Shear stripping coupling failure test method for adhesive
By designing porous sector fixtures and adhesive specimens, shear stripping coupling failure tests are realized with different angles loading, which solves the problem that the existing technology cannot carry out shear stripping failure tests of bond interfaces under different load ratios, and provides multiple The flexibility of this damage mode supports the testing of the mechanical properties of the adhesive and the constitutive equations.
Patent Information
- Application Number
- CN202411106550.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art cannot effectively carry out shear peeling failure tests for bonding interfaces under different load ratios, and it is difficult to provide effective test support for adhesive failure mode and constitutive equations, and it is impossible to achieve shear peeling coupling of the full range of adhesive interfaces. Failed loading.
A porous sector-shaped fixture was designed to achieve loading at different angles by drilling holes on the steel plate and processing them into sector sections, combining the design of glued samples and bolt holes, simulating pure shear, shear/peel coupling and pure peeling The damage mode is performed by connecting the fan clamp to the adhesive specimen.
The shear strip coupling failure test of the adhesive structure under different load ratios is realized, providing flexibility for multiple failure modes, supporting the effective testing of the mechanical properties of the adhesive and constitutive equations.
Smart Images

Figure CN119023399A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer mechanical property testing, in particular to a shear peeling coupling failure test method for an adhesive. Background Art
[0002] The governing equation of the single-layer lap joint of linear elastic adhesive shows that the failure mode of the adhesive layer depends on the external load, the adhesive's own properties and the flexibility of the adhesive layer, which makes the deformation of the adhesive layer at the crack tip closely related to the mixed degree of shear stress and peel stress it is subjected to. Therefore, obtaining the shear peel failure behavior of the adhesive layer of the single-lap joint structure under different modes through test means has a key data support role in describing the mechanical properties of the adhesive and establishing the constitutive equation.
[0003] At present, the test methods for testing the shear peeling performance of adhesives in China mainly include the test methods for testing peel strength, the test methods for testing shear strength, and the test methods for testing the adhesive layer under shear peeling orthogonal loads. The test methods for testing peel strength are mainly based on the national standards or industry standards for 90° peeling and 180° peeling tests of adhesives. The relevant standards have the problems of harsh test conditions and difficult operation. Enterprises usually formulate enterprise standards according to product requirements. The test methods for testing shear strength mainly design customized chemical equipment to realize the test of bonding shear strength of the bonding interface in different application scenarios: such as the invention patent "Device and test method for testing shear strength of structural adhesive interface" CN10432856A, designed a cross-shaped specimen bonded by adhesive, and tested the shear stress generated at the bonding interface of the two materials by applying pressure on the bonding substrate; another example is the invention patent "A device and method for testing the shear strength of the bonding interface of structural adhesive" CN106124342A, designed an L-shaped positioning plate to assist in simulating the shear stress working conditions of the bonding interface between glass and substrate in actual engineering. The experimental method for testing the adhesive layer under shear peeling orthogonal loads is to design a device so that the adhesive bonding interface is subjected to horizontal shear and vertical peeling orthogonal loads at the same time to obtain the shear coupling failure mode of the adhesive layer.
[0004] However, as a local component unit of the overall structure of the equipment, the stress form of the adhesive structure is determined by complex boundary conditions and operating loads. Compared with pure shear or pure peel failure, the structure will more often experience shear-peel coupled failure of varying degrees rather than ideal orthogonal coupling. The current testing methods cannot achieve shear-peel failure tests on the bonding interface under different load ratios, nor can they use a set of equipment to complete shear-peel coupled failure loading of the entire range of adhesive interfaces, making it difficult to provide effective experimental support for the establishment of adhesive failure modes and constitutive equations. Summary of the invention
[0005] In order to solve the above problems, the present invention proposes a shear peeling coupling failure test method for an adhesive.
[0006] A shear peeling coupling failure test method for an adhesive, comprising:
[0007] S1. Preparation of porous sector-shaped fixture:
[0008] S11. Select a steel plate with high hardness and strength and process it into the required shape. Drill two bolt holes with equal distance and radius r at the end of the straight section of the steel plate.
[0009] S12, nine bolt holes with a radius of R are drilled at equal intervals in the steel plate sector, and the connecting lines of different bolt holes 2 and bolt holes 1 have different angles with the straight line of the opening segment;
[0010] S2. Preparation of bonding specimens:
[0011] S21, processing the bonded plate: using a milling machine to process the metal block into two rectangular blocks with a size of L×W×H, which are respectively used as bonded plate 1 and bonded plate 2;
[0012] S22, drilling: Drill two bolt holes three with symmetrical equidistant spacing and a radius of r at a position slightly above one end of the bonded plate and a position slightly above the second end of the bonded plate;
[0013] S23, surface treatment: using sandpaper to polish the L×W lower surface of the first bonded board and the L×W upper surface of the second bonded board in turn, then cleaning and drying the polished surfaces with an organic solvent, and performing surface activation treatment;
[0014] S24, bonding positioning: Apply adhesive to the surface-treated bonding surfaces of the L×W lower surface of the first bonded board and the L×W upper surface of the second bonded board, and the adhesive bonds the two bonded boards together to form an uncured bonding sample. After the three are compacted, they are fixed with a mold containing a guide groove;
[0015] S25, curing: according to the curing process requirements of the adhesive, the uncured adhesive specimen is heated and kept warm by a heating device, and then naturally cooled to room temperature, and finally the specimen and the mold are taken out and separated;
[0016] S26. Clean the surface quality: Use sandpaper to smooth the excess adhesive;
[0017] S3. Connect the fan-shaped fixture and the bonding specimen:
[0018] Use four bolts with an outer diameter of 2r to connect the fan-shaped fixture and the bonding specimen together and secure them with nuts;
[0019] S4. Loading test:
[0020] According to different test requirements, bolts with an outer diameter of 2R are used to connect the upper and lower connecting heads of the testing machine to the αi and αi bolt holes of the fan-shaped fixture, and then fixed with nuts to start the test.
[0021] The angles of step S12 are 0°, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80°, and 90°, respectively.
[0022] In step S23, the sandpaper grinding direction should be 45° with the direction of the metal plate L.
[0023] The adhesive in step S24 is coupling agent AC130-2.
[0024] In the step S24 of applying glue, a layer of polytetrafluoroethylene film with a thickness of t needs to be filled between the two bonded boards to ensure that the thickness of the glue layer 3 is equal to t after curing, and at the same time, it can assist in positioning the connection hole position of the test and the fixture 4.
[0025] In the step S4, when αi=0, it is pure shear loading.
[0026] In the step S4, when αi=90, it is pure stripping loading.
[0027] In step S4, the loading angles corresponding to the remaining seven loading pairs are 10°, 20°, 30°, 40°, 50°, 60°, 70°, and 80°, respectively, which can achieve different degrees of shear-stripping coupling loading.
[0028] The beneficial effect of the present invention is that compared with the existing single shear test and peel test, the pair of fan-shaped porous clamps designed in the present invention provide different combinations of loading through multiple connecting holes, so that the adhesive structure undergoes a variety of different failure modes such as pure shear → shear / peel coupling → pure peeling, and flexibly realizes the shear-peel coupling failure test of the adhesive. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0030] Figure 1 It is a schematic diagram of the adhesive shear peeling coupling failure test device of the present invention. DETAILED DESCRIPTION
[0031] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below.
[0032] like Figure 1 As shown, a shear peeling coupling failure test method of an adhesive comprises:
[0033] S1. Prepare a multi-hole fan-shaped fixture. The circular design of the fixture's outer contour can effectively avoid the problem of loading interference. After any pair of loading holes is connected to the chuck of the testing machine, the entire sample device will not interfere with the movement of the testing machine:
[0034] S11. Select a steel plate with high hardness and strength and process it into the required shape. Drill two bolt holes with equal distance and radius r at the end of the straight section of the steel plate. The fixture has the same shape and is replaceable. For test samples of different sizes, it is only necessary to enlarge the size of the fixture in proportion without additionally designing the fixture shape. It has strong applicability and scalability.
[0035] S12, nine bolt holes with a radius of R are drilled at equal intervals in the steel plate sector, and the connecting lines of different bolt holes 2 and bolt holes 1 have different angles with the straight line of the opening segment;
[0036] S2. Preparation of bonding specimens:
[0037] S21, processing the bonded plate: using a milling machine to process the metal block into two rectangular blocks with a size of L×W×H, which are respectively used as bonded plate 1 and bonded plate 2;
[0038] S22, drilling: drill two bolt holes three with symmetrical equidistant spacing and a radius of r at a position slightly above the end of the bonded plate 1 and a position slightly above the end of the bonded plate 2;
[0039] S23, surface treatment: using sandpaper to polish the L×W lower surface of the bonded board 1 and the L×W upper surface of the bonded board 2 in sequence, then cleaning and drying the polished surfaces with an organic solvent, and performing surface activation treatment;
[0040] S24, bonding positioning: applying adhesive to the surface-treated bonding surfaces of the L×W lower surface of the bonded board 1 and the L×W upper surface of the bonded board 2, the adhesive bonds the two bonded boards together to form an uncured bonding sample, and the three are compacted and fixed with a mold containing a guide groove;
[0041] S25, curing: according to the curing process requirements of the adhesive, the uncured adhesive specimen is heated and kept warm by a heating device, and then naturally cooled to room temperature, and finally the specimen and the mold are taken out and separated;
[0042] S26. Clean the surface quality: Use sandpaper to smooth the excess adhesive;
[0043] S3. Connect the fan-shaped fixture and the bonding specimen:
[0044] Use four bolts with an outer diameter of 2r to connect the fan-shaped fixture and the bonding specimen together and secure them with nuts;
[0045] S4. Loading test:
[0046] like Figure 1 As shown, according to different test requirements, bolts with an outer diameter of 2R are used to connect the upper and lower connectors of the testing machine to the αi and αi bolt holes of the fan-shaped fixture, and fixed with nuts to start the test. Figure 1 The reference numeral a represents pure peeling, and the reference numeral b represents pure shearing.
[0047] The steel plate with high hardness and strength in step S1 is preferably a 7B04-T6 aluminum plate alloy block.
[0048] The porous design of the clamp in step S12 ensures that the angles between the loading direction and the adhesive plane direction are 0°, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80°, and 90°, respectively. A pair of clamps can realize the loading of 9 coupled failure modes with strong flexibility, among which 0° is pure shear and 90° is pure peeling.
[0049] Compared with the existing single shear test and peel test, the pair of fan-shaped porous clamps designed in the present invention provide different combinations of loading through multiple connecting holes, so that the adhesive structure undergoes a variety of different failure modes such as pure shear → shear / peel coupling → pure peeling, and flexibly realizes the shear-peel coupling failure test of the adhesive.
[0050] In step S21, a milling machine is used to process the 7B04-T6 aluminum plate alloy block into two rectangular blocks with a size of 100 mm×4 mm×10 mm.
[0051] In step S23, 80-grit sandpaper is used, and the sandpaper is 45° with the length direction of the bonded board to grind the 100mm×4mm lower surface of the bonded board 1 and the 100mm×4mm upper surface of the bonded board 2, and then acetone is used as an organic solvent for cleaning, and then the polished surface is dried.
[0052] The adhesive in step S24 is coupling agent AC130-2.
[0053] In the step S24 of applying glue, a layer of polytetrafluoroethylene film with a thickness of t needs to be filled between the two bonded boards to ensure that the thickness of the glue layer is equal to t after curing, and at the same time, it can assist in positioning the connection hole position of the test and the fixture.
[0054] In the step S25, the bonding test piece is placed in a high temperature oven, heated to 80°C at a heating rate of 2°C / min, kept warm for 3 hours, and then naturally cooled to room temperature. Finally, the sample and the mold are taken out and separated.
[0055] In the step S26, the excess adhesive is smoothed using 120-grit sandpaper.
[0056] In the step S4, when αi=0, it is pure shear loading.
[0057] In the step S4, when αi=90, it is pure stripping loading.
[0058] In step S4, the loading angles corresponding to the remaining seven loading pairs are 10°, 20°, 30°, 40°, 50°, 60°, 70°, and 80°, respectively, which can achieve different degrees of shear-stripping coupling loading.
[0059] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A shear peel coupling failure test method for adhesives, Features: include: S1. Preparation of porous sector-shaped fixture: S11. Select a steel plate with high hardness and strength and process it into the required shape. Drill two bolt holes with equal distance and radius r at the end of the straight section of the steel plate. S12, nine bolt holes with a radius of R are drilled at equal intervals in the steel plate sector, and the connecting lines of different bolt holes 2 and bolt holes 1 have different angles with the straight line of the opening segment; S2. Preparation of bonding specimens: S21, processing the bonded plates: using a milling machine to process the metal block into two rectangular blocks with dimensions of L×W×H, which are bonded plates 1 (1) and 2 (2), respectively; S22, drilling: Drill two bolt holes three symmetrically and equidistantly with a radius of r at a position slightly above the end of the first bonded plate (1) and at a position slightly above the end of the second bonded plate (2); S23, surface treatment: using sandpaper to polish the L×W lower surface of the first bonded board (1) and the L×W upper surface of the second bonded board (2) in sequence, then cleaning and drying the polished surfaces with an organic solvent, and performing a surface activation treatment; S24, bonding positioning: Apply adhesive to the surface-treated bonding surfaces of the L×W lower surface of the first bonded board (1) and the L×W upper surface of the second bonded board (2), and the adhesive bonds the two bonded boards together to form an uncured bonding sample. After the three are compacted, they are fixed with a mold containing a guide groove; S25, curing: according to the curing process requirements of the adhesive, the uncured adhesive specimen is heated and kept warm by a heating device, and then naturally cooled to room temperature, and finally the specimen and the mold are taken out and separated; S26. Clean the surface quality: Use sandpaper to smooth the excess adhesive; S3. Connect the fan-shaped fixture and the bonding specimen: Use four bolts with an outer diameter of 2r to connect the fan-shaped fixture and the bonding specimen together and secure them with nuts; S4. Loading test: According to different test requirements, bolts with an outer diameter of 2R are used to connect the upper and lower connecting heads of the testing machine to the αi and αi bolt holes of the fan-shaped fixture, and then fixed with nuts to start the test.
2. The shear peeling coupling failure test method of an adhesive according to claim 1, Features: The angles of step S12 are 0°, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80°, and 90°, respectively.
3. The shear peel coupling failure test method of an adhesive according to claim 1, Features: In step S23, the sandpaper grinding direction should be 45° with the direction of the metal plate L.
4. The shear peeling coupling failure test method of an adhesive according to claim 1, Features: The adhesive in step S24 is coupling agent AC130-2.
5. The shear peeling coupling failure test method of an adhesive according to claim 1, Features: In the step S24 of applying glue, a layer of polytetrafluoroethylene film with a thickness of t needs to be filled between the two bonded plates to ensure that the thickness of the glue layer (3) is equal to t after curing, and at the same time can assist in positioning the connection hole position of the test and the fixture (4).
6. The shear peeling coupling failure test method of an adhesive according to claim 1, Features: In the step S4, when αi=0, it is pure shear loading.
7. The shear peeling coupling failure test method of an adhesive according to claim 6, Features: In the step S4, when αi=90, it is pure stripping loading.
8. The shear peeling coupling failure test method of an adhesive according to claim 7, Features: In step S4, the loading angles corresponding to the remaining seven loading pairs are 10°, 20°, 30°, 40°, 50°, 60°, 70°, and 80°, respectively, which can achieve different degrees of shear-stripping coupling loading.