension improver to the surface of the fine fluid; s5, fine fluid stretching: stretching the fine fluid to form fibers; s6, cooling and shaping: performing air-drying, cooling and shaping on the fine fluid; s7, fiber oiling and wetting, wherein fiber oil is evenly smeared on the surfaces of the fibers; and S8, fiber winding: winding the finished fiber into a disc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textiles, and in particular relates to a high-pressure melt spinning production process. Background Art

[0002] Melt spinning refers to the process of forming a relatively stable spinning melt by melting a fiber-forming polymer above its melting point, which is then extruded through a spinneret. The melt jet is cooled and solidified in air or liquid medium to form a semi-finished fiber, which then undergoes post-processing steps such as stretching and heat setting to become a finished fiber. During the fiber forming process, only heat exchange occurs between the melt stream and the surrounding air, and there is no mass transfer process, so the melt spinning process is relatively simple. Among the varieties of synthetic fibers, polyester, nylon and polypropylene are all produced by melt spinning.

[0003] After the melt stream is generated, the winding machine needs to maintain a certain rotation speed to generate a stretching force on the thin fluid, so that the thin fluid is stretched into a fiber with a diameter of 20-30μm before it is completely cooled and formed. Before the thin fluid is solidified to form a fiber, it is in a molten fluid state, and the cohesive force of the liquid molecules on its surface will cause it to generate surface tension; during the stretching process, the surface tension of the thin fluid will directly affect the elongation and breaking strength of the fiber; if the surface tension of the thin fluid is too large, it is easy to break when it is stretched. In the prior art, surfactants and silicone oils are usually used to improve the surface tension, further reduce the surface tension, and improve the tensile properties of the thin fluid.

[0004] In the melt spinning process, surface tension improvers are usually mixed into the melt raw materials to achieve the purpose of improving surface tension; however, since the polymer needs to form a melt in a screw extruder under high temperature conditions of 220-290°C, some surfactants may not be able to withstand the high melting temperature of the polymer, which will affect the performance of the surfactant and thus the surface tension improvement effect of the fluid; in addition, to improve the surface tension of a thin fluid, it is only necessary to destroy or reduce the cohesion of the liquid molecules on its surface, and there is no need to mix the improver into the spinning melt raw materials, which will cause a waste of raw materials. In addition, the surface tension improver may also change the performance of the raw materials. Summary of the invention

[0005] The present invention provides a high-pressure melt spinning production process. After a polymer melt is formed into a thin fluid through a spinneret, a surface tension modifier is directly applied to the thin fluid at the outlet of the spinneret to reduce the liquid cohesion on the surface of the thin fluid, thereby reducing the surface tension of the thin fluid, improving the tensile performance of the thin fluid, and reducing the breakage rate of the thin fluid during the stretching process. The surface tension modifier is directly sprayed on the surface of the formed thin fluid instead of being directly mixed into the polymer melt material, thereby avoiding the influence of high temperature on the performance of the surface tension modifier, resulting in no obvious improvement in the surface tension of the thin fluid. While achieving the purpose of reducing the surface tension of the thin fluid, the raw materials of the surface tension modifier are saved.

[0006] In order to achieve the above technical objectives, the present invention is implemented by the following technical solutions:

[0007] A high pressure melt spinning production process comprises the following steps:

[0008] S1: Preparation of melt raw material: drying polymer particles; feeding the dried polymer particles into a screw extruder, and preparing a polymer melt raw material by high-temperature melting;

[0009] S2: Melt pumping: The polymer melt is continuously and evenly extruded into the spinneret using a metering pump;

[0010] S3: Thin fluid preparation: squeeze out thin fluid through the fine holes in the spinneret;

[0011] S4: Surface tension improvement: At the outlet of the spinneret, a surface tension improver is sprayed on the surface of the formed thin fluid in a circular shape;

[0012] S5: Thin fluid stretching: The thin fluid sprayed with the surface tension modifier is stretched to form fibers; the stretching is accomplished by the rotation of the winding machine;

[0013] S6: Cooling and shaping: While the thin fluid is being stretched, it is air-dried, cooled and shaped in the spinning box so that it will not deform after forming fibers;

[0014] S7: Fiber oiling and wetting: the formed fiber is passed through a roller oiling machine to evenly apply fiber oil on the fiber surface;

[0015] S8: Fiber Winding: The fiber coated with oil enters the winder, and the fiber is wound into a disk through the winder.

[0016] Preferably, the polymer raw material includes any one of polyamide, polyester and polyolefin.

[0017] Preferably, 1-2% of nanocellulose is added to the polymer raw material.

[0018] Preferably, in S1, the melting temperature of the polymer raw material in the screw extruder is set to 220-290°C;

[0019] At the same time, the polymer raw material is preheated and softened in the feeding section of the screw extruder, and inert gas is introduced to remove the air between the polymer raw material particles.

[0020] Preferably, before starting the metering pump in S2, it should be confirmed that the pump is full of melt; and the pressure at the inlet of the metering pump is set to 5-15 MPa.

[0021] Preferably, the spinneret aperture in the spinneret is set to 0.1-0.4 mm;

[0022] The ratio of the length to the diameter of the small holes on the spinneret is set to 20 to 30:1.

[0023] Preferably, the surface tension modifier comprises: one or a mixture of surfactants, silicone oil and lubricants.

[0024] Preferably, the surface tension modifier should be sprayed in a mist form, and the spraying pressure is set to 0.3-0.5 MPa.

[0025] Preferably, in S5, when the thin fluid is stretched, the winding speed of the winder is maintained at 3200-5500 m / min; and the cooling temperature in the spinning box is maintained at 20-25°C.

[0026] Preferably, the fiber oil component in S7 includes: mineral oil, emulsifier, silicone oil, thickener;

[0027] After the fiber surface is coated with oil, the oil content must be maintained at 0.3% to 0.5%.

[0028] The beneficial effects of the present invention are:

[0029] In the melt spinning process provided by the present invention, the surface tension of the thin fluid formed by the melt is improved, and its surface tension is appropriately reduced to enhance the tensile properties of the thin fluid and reduce the tensile fracture rate of the thin fluid; the present invention reduces the surface tension of the thin fluid by spraying a surface tension modifier directly on the surface of the thin fluid at the outlet of the spinneret; the surface tension modifier is not directly mixed into the melt raw material, which ensures that the surface tension modifier will not become invalid at high temperature and affect the purpose of reducing the surface tension; on the other hand, it is only sprayed on the surface of the thin fluid, which saves the surface tension modifier and achieves the purpose of reducing the surface tension of the thin fluid.

[0030] By adding nanocellulose to the melt spinning polymer raw materials, it helps to improve the high temperature stability of the polymer during the high temperature melting process; after the melt material with added nanocellulose is made into fibers, the overall strength performance of the fibers is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] A high pressure melt spinning production process comprises the following steps:

[0036] S1: Preparation of melt raw material: drying the polymer particles; feeding the dried polymer particles into a screw extruder, melting them at a high temperature of 220-290°C to prepare a polymer melt raw material, and preheating and softening the polymer raw material in the feeding section of the screw extruder, and introducing an inert gas to remove the air between the polymer raw material particles; the use of inert gas not only helps preheating and softening, but also maintains the chemical stability of polypropylene during the heating process, avoiding oxidation reaction when it comes into contact with oxygen, thereby affecting the quality of the final product.

[0037] In this embodiment, any one of polyamide, polyester, and polyolefin is used as the raw material for melt spinning; the melting point of the above polymer is lower than the decomposition temperature, and it can be melted and transformed into a viscous flow state after high-temperature heating without significant degradation; when polyester and polyolefin are selected as the spinning melt raw material, the melting temperature is set to 220°C; when polyamide is selected as the spinning melt raw material, the melting temperature is set to 290°C.

[0038] 1-2% of nanocellulose is added to the polymer raw material. Nanocellulose is made from plant cell walls. Adding nanocellulose to the polymer melt raw material can improve the overall high temperature stability of the melt raw material and help improve the strength performance of the final finished fiber.

[0039] S2: Melt pumping: In order to ensure the normal operation of the metering pump gear to transport the melt, before starting the metering pump, make sure that the pump is full of melt; because the viscosity of the melt will change with the change of temperature, which will affect the pressure in the pump and interfere with the accuracy of the metering pump, by ensuring that the pump is pre-filled with melt, the impact of melt temperature fluctuations on the pump accuracy can be minimized.

[0040] Before extruding the melt in the pump, the pressure at the inlet of the metering pump is set to 5-15 MPa in advance to ensure sufficient pressure, and the metering pump is used to accurately and continuously and evenly extrude the polymer melt into the spinneret.

[0041] S3: Thin fluid preparation: squeeze out thin fluid through the fine holes in the spinneret;

[0042] A spinneret is provided in the spinneret. The spinneret is made of heat-resistant and corrosion-resistant stainless steel. A number of spinneret holes are evenly provided on the spinneret. The diameter of the spinneret holes is set to 0.1-0.4 mm. After the fluid coming out of the spinneret holes is stretched to form fibers, the diameter of the fibers is only 20-30 μm.

[0043] The melt passes through the small holes on the spinneret to form a melt stream. The diameter of the stream will expand at the exit of the spinneret hole due to the elasticity of the melt. Different polymers have different degrees of orifice expansion.

[0044] In order to eliminate the orifice expansion effect as much as possible, the ratio of the length to the aperture of the spinneret is increased. In this embodiment, the ratio of the aperture to the length of the spinneret is set to 30:1 based on the aperture of 0.1 mm, which is equivalent to setting the length of the spinneret to 3 mm; the aperture is reduced and the length is increased, so that the fluid has a long enough path to pass through the spinneret. In the slit, the fluid can be gradually and evenly transferred and solidified, and finally come out of the spinneret, and the obvious expansion caused by the aperture limitation is reduced as much as possible. Excessive expansion will affect the stretching effect, resulting in the final fiber formation being affected.

[0045] S4: Surface tension improvement: At the outlet of the spinneret, a surface tension improver is sprayed on the surface of the formed thin fluid in a circular shape;

[0046] The fluid just coming out of the spinneret is in a semi-solid liquid state, and there may be a water film on its surface. The cohesive force between water molecules will form surface tension on the surface of the thin fluid; the surface tension will hinder the stretching of the thin fluid and force the stretching force to increase, while the stretching force that the thin fluid itself can withstand is fixed, so the increase in stretching force may cause the thin fluid to break; therefore, eliminating the surface tension of the thin fluid is the key to stretching to form fibers.

[0047] Surfactants, silicone oils or lubricants can all be used as surface tension modifiers, either alone or as a mixture of several of them. Directly mixing surface tension modifiers into polymer melt materials can improve the surface tension of the thin fluid formed by the melt. However, due to the high temperature of the melt in the screw extruder, the performance of some surface tension modifiers will be affected at high temperatures, and the surface tension modifier only needs to destroy the cohesive force of water molecules on the surface of the thin fluid; there is no need to incorporate it into the raw materials.

[0048] In this embodiment, a circle of atomizing nozzles is arranged in a circular shape below the outlet of the spinneret. The surface tension modifier is sprayed on the surface of the fine fluid coming out of the spinneret by the atomizing nozzles to destroy the cohesive force of water molecules on the surface, thereby achieving the purpose of reducing the surface tension of the fine fluid and increasing the tensile force.

[0049] In order to ensure uniform spraying of the surface tension modifier, the spray pressure of the atomizing nozzle needs to be set within the range of 0.3 to 0.5 MPa.

[0050] S5: Thin fluid stretching: The thin fluid sprayed with the surface tension modifier is stretched to form fibers; the stretching is accomplished by the rotation of the winding machine;

[0051] The winding roller of the winder at the rear end rotates, exerting a stretching force on the thin fluid at the front end; the rotation speed of the winding roller will affect the stretching quality of the thin fluid. If the winding roller rotates too fast, it will cause uneven stretching of the fiber during the stretching process, resulting in problems such as straight fibers and necking; if the winding roller rotates too slowly, it will cause incomplete stretching and the fiber will not have sufficient tension. In this embodiment, the winding speed of the winder is controlled within the range of 3200 to 5500 m / min, and the winding speed is accurately set according to the difference in the polymer melt material used.

[0052] S6: Cooling and shaping: While the thin fluid is being stretched, it is air-dried, cooled and shaped in the spinning box so that it will not deform after forming fibers;

[0053] The wind speed and wind temperature of the cold air blown out of the cooling chamber need to be uniform and constant to ensure that the temperature distribution, velocity distribution and position of the solidification point of the melt flow are constant during the spinning process. Only when the axial tension on the fiber is constant can fibers with uniform thickness and structure be produced. In this embodiment, a number of wind heads are evenly distributed in the spinning box, and the air that absorbs heat and heats up in the spinning box is discharged in a circulating manner. After the air is cooled by refrigerant exchange and becomes cold air, it is circulated into the spinning box. Through continuous circulation of discharging the old and introducing the new, the purpose of maintaining a constant and uniform low-temperature environment in the spinning box is achieved, ensuring that the viscosity critical value and solidification point of the thin fluid can be unified; and the cold air formed by the refrigerant exchange needs to control its temperature within the range of 20 to 25°C, so that there is enough temperature difference between the thin fluid and the environment in the spinning box for heat exchange.

[0054] S7: Fiber oiling and wetting: the formed fiber is passed through a roller oiling machine to evenly apply fiber oil on the fiber surface;

[0055] When the melt fiber is just formed, the surface is relatively dry, which is easy to generate static electricity. The cohesion between the fibers is poor, and the friction with the equipment is large. Therefore, before winding the fiber, it is necessary to evenly coat a layer of oil film on the fiber surface to prevent or eliminate the accumulation of static electricity and make the fiber softer and smoother.

[0056] However, the fiber oil should be selected to eliminate static electricity and soften the fiber without causing mechanical corrosion. The fiber oil components in this embodiment include: mineral oil, emulsifier, silicone oil, thickener; the thickener can be made of natural thickener raw materials such as pectin, alginate, agar, etc.

[0057] The oil content of the fiber after being coated with oil should be kept within the range of 0.3% to 0.5%. If the oil content is too high, white powder will increase during the processing of POY into DTY; while if the oil content is too low, static electricity elimination will be incomplete.

[0058] In addition, it is necessary to ensure that the oil is evenly applied to the fiber surface. If the uneven oil content is too high, the finished silk will become stiff and dyed unevenly.

[0059] S8: Fiber Winding: The fiber coated with oil enters the winder, and the fiber is wound into a disk through the winder.

[0060] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0061] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can well understand and use the present invention. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A high pressure melt spinning production process, characterized in that: The following steps are involved: S1: Preparation of melt raw material: drying polymer particles; feeding the dried polymer particles into a screw extruder, and preparing a polymer melt raw material by high-temperature melting; S2: Melt pumping: The polymer melt is continuously and evenly extruded into the spinneret using a metering pump; S3: Thin fluid preparation: squeeze out thin fluid through the fine holes in the spinneret; S4: Surface tension improvement: At the outlet of the spinneret, a surface tension improver is sprayed on the surface of the formed thin fluid in a circular shape; S5: Thin fluid stretching: The thin fluid sprayed with the surface tension modifier is stretched to form fibers; the stretching is accomplished by the rotation of the winding machine; S6: Cooling and shaping: While the thin fluid is being stretched, it is air-dried, cooled and shaped in the spinning box so that it will not deform after forming fibers; S7: Fiber oiling and wetting: the formed fiber is passed through a roller oiling machine to evenly apply fiber oil on the fiber surface; S8: Fiber Winding: The fiber coated with oil enters the winder, and the fiber is wound into a disk through the winder.

2. A high pressure melt spinning production process according to claim 1, characterized in that: The polymer raw material includes any one of polyamide, polyester and polyolefin.

3. A high pressure melt spinning production process according to claim 1, characterized in that: 1-2% of nanocellulose is added to the polymer raw material.

4. A high pressure melt spinning production process according to claim 1, characterized in that: In S1, the melting temperature of the polymer raw material in the screw extruder is set to 220-290° C.; At the same time, the polymer raw material is preheated and softened in the feeding section of the screw extruder, and inert gas is introduced to remove the air between the polymer raw material particles.

5. A high pressure melt spinning production process according to claim 1, characterized in that: Before starting the metering pump in S2, it should be confirmed that the pump is full of melt; and the pressure at the inlet of the metering pump is set to 5-15 MPa.

6. A high pressure melt spinning production process according to claim 1, characterized in that: The spinneret aperture in the spinneret is set to 0.1 to 0.4 mm; The ratio of the length to the diameter of the small holes on the spinneret is set to 20 to 30:

1.

7. A high pressure melt spinning production process according to claim 1, characterized in that: The surface tension improver includes: one or a mixture of surfactants, silicone oil and lubricants.

8. A high pressure melt spinning production process according to claim 7, characterized in that: The surface tension modifier should be sprayed in a mist form, and the spray pressure is set to 0.3-0.5 MPa.

9. A high pressure melt spinning production process according to claim 1, characterized in that: When the thin fluid is stretched in S5, the winding speed of the winder is maintained at 3200-5500 m / min; and the cooling temperature in the spinning box is maintained at 20-25°C.

10. A high pressure melt spinning production process according to claim 1, characterized in that: The fiber oil component in S7 includes: mineral oil, emulsifier, silicone oil, thickener; After the fiber surface is coated with oil, the oil content must be maintained at 0.3% to 0.5%.

Citation Information

Patent Citations

  • Method of preparing inorganic fiber by utilization of construction waste

    CN103981594A

  • Foam preparation and regenerative spinning forming methods for polyester-cotton blended fabric

    CN109594150A

  • Brittle oligomer continuous melting spinning bundling device

    CN109881275A

  • Heat-resistant hydrolysis-resistant polylactic acid fiber and preparation method thereof

    CN114737276A

  • Wind-free type spinning cooling forming process and device and spinning equipment

    CN114875503A