Lithium secondary battery and electric device

By using electrolyte solvents and additives with specific structures in lithium secondary batteries, the lithium-ion diffusion coefficient is controlled to form an SEI film, which solves the problem of lithium-ion diffusion mismatch and improves the fast-charging performance and cycle performance of lithium secondary batteries.

CN119029321AActive Publication Date: 2024-11-26CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202411114041.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-11-26
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

The mismatch in the diffusion coefficients of lithium ions in the positive electrode active material layer and the electrolyte in lithium secondary batteries limits fast charging performance and affects charge and discharge performance.

Method used

By employing electrolyte solvents and additives with specific structures, the lithium-ion diffusion coefficient and electrolyte transport rate are controlled to form a stable SEI film, thereby improving the lithium-ion transport rate in the electrolyte and the stability of the negative electrode active material layer.

Benefits of technology

It improves the fast-charging and cycle performance of lithium secondary batteries, and enhances the energy density and lifespan of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029321A_ABST
    Figure CN119029321A_ABST
Patent Text Reader

Abstract

The invention provides a lithium secondary battery and an electric device. The lithium secondary battery comprises a positive pole piece, the positive pole piece comprises a positive current collector and a positive active material layer arranged on at least one side of the positive current collector, and the lithium ion diffusion coefficient Ds of the positive active material layer is 10 <-16 > cm < 2 > / s-10 <-5 > cm < 2 > / s; the electrolyte comprises a solvent, the solvent comprises at least one of compounds shown in the formula (I), and the mass fraction W1 of the compounds shown in the formula (I) in the solvent is 20%-80%; in the formula (I), R1 and R2 respectively and independently comprise at least one of alkyl with the carbon atom number of 1-3 and halogenated alkyl with the carbon atom number of 1-3. According to the lithium secondary battery, the lithium ion diffusion coefficient Ds of the positive electrode material and the use amount of the compound shown in the formula (I) are regulated and controlled, so that the transmission rate of lithium ions in electrolyte can be effectively improved, and the energy density and the fast charging performance of the lithium secondary battery are improved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of Chinese patent application No.: 202380011591.X, filed on February 24, 2023, with the invention name “Lithium Secondary Battery and Electrical Device”. Technical Field

[0002] The present application relates to the field of battery technology, and in particular to a lithium secondary battery and an electrical device. Background Art

[0003] In recent years, secondary batteries have been widely used in various electronic products and electric vehicles due to their high power density and volumetric capacity. With the great development and wide application of secondary batteries, higher requirements have been put forward for their energy density and fast charging performance.

[0004] The fast charging of lithium secondary batteries relies on the rapid release of lithium ions from the positive electrode active material, moving to the negative electrode through the electrolyte and quickly embedding into the negative electrode active material. Therefore, the fast charging performance of lithium secondary batteries is closely related to the transmission rate of lithium ions in the electrode material and the electrolyte. The diffusion coefficient of lithium ions in the electrode material and the electrolyte is one of the parameters that reflect the transmission rate of lithium ions in the electrode material and the electrolyte. However, the diffusion coefficient of lithium ions in the electrode material is difficult to match the diffusion coefficient of lithium ions in the electrolyte, which seriously affects the charging and discharging performance of lithium ions. Therefore, how to improve the charging and discharging performance of lithium secondary batteries has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] The present application is made in view of the above technical problems, and its purpose is to provide a lithium secondary battery and an electric device, wherein the lithium secondary battery can improve the transfer of lithium ions in the positive electrode active material layer and the electrolyte.

[0006] The transmission rate can be increased, thereby helping to improve the fast charging performance of lithium secondary batteries.

[0007] In a first aspect, the present application provides a lithium secondary battery, the lithium secondary battery comprising: a positive electrode plate, the positive electrode plate comprising a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, the lithium ion diffusion coefficient of the positive electrode active material layer being Ds; an electrolyte, the electrolyte comprising a solvent, the solvent comprising at least one of the compounds of the following formula (I), the mass fraction of the compound of formula (I) in the solvent being W1, the mass fraction W1 of the compound of formula (I) and the lithium ion diffusion coefficient Ds of the positive electrode active material layer satisfying: 2×10 -18 cm 2 / s≤W1×Ds≤8×10 -6 cm 2 / s; optionally, 3×10 -14 cm2 / s≤W1×Ds≤7×10 -10 cm 2 / s;

[0008]

[0009] Wherein, R1 and R2 independently include at least one of an alkyl group having 1 to 3 carbon atoms and a halogenated alkyl group having 1 to 3 carbon atoms.

[0010] In the embodiments of the present application, the compound shown in formula (I) as a solvent or as a part of a solvent can make the electrolyte have a higher conductivity. When the lithium secondary battery is charged, lithium ions are released from the positive electrode active material, move to the surface of the negative electrode active material layer through the electrolyte, and then embed into the negative electrode active material. According to the lithium ion diffusion coefficient Ds of the positive electrode material in the lithium secondary battery, by controlling the amount of the compound shown in formula (I), the transmission rate of lithium ions in the electrolyte can be effectively improved, so that the electrolyte can transfer a large amount of lithium ions released from the positive electrode active material to the negative electrode in time, thereby improving the fast charging performance of the lithium secondary battery.

[0011] In some embodiments, R1 and R2 each independently include at least one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl, and fluoropropyl.

[0012] In some embodiments, 10 -16 cm 2 / s≤Ds≤10 -5 cm 2 / s; optionally, 10 -14 cm 2 / s≤Ds≤10 -9 cm 2 / s.

[0013] In some embodiments, 20%≤W1≤80%; alternatively, 30%≤W1≤70%.

[0014] In some embodiments, the compound of formula (I) comprises at least one of the following compounds:

[0015]

[0016] Optionally, the compound of formula (I) includes at least one of a compound of formula (II), a compound of formula (I-II), a compound of formula (IV), and a compound of formula (I-VIII).

[0017] In some embodiments, the electrolyte includes a first additive, the first additive including at least one of the compounds of formula (II):

[0018]

[0019] Among them, R3 includes at least one of an alkylene group with 2-10 carbon atoms which is substituted or unsubstituted by Ra, a heteroalkylene group with 2-10 carbon atoms which is substituted or unsubstituted by Ra, an arylene group with 6-18 carbon atoms which is substituted or unsubstituted by Ra, a heteroarylene group with 6-18 carbon atoms which is substituted or unsubstituted by Ra, a cycloaliphatic group with 3-18 carbon atoms which is substituted or unsubstituted by Ra, and a heterocycloaliphatic group with 3-18 carbon atoms which is substituted or unsubstituted by Ra; Ra includes at least one of a halogen atom, a cyano group, an isocyanate group, a hydroxyl group, a carboxyl group, a sulfonic acid group, an ester group, an alkyl group with 2-10 carbon atoms, an alkenyl group with 2-10 carbon atoms, an alkynyl group with 2-10 carbon atoms, and an oxoalkyl group with 2-10 carbon atoms.

[0020] The embodiments of the present application, by introducing a first additive into the electrolyte, help to form a protective SEI (Solid Electrolyte Interface, SEI) film on the surface of the negative electrode active material layer of the lithium secondary battery, which can effectively improve the stability of the solid-liquid interface between the negative electrode and the electrolyte, and improve the problem of gas generation of the electrolyte at the interface between the negative electrode active material layer and the electrolyte during the fast charging process of the lithium secondary battery, thereby helping to improve the cycle performance of the lithium secondary battery.

[0021] In some embodiments, the mass fraction of the first additive in the electrolyte is W2, and W2, W1, and Ds satisfy: 2×10 -22 cm 2 / s≤W2×W1×Ds≤1.6×10 -6 cm 2 / s; optionally, 2×10 -21 cm 2 / s≤W2×W1×Ds≤8×10 -7 cm 2 / s; optionally, 4×10 -21 cm 2 / s≤W2×W1×Ds≤4×10 -7 cm 2 / s.

[0022] In some embodiments, W2 satisfies: 0.01%≤W2≤20%; optionally, 0.1%≤W2≤10%; optionally, 0.2%≤W2≤5%.

[0023] In some embodiments, the first additive includes at least one of the following compounds:

[0024]

[0025]

[0026] In some embodiments, the electrolyte includes a second additive, wherein the second additive includes M a+ [F w PO t ] b- 、M a+ [BF4] - a 、M a+ [FSO3] - a and at least one of the compounds of formula (III):

[0027]

[0028] Among them, M a+ It includes at least one of lithium ion, sodium ion, potassium ion, rubidium ion, cesium ion, magnesium ion, calcium ion, barium ion, aluminum ion, iron ion, copper ion, nickel ion and organic cation, a, b and c all represent natural numbers; t represents an integer of 0-3, w represents an integer of 1-6; X includes at least one of halogen atoms, n represents an integer of 0-4; Y includes at least one of boron atom and phosphorus atom; R4 includes substituted or unsubstituted alkylene with 1-10 carbon atoms, substituted or unsubstituted halogenated alkylene with 1-10 carbon atoms, substituted or unsubstituted arylene with 6-20 carbon atoms, substituted or unsubstituted halogenated arylene with 6-20 carbon atoms, q represents an integer of 0-1, and m represents an integer of 1-3.

[0029] In the embodiments of the present application, the introduction of the second additive into the electrolyte helps to form a SEI film on the surface of the negative electrode active material layer, further improving the stability of the solid-liquid interface between the negative electrode and the electrolyte, thereby further improving the cycle performance of the lithium secondary battery.

[0030] In some embodiments, the mass fraction of the second additive in the electrolyte is W3, and W3, W1, and Ds satisfy: 2×10 -22 cm 2 / s≤W3×W1×Ds≤1.6×10 -6 cm 2 / s; optionally, 2×10 -21 cm 2 / s≤W3×W1×Ds≤8×10 -7 cm 2 / s; optionally, 4×10 -21 cm 2 / s≤W3×W1×Ds≤4×10 -7 cm2 / s.

[0031] In some embodiments, 0.01%≤W3≤20%; alternatively, 0.1%≤W3≤10%; alternatively, 0.2%≤W3≤5%.

[0032] In some embodiments, in M a+ [FSO3] - a In, M a+ Including Li + , Na + , K + , Rb + , Cs + ,Mg 2+ , Ca 2+ , Ba 2+ , Al 3 + , Fe 2+ , Cu 2+ , Fe 3+ , Ni 2+ , Ni 3+ At least one of .

[0033] In some embodiments, the positive electrode active material layer includes a first positive electrode active material and a second positive electrode active material; the average particle size Dv501 of the first positive electrode active material satisfies: 8μm≤Dv501≤50μm; the average particle size Dv502 of the second positive electrode active material satisfies: 0.02μm≤Dv502≤8μm.

[0034] In the embodiments of the present application, by combining a first active material having a larger average (volume) particle size with a second active material having a smaller average (volume) particle size, it helps to increase the powder compaction density of the positive electrode sheet, thereby helping to increase the energy density of the lithium secondary battery.

[0035] In some embodiments, the mass fraction W4 of the second positive electrode active material in the positive electrode active material layer satisfies: 0%≤W4≤60%; optionally, 20%≤W4≤40%.

[0036] In some embodiments, the lithium secondary battery includes: a negative electrode plate, the negative electrode plate includes a negative electrode collector and a negative electrode active material layer disposed on the negative electrode collector, the negative electrode active material layer includes a negative electrode active material; the average particle size Dv503 of the negative electrode active material satisfies: 6μm≤Dv503; optionally, 15μm≤Dv503≤20μm.

[0037] In the embodiments of the present application, by setting the average (volume) particle size of the negative electrode active material within a suitable range, after the first additive and / or the second additive forms a SEI film of a certain thickness on the surface of the negative electrode active material layer, the average volume particle size of the surface negative electrode active material increases and the specific surface area decreases, thereby helping to reduce the contact area between the surface negative electrode active material and the electrolyte, thereby reducing the probability of side reactions of the electrolyte on the surface of the negative electrode active material layer and improving the cycle performance of the lithium secondary battery.

[0038] In some embodiments, the specific surface area of ​​the negative electrode active material satisfies: 0.5 m 2 / g≤BET≤2.0m 2 / g; optionally, 0.8m 2 / g≤BET≤1.5m 2 / g.

[0039] In the embodiments of the present application, by setting the specific surface area of ​​the negative electrode active material within a suitable range, after the first additive and / or the second additive forms an SEI film of a certain thickness on the surface of the negative electrode active material layer, the specific surface area of ​​the surface negative electrode active material is reduced, thereby reducing the contact area between the negative electrode active material and the electrolyte, reducing the probability of side reactions of the electrolyte on the surface of the negative electrode active material layer, and improving the cycle performance of the lithium secondary battery.

[0040] In a second aspect, an electrical device is provided, wherein the electrical device comprises a lithium secondary battery as described in any embodiment of the first aspect.

[0041] Therefore, the lithium secondary battery provided in the present application has good fast charging performance and cycle performance, and the power-consuming device provided in the present application can be efficiently fast charged and has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work. In the drawings, the drawings are not drawn according to the actual scale.

[0043] Figure 1 It is a schematic diagram of a secondary battery of the present application.

[0044] Figure 2 It is a schematic structural diagram of a secondary battery of the present application.

[0045] Figure 3 It is a schematic structural diagram of a battery module of the present application.

[0046] Figure 4 It is a schematic diagram of a battery pack of the present application.

[0047] Figure 5 It is a schematic structural diagram of a battery pack of the present application.

[0048] Figure 6 It is a schematic diagram of an electrical device of the present application. DETAILED DESCRIPTION

[0049] Hereinafter, the embodiments of the lithium secondary battery and the electric device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0050] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0051] In the description of the present application, it should be noted that, unless otherwise specified, "multiple" means more than two; the terms "upper", "lower", "left", "right", "inside", "outside", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first", "second", "third", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. "Vertical" is not strictly vertical, but is within the allowable error range. "Parallel" is not strictly parallel, but is within the allowable error range.

[0052] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0053] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0054] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0055] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0056] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0057] Unless otherwise specified, the following terms have the following meanings. Any undefined terms have their generally accepted meanings in the art.

[0058] The term "alkyl" has a general meaning and refers to a monovalent saturated hydrocarbon group having one or more carbon atoms, optionally 1 to 3. For example, alkyl includes straight chain hydrocarbon groups and branched chain hydrocarbon groups, such as methyl, ethyl, n-propyl, isopropyl, etc.

[0059] The term "haloalkyl" has a common meaning and refers to an alkyl group in which one or more hydrogen atoms on one or more carbon atoms in a straight chain, branched chain or ring skeleton are replaced by halogen atoms, for example, monochloromethyl, monofluoromethyl, trifluoromethyl, monofluoroethyl, monofluoropropyl, etc.

[0060] The term "alkylene" has a general meaning and refers to a divalent hydrocarbon group having one or more carbon atoms, optionally 1 to 10. For example, alkylene includes divalent straight-chain hydrocarbon groups and divalent branched hydrocarbon groups, such as ethylene, methylethylene, n-propylene, and the like.

[0061] The term "alkylene substituted with Ra" refers to an alkylene group in which one or more hydrogen atoms on one or more carbon atoms in a linear, branched or cyclic backbone are replaced with Ra.

[0062] The term "heteroalkylene" has a common meaning and refers to an alkylene group in which one or more carbon atoms in a straight chain, branched chain or ring backbone are independently substituted by the same or different heteroatoms or groups. The heteroatoms or groups include, but are not limited to, halogen atoms, oxygen atoms, sulfur atoms, peroxy groups, perthio groups, thiooxy groups, phenyl groups, etc.

[0063] The term "heteroalkylene substituted with Ra" refers to heteroalkylene groups in which one or more hydrogen atoms on one or more carbon atoms in the linear, branched or cyclic backbone are replaced with Ra.

[0064] The term "arylene group" has a general meaning and refers to a divalent aromatic group derived by removing one hydrogen atom each from two different carbon atoms of an aromatic compound or removing two hydrogen atoms from one carbon atom of an aromatic compound.

[0065] The term "arylene substituted with Ra" refers to an arylene group in which one or more hydrogen atoms on one or more carbon atoms in a linear, branched or cyclic backbone are replaced with Ra.

[0066] The term "heteroarylene" has the usual meaning and refers to an arylene group in which one or more carbon atoms are each independently substituted with the same or different heteroatoms or groups.

[0067] The term "heteroarylene substituted with Ra" refers to a heteroarylene group in which one or more hydrogen atoms on one or more carbon atoms in a linear, branched or cyclic backbone are replaced with Ra.

[0068] The term "alicyclic group" has a general meaning, and refers to a divalent alicyclic group derived from an alicyclic hydrocarbon molecule by removing two hydrogen atoms.

[0069] The term "alicyclic group substituted with Ra" refers to an alicyclic group in which one or more hydrogen atoms on one or more carbon atoms in a linear, branched or cyclic backbone are replaced with Ra.

[0070] The term "heteroalicyclic group" has a general meaning, and refers to a heteroalicyclic group in which one or more carbon atoms in the straight chain, branched chain or ring backbone are independently substituted by the same or different heteroatoms or groups.

[0071] The term "alicyclic group substituted with Ra" refers to a heteroalicyclic group in which one or more hydrogen atoms on one or more carbon atoms in a linear, branched or cyclic backbone are replaced with Ra.

[0072] The term "halogen atom" has a usual meaning, and refers to a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, and an astatine atom.

[0073] The term "alkenyl" has a common meaning and refers to a hydrocarbon group having one or more carbon atoms and having at least one double bond unsaturated site. Optionally, the number of carbon atoms is 2-10. For example, alkenyl includes straight chain alkenyl and straight chain alkenyl. For example, vinyl, propenyl, n-butenyl, etc. In some other examples, alkenyl can also include cyclic alkenyl, bicycloalkenyl, etc. For example, cyclohexyl.

[0074] The term "alkynyl" has the usual meaning and refers to a hydrocarbon group having one or more carbon-carbon triple bonds. Optionally, the number of carbon atoms is 2-10. For example, ethynyl.

[0075] The term "oxaalkyl" has the usual meaning and refers to an alkyl group in which one or more carbon atoms in the straight chain, branched chain or ring backbone are replaced by oxygen atoms.

[0076] The term "substituted alkylene" has the usual meaning and refers to an alkylene group in which one or more hydrogen atoms on one or more carbon atoms in the linear, branched or cyclic backbone are replaced by the same or different heteroatoms or groups.

[0077] The term "haloalkylene" has a general meaning and refers to an alkylene group in which one or more hydrogen atoms on one or more carbon atoms in a linear, branched or cyclic backbone are replaced by the same or different halogen atoms.

[0078] The term "substituted haloalkylene" has the usual meaning and refers to a haloalkylene group in which one or more hydrogen atoms on one or more carbon atoms in a linear, branched or cyclic backbone are replaced by the same or different heteroatoms or groups.

[0079] The term "substituted arylene" refers to an arylene group in which one or more hydrogen atoms on one or more carbon atoms in the linear, branched or cyclic backbone are replaced by the same or different heteroatoms or groups.

[0080] The term "haloarylene" refers to an arylene group in which one or more hydrogen atoms on one or more carbon atoms in the linear, branched or cyclic backbone are replaced by the same or different halogen atoms or groups.

[0081] The term "substituted haloarylene" refers to a haloarylene group in which one or more hydrogen atoms on one or more carbon atoms in the linear, branched or cyclic backbone are replaced by the same or different heteroatoms or groups.

[0082] The term "lithium ion diffusion coefficient" refers to the average number of lithium ions passing through a medium per unit area per unit time, which can represent the penetration rate of lithium ions in the medium. The diffusion process of lithium ions in the solid phase includes diffusion based on the transposition mechanism in ionic crystals, diffusion caused by the influence of concentration gradients, and diffusion caused by chemical potential. In the embodiments of the present application, the lithium ion diffusion coefficient can also be expressed by the chemical diffusion coefficient of lithium ions, which covers the above-mentioned multiple diffusion processes.

[0083] In the examples of the present application, the particle size distribution is used to reflect the average (volume) particle size of the material.

[0084] The term "Dv50" refers to the particle size corresponding to the cumulative particle size distribution of the material reaching 50%. Its physical meaning is that the particles larger or smaller than this particle size account for 50% of the total number of particles in the material. The "1" in "Dv501" is a superscript, indicating the Dv50 of a certain material, which is used to distinguish it from the Dv50 of other materials and has no other restrictive meaning.

[0085] Next, embodiments of the present application are introduced.

[0086] In recent years, secondary batteries have been widely used in power tools, electronic products, electric vehicles, aerospace and other fields due to their high energy density and long service life, and have achieved great development. Usually, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the charge and discharge process of the battery, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. Among them, the electrolyte plays a role in conducting active ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, which allows active ions to pass through while preventing the positive and negative electrodes from short-circuiting, so that the electrochemical reaction of the secondary battery proceeds normally.

[0087] Take lithium secondary ion battery as an example. Lithium secondary battery is a typical secondary battery. Because it relies on the chemical reaction of lithium ion intercalation between positive and negative electrodes for charging and discharging, lithium secondary battery is also called rocking chair battery. During the charging process of lithium secondary battery, lithium ions are released from the positive electrode active material, moved to the negative electrode through the conduction of electrolyte and embedded in the negative electrode active material; and during the discharge process, lithium ions are released from the negative electrode active material, moved to the positive electrode through the conduction of electrolyte and embedded in the positive electrode active material.

[0088] It should be understood that the "lithium insertion" and "embedding" processes described in this application refer to the process in which lithium ions are embedded in the positive electrode active material or the negative electrode active material due to an electrochemical reaction, and the "extraction", "delithium" and "extraction" processes described in this application refer to the process in which lithium ions are extracted from the positive electrode active material or the negative electrode active material due to an electrochemical reaction.

[0089] With the increasing application of lithium secondary batteries, the requirements for the performance of lithium secondary batteries in different fields are also getting higher and higher. For example, in the field of electric vehicles, lithium secondary batteries are required to have high energy density and fast charging capabilities. As can be seen from the above, during the charging process of lithium secondary batteries, lithium ions are released from the positive electrode active material, moved to the negative electrode through the electrolyte and embedded in the negative electrode active material. On the one hand, in order to achieve a higher energy density, more positive and negative electrode active materials need to be loaded on the positive and negative electrode sheets, which makes the thickness of the positive and negative electrode active material layers of the sheets thicker than that of ordinary lithium secondary batteries. Taking the positive electrode sheet as an example, in order to ensure that the lithium ions in the positive electrode active material away from the surface of the positive electrode active material layer can be smoothly released, the lithium ion diffusion coefficient of the positive electrode active material layer is usually large. On the other hand, the positive electrode active material layer and the electrolyte have different abilities to conduct lithium ions. Generally speaking, the lithium ion diffusion coefficient of lithium ions in the positive electrode active material layer (solid phase) is greater than the lithium ion diffusion coefficient of lithium ions in the electrolyte (liquid phase). The mismatch between the solid-phase diffusion coefficient and the liquid-phase diffusion coefficient of lithium ions results in a large number of lithium ions being released from the positive electrode active material during the fast charging process of lithium secondary batteries. Due to the limited lithium ion conductivity of the electrolyte, they cannot be transferred to the negative electrode in time, limiting the fast charging performance of lithium secondary batteries.

[0090] In view of this, an embodiment of the present application provides a lithium secondary battery, in which the solvent of the electrolyte includes a linear carboxylic acid ester compound as shown in formula (I), and the compound shown in formula (I) has a higher dielectric constant and a lower viscosity, thereby improving the ability of the electrolyte to conduct lithium ions. In addition, in the lithium secondary battery, the mass fraction of the compound shown in formula (I) is regulated within a suitable range according to the lithium ion diffusion coefficient of the positive electrode active material layer, so that the lithium secondary battery has a higher energy density and good fast charging performance.

[0091] In one embodiment of the present application, a lithium secondary battery is provided. Generally, the lithium secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. Next, the lithium secondary battery provided by the present application and various parts of the lithium secondary battery are introduced.

[0092] In one embodiment of the present application, a lithium secondary battery is provided. The lithium secondary battery includes a positive electrode plate and an electrolyte.

[0093] The positive electrode plate includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, and the lithium ion diffusion coefficient of the positive electrode active material layer is Ds.

[0094] The electrolyte includes a solvent, and the solvent includes at least one of the compounds of the following formula (I), and the mass fraction of the compound represented by the formula (I) in the electrolyte is W1. The mass fraction W1 of the compound represented by the formula (I) and the lithium ion diffusion coefficient Ds of the positive electrode active material layer satisfy: 2×10 -18 cm 2 / s≤W1×Ds≤8×10 -6 cm 2 / s; optionally, 3×10 -14 cm 2 / s≤W1×Ds≤7×10 -10 cm 2 / s;

[0095]

[0096] Wherein, R1 and R2 independently include at least one of an alkyl group having 1 to 3 carbon atoms and a halogenated alkyl group having 1 to 3 carbon atoms.

[0097] Specifically, W1×Ds can be 2×10 -18 cm 2 / s, 2×10 -17 cm 2 / s, 2×10 -16 cm 2 / s, 2×10 - 15 cm 2 / s, 2×10 -14 cm 2 / s, 3×10 -14 cm 2 / s, 2×10 -12 cm 2 / s, 2×10 -11 cm 2 / s, 7×10 -10 cm 2 / s, 2×10 -9 cm 2 / s, 2×10 -8 cm 2 / s, 2×10 -7 cm 2 / s, 8×10 -6 cm 2 / s, or its value is within the range obtained by combining any two of the above values.

[0098] In this embodiment, the lithium secondary battery has a positive electrode active material layer with a lithium ion diffusion coefficient of Ds, and has an electrolyte matched with the positive electrode active material layer. The solvent of the electrolyte includes a compound shown in formula (I), so that the electrolyte has a higher conductivity. The mass fraction W1 of the compound in the electrolyte is regulated according to the lithium ion diffusion coefficient Ds of the positive electrode active material layer so that the product of the two is within an appropriate range. This can improve the problem of mismatch between the lithium ion diffusion capacity of the positive electrode active material layer and the electrolyte in the lithium secondary battery, and improve the fast charging capability of the lithium secondary battery while achieving a higher energy density of the lithium secondary battery.

[0099] The lithium ion diffusion coefficient Ds of the positive electrode active material is related to factors such as the particle size of the positive electrode active material, the morphology of the positive electrode active material, and the ion conductivity of the positive electrode active material itself. The lithium ion diffusion coefficient Ds of the positive electrode active material can be regulated by regulating the particle size of the positive electrode active material, changing the morphology of the positive electrode active material, and the like.

[0100] As an example, the lithium ion diffusion coefficient Ds of the positive electrode active material can be regulated by the following method: the raw materials Li2CO3, H3PO4, and FeCl2·4H2O are added to anhydrous ethanol in a molar ratio of 1:1:1, stirred evenly, and the stirring was stopped after the reaction of the raw materials was completed, and the sol was immediately converted into a gray gel. After standing at room temperature, the gray gel was transferred to a blast drying oven at 80°C and dried for 12 hours. Then the dried gel was placed in an alumina magnetic boat, moved into a tubular atmosphere furnace, and heat treated in an argon atmosphere. The heat treatment can be carried out by a two-step calcination method, namely pre-calcination and final calcination. The heat treatment conditions for pre-calcination are to keep warm at 350°C for 5 hours. The heat treatment conditions for the final calcination are to keep warm at 500°C-800°C for 10h-25h. In order to achieve the regulation of the lithium ion diffusion coefficient Ds, an appropriate amount of citric acid (e.g., 0 mol, 0.2 mol, 0.5 mol, 1 mol or 2 mol) can be added to the sol after the raw material reaction is completed, and the stirring time can be extended by 3 hours. By adding citric acid to the sol after the raw material reaction is completed, in the process of subsequent calcination, the amorphous carbon obtained by the pyrolysis of citric acid can be coated on the surface of the particles. The presence of the carbon coating will limit the further diffusion of the reactants, play a steric hindrance effect, thereby reducing the growth rate of the crystal, and the introduction of carbon is conducive to the refinement of the grains. Thus, by regulating the addition amount of citric acid, positive electrode materials of different particle sizes can be obtained, and then positive electrode materials of different lithium ion diffusion coefficients can be obtained. The lithium ion diffusion coefficient Ds can be directly tested by constant current intermittent titration (GITT method).

[0101] In one embodiment of the present application, the solvent may include only the compound of formula (I). When the solvent includes only the compound of formula (I), the electrode liquid has good conductivity and fluidity due to the higher conductivity and lower viscosity of the compound of formula (I), and can also improve the problem of mismatch between the lithium ion diffusion capacity of the positive electrode active material layer and the electrolyte in the lithium secondary battery, and improve the fast charging capability of the lithium secondary battery while realizing a high energy density lithium secondary battery.

[0102] Optionally, R1 and R2 independently include at least one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl, and fluoropropyl.

[0103] Optionally, the compound of formula (I) comprises at least one of the following compounds:

[0104]

[0105] Optionally, the compound of formula (I) includes at least one of a compound of formula (II), a compound of formula (I-II), a compound of formula (IV), and a compound of formula (I-VIII).

[0106] Next, the positive electrode sheet and the electrolyte in the lithium secondary battery are introduced in detail.

[0107] [Electrolyte]

[0108] The electrolyte plays a role in conducting lithium ions between the positive electrode and the negative electrode. The electrolyte includes a solute and a solvent, and the solute is dissolved in the solvent to form a uniform electrolyte.

[0109] In the lithium secondary battery provided in the present application, the solvent of the electrolyte includes the compound represented by formula (I).

[0110] Optionally, the mass fraction W1 of the compound represented by formula (I) in the electrolyte is positively correlated with the lithium ion diffusion coefficient Ds of the positive electrode active material layer.

[0111] Specifically, as the positive electrode active material load increases, a positive electrode active material with a larger lithium ion diffusion coefficient Ds is selected, and a higher proportion of the compound represented by formula (I) is required to improve the lithium ion conductivity of the electrolyte to match the lithium ion conductivity of the positive electrode active material layer.

[0112] Optionally, the mass fraction W1 of the compound represented by formula (I) in the electrolyte satisfies: 20%≤W1≤80%; further optionally, 30%≤W1≤70%.

[0113] Specifically, W1 can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, or its value is within the range obtained by combining any two of the above values.

[0114] Optionally, in some other embodiments, the solvent may also include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0115] Optionally, the solute of the electrolyte includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate and lithium tetrafluorooxalatophosphate.

[0116] Optionally, the electrolyte includes a first additive, the first additive including at least one of the compounds of formula (II):

[0117]

[0118] Wherein, R3 includes at least one of an alkylene group having 2-10 carbon atoms which is substituted or unsubstituted by Ra, a heteroalkylene group having 2-10 carbon atoms which is substituted or unsubstituted by Ra, an arylene group having 6-18 carbon atoms which is substituted or unsubstituted by Ra, a heteroarylene group having 6-18 carbon atoms which is substituted or unsubstituted by Ra, an alicyclic group having 3-18 carbon atoms which is substituted or unsubstituted by Ra, and a heteroalicyclic group having 3-18 carbon atoms which is substituted or unsubstituted by Ra;

[0119] Ra includes at least one of a halogen atom, a cyano group, an isocyanate group, a hydroxyl group, a carboxyl group, a sulfonic acid group, an ester group, an alkyl group having 2 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, and an oxaalkyl group having 2 to 10 carbon atoms.

[0120] Specifically, the electrolyte may also include additives, such as the first additive. The first additive is a negative electrode film-forming additive, which can form a stable SEI (Solid Electrolyte Interface, SEI) film on the surface of the negative electrode active material layer to reduce the direct contact between the negative electrode active material and the electrolyte. Introducing the compound represented by formula (I) as a solvent or as part of the solvent in the electrolyte, on the one hand, helps to improve the lithium ion conductivity of the electrolyte; on the other hand, the compound represented by formula (I) may produce gas by side reactions on the surface of the negative electrode active material layer during the charge and discharge process of the lithium secondary battery, which will consume the electrolyte in the lithium secondary battery and cause damage to the negative electrode active material and the structure of the negative electrode active material layer, affecting the cycle performance and safety performance of the lithium secondary battery.

[0121] Therefore, in this embodiment, by introducing the first additive into the electrolyte, the negative electrode active material layer can be effectively protected from direct contact with the electrolyte, the stability of the solid-liquid interface between the negative electrode active material layer and the electrolyte is improved, and the possibility of the compound represented by formula (I) generating gas on the surface of the negative electrode active material layer is reduced, thereby helping to improve the cycle performance of the lithium secondary battery while achieving high energy density and fast charging performance of the lithium secondary battery.

[0122] Optionally, the first additive includes at least one of the following compounds:

[0123]

[0124]

[0125] Optionally, the mass fraction W2 of the first additive in the electrolyte satisfies: 0.01%≤W2≤20%; optionally, 0.1%≤W2≤10%; optionally, 0.2%≤W2≤5%.

[0126] Specifically, W2 can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or its value is within the range obtained by combining any two of the above values.

[0127] Optionally, the mass fraction W2 of the first additive in the electrolyte, the mass fraction W1 of the compound of formula (I) in the electrolyte, and the lithium ion diffusion coefficient Ds of the positive electrode active material layer satisfy: 2×10 -22 cm 2 / s≤W2×W1×Ds≤1.6×10 -6 cm 2 / s; optionally, 2×10 -21 cm 2 / s≤W2×W1×Ds≤8×10 -7 cm 2 / s; optionally, 4×10 -21 cm 2 / s≤W2×W1×Ds≤4×10 -7 cm 2 / s.

[0128] Specifically, W2×W1×Ds can be 2×10 -22 cm 2 / s, 2×10 -21 cm 2 / s, 4×10 -21 cm 2 / s, 2×10 -20 cm 2 / s, 2×10 -19 cm 2 / s, 2×10 -18 cm 2 / s, 2×10 -17 cm 2 / s, 2×10 -16 cm 2 / s, 2×10 -15 cm 2 / s, 2×10 -14 cm 2 / s, 2×10 -13 cm 2 / s, 2×10-12 cm 2 / s, 2×10 -11 cm 2 / s, 2×10 -10 cm 2 / s, 2×10 -9 cm 2 / s, 2×10 - 8 cm 2 / s, 4×10 -7 cm 2 / s, 8×10 -7 cm 2 / s, 1.6×10 -6 cm 2 / s, or its value is within the range obtained by combining any two of the above values.

[0129] Optionally, the mass fraction W2 of the first additive in the electrolyte is positively correlated with the mass fraction W1 of the compound of formula (I) in the electrolyte.

[0130] Specifically, as the content of the compound represented by formula (I) in the electrolyte increases, the possibility of the compound represented by formula (I) producing gas on the surface of the negative electrode active material layer increases. Therefore, more first additive is required to form a film on the surface of the negative electrode active material layer to reduce the possibility of the compound represented by formula (I) producing gas due to a reduction reaction on the surface of the negative electrode active material layer.

[0131] Optionally, the electrolyte includes a second additive, the second additive includes M a+ [F w PO t ] b- 、M a+ [BF4] - a 、M a+ [FSO3] - a and at least one of the compounds of formula (III):

[0132]

[0133] Among them, M a+It includes at least one of lithium ion, sodium ion, potassium ion, rubidium ion, cesium ion, magnesium ion, calcium ion, barium ion, aluminum ion, iron ion, copper ion, nickel ion and organic cation, a, b and c all represent natural numbers; t represents an integer of 0-3, w represents an integer of 1-6; X includes at least one of halogen atoms, n represents an integer of 0-4; Y includes at least one of boron atom and phosphorus atom; R4 includes substituted or unsubstituted alkylene with 1-10 carbon atoms, substituted or unsubstituted halogenated alkylene with 1-10 carbon atoms, substituted or unsubstituted arylene with 6-20 carbon atoms, substituted or unsubstituted halogenated arylene with 6-20 carbon atoms, q represents an integer of 0-1, and m represents an integer of 1-3.

[0134] Specifically, the electrolyte may also include another negative electrode film-forming additive, namely the second additive. The second additive can also form a stable SEI film on the surface of the negative electrode active material layer, thereby isolating the electrolyte and the negative electrode active material layer, protecting the negative electrode active material, reducing the possibility of the electrolyte producing gas on the surface of the negative electrode active material layer, and further improving the cycle performance of the lithium secondary battery. In addition, the second additive has little effect on the impedance of the lithium secondary battery after film formation, reducing the possibility of lithium precipitation during the charge and discharge process of the lithium secondary battery due to excessive impedance, which helps to improve the charge and discharge performance of the battery.

[0135] It should be understood that the electrolyte may include only the first additive, only the second additive, or both the first additive and the second additive. When the electrolyte includes both the first additive and the second additive, the first additive and the second additive work together to form a SEI film on the surface of the negative electrode active material layer, and the film-forming effect is good while the impedance of the lithium secondary battery is less affected.

[0136] Optionally, the mass fraction W3 of the second additive in the electrolyte satisfies: 0.01%≤W3≤20%; optionally, 0.1%≤W3≤10%; optionally, 0.2%≤W3≤5%.

[0137] Specifically, W3 can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0..7%, 0.8%, 0.9%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or its value is within the range obtained by combining any two of the above values.

[0138] Optionally, the mass fraction W3 of the second additive in the electrolyte, the mass fraction W1 of the compound represented by formula (I) in the electrolyte, and the lithium ion diffusion coefficient Ds of the positive electrode active material layer satisfy: 2×10 -22 cm 2 / s≤W3×W1×Ds≤1.6×10 -6 cm 2 / s; optionally, 2×10 -21 cm 2 / s≤W3×W1×Ds≤8×10 -7 cm 2 / s; optionally, 4×10 -21 cm 2 / s≤W3×W1×Ds≤4×10 -7 cm 2 / s.

[0139] Specifically, W3×W1×Ds can be 2×10 -22 cm 2 / s, 2×10 -21 cm 2 / s, 4×10 -21 cm 2 / s, 2×10 -20 cm 2 / s, 2×10 -19 cm 2 / s, 2×10 -18 cm 2 / s, 2×10 -17 cm 2 / s, 2×10 -16 cm 2 / s, 2×10 -15 cm 2 / s, 2×10 -14 cm 2 / s, 2×10 -13 cm 2 / s, 2×10 -12 cm 2 / s, 2×10 -11 cm 2 / s, 2×10 -10 cm 2 / s, 2×10 -9 cm 2 / s, 2×10 - 8 cm 2 / s, 4×10 -7 cm 2 / s, 8×10 -7 cm 2 / s, 1.6×10 -6 cm 2 / s, or its value is within the range obtained by combining any two of the above values.

[0140] Optionally, the mass fraction W3 of the second additive in the electrolyte is positively correlated with the mass fraction W1 of the compound of formula (I) in the electrolyte.

[0141] Similar to the first additive, as the content of the compound represented by formula (I) in the electrolyte increases, the possibility of the compound represented by formula (I) producing gas on the surface of the negative electrode active material layer increases. Therefore, more negative electrode film-forming additives are needed to form a film on the surface of the negative electrode active material layer to reduce the possibility of the compound represented by formula (I) producing gas by undergoing a reduction reaction on the surface of the negative electrode active material layer.

[0142] Optionally, in M a+ [FSO3] - a In, M a+ Including Li + , Na + , K + , Rb + , Cs + ,Mg 2+ , Ca 2+ , Ba 2+ , Al 3+ , Fe 2+ , Cu 2 + , Fe 3+ , Ni 2+ , Ni 3+ At least one of .

[0143] Optionally, the electrolyte may further include additives that can improve certain properties of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high or low temperature performance of the battery, etc.

[0144] [Positive electrode]

[0145] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector.

[0146] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two facing surfaces of the positive electrode current collector.

[0147] Alternatively, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0148] Optionally, the positive electrode active material layer includes a first positive electrode active material and a second positive electrode active material.

[0149] Optionally, the first positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the first positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (LiFePO4, also referred to as LFP), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0150] Optionally, the average (volume) particle size Dv501 of the first positive electrode active material satisfies: 8 μm≤Dv501≤50 μm.

[0151] Specifically, Dv501 can be 8μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, or its value is within the range obtained by combining any two of the above values.

[0152] Alternatively, the second positive electrode active material may also be a positive electrode active material for a battery known in the art, as long as the average (volume) particle size of the second positive electrode active material is smaller than the average (volume) particle size of the selected first positive electrode active material. As an example, the second positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. Among them, examples of lithium transition metal oxides may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. These positive electrode active materials may be used alone or in combination of two or more.

[0153] Alternatively, the average (volume) particle size Dv502 of the second positive electrode active material satisfies: 0.02 μm≤Dv502≤8 μm.

[0154] Specifically, Dv502 can be 0.02μm, 0.04μm, 0.06μm, 0.08μm, 0.1μm, 0.5μm, 1μm, 2μm, 4μm, 6μm, 8μm, or its value is within the range obtained by combining any two of the above values.

[0155] Optionally, the mass fraction W4 of the second positive electrode active material in the positive electrode active material layer satisfies: 0%≤W4≤60%; further optionally, 20%≤W4≤40%.

[0156] Specifically, W4 can be 0%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 25%, 30%, 40%, 50%, 60%, or its numerical range is within the range obtained by combining any two of the above numerical values.

[0157] It should be understood that the first positive electrode active material and the second positive electrode active material can be active materials of the same type. For example, the first positive electrode active material is lithium iron phosphate with an average volume particle size of micrometers, and the second positive electrode active material is lithium iron phosphate with an average volume particle size of nanometers. The first positive electrode active material and the second positive electrode active material can also be active materials of different types. For example, the first positive electrode active material is lithium iron phosphate with an average particle size of micrometers, and the second positive electrode active material is lithium iron manganese phosphate with an average volume particle size of nanometers.

[0158] In this embodiment, by combining a first active material with a larger average (volume) particle size and a second active material with a smaller average (volume) particle size, it helps to increase the powder compaction density of the positive electrode active material layer, thereby increasing the energy density of the lithium secondary battery.

[0159] Optionally, the positive electrode active material layer further includes a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0160] Optionally, the positive electrode active material layer further includes a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0161] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet are respectively formed into positive electrode slurries. For example, the first positive electrode active material and / or the second positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry. Then, the positive electrode slurry is coated on at least one side of the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0162] [Negative electrode]

[0163] The negative electrode sheet generally includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.

[0164] As an example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two facing surfaces of the negative electrode current collector.

[0165] Alternatively, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0166] Optionally, the average (volume) particle size Dv503 of the negative electrode active material satisfies: 6 μm≤Dv503; optionally, 15 μm≤Dv503≤20 μm.

[0167] Specifically, Dv503 can be 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, or its value is within the range obtained by combining any two of the above values.

[0168] In this embodiment, by setting the average (volume) particle size of the negative electrode active material within a suitable range, it is helpful to increase the powder compaction density of the negative electrode active material layer. In addition, after the first additive and / or the second additive forms an SEI film on the surface of the negative electrode active material layer, the average (volume) particle size of the negative electrode active material on the surface of the negative electrode active material layer increases, and the specific surface area decreases, which helps to further reduce the contact between the negative electrode active material and the electrolyte, thereby reducing the probability of the electrolyte generating gas on the surface of the negative electrode active material layer, and helping to improve the cycle performance of the lithium secondary battery.

[0169] Optionally, the specific surface area of ​​the negative electrode active material satisfies: 0.5 m 2 / g≤BET≤2.0m 2 / g; optionally, 0.8m 2 / g≤BET≤1.5m 2 / g.

[0170] Specifically, BET can be 0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, 1.9m 2 / g, 2.0m 2 / g, or its value is within the range obtained by combining any two of the above values.

[0171] In the present embodiment, by setting the specific surface area of ​​the negative electrode active material within a suitable range, after the first additive and / or the second additive forms an SEI film on the surface of the negative electrode active material layer, the specific surface area of ​​the negative electrode active material on the surface of the negative electrode active material layer is further reduced, which helps reduce the probability of the electrolyte generating gas on the surface of the negative electrode active material layer, thereby further improving the cycle performance of the lithium secondary battery.

[0172] Optionally, the negative electrode active layer material layer further includes a binder. The binder can be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0173] Optionally, in one embodiment, the negative electrode film layer further includes a conductive agent, which can be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0174] Optionally, the negative electrode film layer further includes other additives, such as a thickener (such as sodium carboxymethyl cellulose (CMC-Na)) and the like.

[0175] In some embodiments, the negative electrode sheet can be prepared by the following method: the above components for preparing the negative electrode sheet are respectively formed into negative electrode slurry. For example, the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a negative electrode slurry. Then, the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0176] [Isolator]

[0177] Optionally, in one embodiment, the lithium secondary battery further includes a separator. The present application has no particular limitation on the type of separator, for example, any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0178] Optionally, in one embodiment, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0179] Optionally, in one embodiment, the positive electrode sheet, the negative electrode sheet and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0180] Optionally, in one embodiment, the lithium secondary battery includes an outer package, which can be used to encapsulate the electrode assembly and the electrolyte.

[0181] Optionally, in one embodiment, the outer packaging of the lithium secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and as the plastic, polypropylene, polybutylene terephthalate, and polybutylene succinate can be listed.

[0182] The present application has no particular limitation on the shape of the lithium secondary battery, which may be cylindrical, square or any other shape. Figure 1 The lithium secondary battery 10 is a square structure as an example.

[0183] In some embodiments, reference Figure 2 , the outer packaging may include a shell 22 and a cover plate 21. Among them, the shell 22 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a accommodating cavity. The shell 22 has an opening connected to the accommodating cavity, and the cover plate 21 can be covered on the opening to close the accommodating cavity. The positive electrode sheet, the negative electrode sheet and the separator can form an electrode assembly 23 through a winding process or a lamination process. The electrode assembly 23 is encapsulated in the above-mentioned accommodating cavity. The electrode assembly 23 is immersed in the electrolyte. The number of electrode assemblies 23 contained in the lithium secondary battery 10 can be one or more, and those skilled in the art can choose according to specific actual needs.

[0184] In some embodiments, the lithium secondary batteries 10 can be assembled into a battery module. The number of lithium secondary batteries 10 contained in the battery module can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0185] Figure 3 300 is an example of a battery module. Figure 3In the battery module 300, the plurality of lithium secondary batteries 10 may be arranged in sequence along the length direction of the battery module 300. Of course, they may also be arranged in any other manner. Further, the plurality of lithium secondary batteries 10 may be fixed by fasteners.

[0186] Optionally, in one embodiment, the battery module 300 may further include a housing having a receiving space, and the plurality of lithium secondary batteries 300 are received in the receiving space.

[0187] Optionally, in one embodiment, the battery modules 300 may also be assembled into a battery pack. The battery pack may contain one or more battery modules 300, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0188] Figure 4 and Figure 5 400 is an example of a battery pack. Figure 4 and Figure 5 The battery pack 400 may include a battery box and a plurality of battery modules 300 disposed in the battery box. The battery box includes an upper box body 401 and a lower box body 402. The upper box body 401 can cover the lower box body 402 and form a closed space for accommodating the battery modules 300. The plurality of battery modules 300 may be arranged in the battery box in any manner.

[0189] The lithium secondary battery 10 described in the present application may also be referred to as a lithium battery cell. Optionally, in one embodiment, a plurality of lithium battery cells are first integrated into a battery module, and then the battery module is installed in a battery box to form a battery pack. In other production and processing technologies, a plurality of lithium battery cells may also be directly installed in a battery box to form a battery pack, eliminating the intermediate state of the battery module, thereby reducing the quality of the battery pack and increasing the energy density of the battery pack.

[0190] Figure 6 A schematic diagram of an electrical device 600 provided by itself.

[0191] It should be understood that the power-consuming device 600 includes at least one of the lithium secondary battery 10, the battery module 300, or the battery pack 400 provided in the present application. The lithium secondary battery 10, the battery module 300, or the battery pack 400 can be used as a power source for the power-consuming device 600, or as an energy storage unit for the power-consuming device 600. The power-consuming device 600 may include mobile devices (such as mobile phones, laptop computers, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0192] As the electric device 600 , the lithium secondary battery 10 , the battery module 300 or the battery pack 400 may be selected according to the usage requirements.

[0193] As an example of an electrical device 600, Figure 6 As shown, the electric device 600 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the electric device 600's requirements for high power and high energy density of the lithium secondary battery 10, a battery pack 400 or a battery module 300 may be used.

[0194] As another example, the power-consuming device 600 may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be light and thin, and a lithium secondary battery 10 may be used as a power source.

[0195] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0196] Example 1

[0197] (1) Preparation of positive electrode sheet

[0198] Lithium iron phosphate with a Dv50 of 10 μm was selected as the positive electrode active material. The positive electrode active material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were dissolved in a solvent N-methylpyrrolidone (NMP) at a mass ratio of 90:5:5, and the mixture was stirred and mixed to obtain a slurry. The slurry was evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet. The lithium ion diffusion coefficient Ds of the positive electrode active material layer in the positive electrode sheet is 3.4×10 -12 cm 2 / s, the powder compaction density of the positive electrode is 2.5g / cm 3 .

[0199] (2) Preparation of negative electrode sheet

[0200] Natural graphite was selected as the negative electrode active material. The negative electrode active material, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) were dissolved in deionized water at a mass ratio of 90:4:4:2, and mixed evenly to obtain a negative electrode slurry. The slurry was evenly coated on the negative electrode current collector copper foil, and then dried, cold pressed, and cut to obtain a negative electrode sheet 1. The specific surface area of ​​the negative electrode active material in the negative electrode sheet 1 is 0.8 m 2 / g.

[0201] (3) Preparation of electrolyte

[0202] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed evenly in a volume ratio of 3:7, and then the compound represented by formula (I-II) was added to prepare a solvent, and the amount of the compound represented by formula (I-II) was adjusted so that its mass fraction W1 in the solvent was 60% and mixed evenly. Then, lithium hexafluorophosphate (LiPF6) was added as a solute and dissolved in the solvent so that the mass fraction of the solute in the electrolyte was 12.5%, and stirred evenly to obtain an electrolyte.

[0203] (4) Assembly of lithium secondary batteries

[0204] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, so that the isolation film is located between the positive electrode sheet and the negative electrode sheet and can isolate the positive electrode sheet from the negative electrode sheet; then the stacked components are wound to obtain an electrode assembly; the electrode assembly is set in a shell, and the electrolyte is injected after drying; after the formation, standing and other processes, the lithium secondary battery of Example 1 is obtained.

[0205] Example 2

[0206] Compared with the lithium secondary battery of Example 1, Example 2 selects lithium iron phosphate with a Dv50 of 10 μm as the positive electrode active material, and the lithium ion diffusion coefficient Ds of the positive electrode active material layer in the positive electrode sheet is 2.7×10 -9 cm 2 / s, and the mass fraction W1 of the compound represented by formula (I-II) in the solvent is 70%.

[0207] Example 3

[0208] Compared with the lithium secondary battery of Example 1, Example 3 selected lithium iron phosphate with a Dv50 of 10 μm as the positive electrode active material, and the lithium ion diffusion coefficient Ds of the positive electrode active material layer in the positive electrode sheet was 2.7×10 -9 cm 2 / s.

[0209] Example 4

[0210] Compared with Example 1, the solvent of Example 4 includes the compound represented by formula (IV), and the mass fraction W1 of the compound represented by formula (IV) in the solvent is 60%.

[0211] Example 5

[0212] Compared with Example 1, the solvent of Example 5 includes the compound represented by formula (I-VIII), and the mass fraction W1 of the compound represented by formula (I-VIII) in the solvent is 60%.

[0213] Example 6

[0214] Compared with Example 1, the electrolyte of Example 6 includes a first additive, and the first additive is a compound represented by formula (II-XXXII), and the mass fraction W2 of the compound represented by formula (II-XXXII) in the electrolyte is 1.0%.

[0215] Example 7

[0216] Compared with Example 1, the first additive in Example 7 is a compound represented by formula (II-XVII), and the mass fraction W2 of the compound represented by formula (II-XVII) in the electrolyte is 1.0%.

[0217] Example 8

[0218] Compared with Example 6, the first additive in Example 8 is a compound represented by formula (II-XXXII), and the mass fraction W2 of the compound represented by formula (II-XXXII) in the electrolyte is 1.5%.

[0219] Example 9

[0220] Compared with Example 1, the electrolyte of Example 9 includes a second additive, which is lithium difluorooxalatoborate LiDFOB, and the mass fraction W3 of LiDFOB in the electrolyte is 0.05%.

[0221] Example 10

[0222] Compared with Example 1, the second additive in Example 10 is lithium difluorobis(oxalate)phosphate LiBODFP, and the mass fraction W3 of LiBODFP in the electrolyte is 1.0%.

[0223] Embodiment 11

[0224] Compared with Example 2, the second additive in Example 11 is LiDFOB, the mass fraction W1 of the compound represented by formula (I-II) in the solvent is 70%, and the mass fraction W3 of LiDFOB in the electrolyte is 1.0%.

[0225] Example 12

[0226] Compared with Example 1, the first additive in Example 12 is the compound represented by formula (I-II), and the second additive is LiDFOB, the mass fraction W2 of the compound represented by formula (I-II) in the electrolyte is 0.5%, and the mass fraction W3 of LiDFOB in the electrolyte is 0.5%.

[0227] Embodiment 13

[0228] Compared with Example 1, Example 13 selects lithium iron phosphate with a Dv50 of 10 μm as the first positive electrode active material and lithium iron phosphate with a Dv50 of 2 μm as the second positive electrode active material, and dissolves the first positive electrode active material, the second positive electrode active material, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) in a solvent N-methylpyrrolidone (NMP) at a mass ratio of 63:27:5:5, and obtains a slurry after being fully stirred and mixed. The slurry is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet. Among them, the mass fraction W4 of the second positive electrode active material in the positive electrode active material layer is 30%, and the powder compaction density of the positive electrode sheet is 2.6 g / cm 3 .

[0229] Embodiment 14

[0230] Compared with Example 13, in Example 14, the mass fraction W4 of the second positive electrode active material in the positive electrode active material layer is 10%, and the powder compaction density of the positive electrode sheet is 2.55 g / cm 3 .

[0231] Embodiment 15

[0232] Compared with Example 1, Example 15 selects a specific surface area of ​​1.5m 2 / g of artificial graphite as the negative electrode active material.

[0233] Example 16

[0234] Compared with Example 1, the solvent in Example 16 includes both the compound represented by formula (I-II) and the compound represented by formula (II), wherein the mass ratio of the compound represented by formula (I-II) to the compound represented by formula (II) is 30:30.

[0235] Comparative Example 1

[0236] Compared with Example 1, Comparative Example 1 selects dimethyl carbonate (DMC) as the solvent.

[0237] Comparative Example 2

[0238] Compared with Example 1, lithium iron phosphate is selected as the positive electrode active material, and the lithium ion diffusion coefficient Ds of the positive electrode active material layer is 7.3×10-20 cm 2 / s, the mass fraction W1 of the compound represented by formula (I-II) in the solvent is 60%.

[0239] The product parameters of the embodiments and comparative examples are shown in Table 1.

[0240] Table 1: Product parameters of different embodiments and comparative examples

[0241]

[0242]

[0243] In Table 1, the positive electrode Ds is the lithium ion diffusion coefficient Ds of the positive electrode active material layer of the positive electrode plate, the positive electrode powder compaction density is the powder compaction density of the positive electrode plate, the negative electrode BET is the BET of the negative electrode active material, the compound is the compound included in the solvent, W1 is the mass fraction of the compound in the solvent, W2 is the mass fraction of the first additive in the electrolyte, and W3 is the mass fraction of the second additive in the electrolyte.

[0244] It should be understood that the difference in the lithium ion diffusion coefficient Ds is usually directly reflected in the order of magnitude. Therefore, the lithium ion diffusion coefficient Ds of the positive electrode active material layer in the above table shows the order of magnitude of the lithium ion diffusion coefficient. For example, in Example 1, Ds is specifically 3.4×10 -12 , Table 1 shows only 10 -12 .

[0245] The battery performance test results of the above-mentioned Examples 1-16 and Comparative Examples 1-2 are detailed in Table 2.

[0246] Table 2: Battery performance test results of different embodiments and comparative examples

[0247]

[0248]

[0249] By comparing Example 1, Example 4, Example 5 and Example 16 with Comparative Example 1, it can be seen that by introducing the compounds represented by formula (I-II), formula (IV), formula (I-VIII) and formula (II) into the solvent, the problem of mismatch between the lithium ion diffusion capacity of the positive electrode active material layer and the electrolyte in the lithium secondary battery is improved, so that the discharge capacity, fast charging capability and cycle life of the lithium secondary batteries in Example 1, Example 4, Example 5 and Example 16 are better than those in Comparative Example 1 in which the solvent does not contain the compound represented by formula (I), and the lithium secondary batteries in Example 1, Example 4, Example 5 and Example 16 also have a lower volume expansion rate and significantly improved safety performance.

[0250] By comparing Example 1 with Comparative Example 2, it can be seen that when the compound represented by formula (I) is introduced into the solvent, the product of the mass fraction W1 of the compound in the solvent in Example 1 and the lithium ion diffusion coefficient Ds of the positive electrode active material layer is W1×Ds=6×10 -11 cm 2 / s, at 2×10 -18 cm 2 / s-8×10 -6 cm 2 / s, further, in the range of 3×10 -14 cm 2 / s-7×10 -10 cm 2 / s. In Comparative Example 2, W1×Ds is 9×10 -19 cm 2 / s, which is beyond the above range, the discharge capacity, fast charging capability and cycle life of Comparative Example 2 are worse than those of Example 1. Therefore, it is shown that by controlling Ds×W1 within a suitable range, the problem of mismatch between the lithium ion diffusion capacity of the positive electrode active material layer and the electrolyte in the lithium secondary battery can be improved, thereby helping to improve the discharge capacity, fast charging capability, cycle life and safety performance of the lithium secondary battery.

[0251] By comparing Example 3 with Example 2, it can be seen that when Ds increases, Example 2 increases W1 at the same time, while Example 3 does not increase W1. The performance of the lithium secondary battery of Example 3 is slightly inferior to that of Example 2. Therefore, by controlling Ds to be positively correlated with W1, it is helpful to improve the discharge capacity, fast charging capability, cycle life and safety performance of the lithium secondary battery.

[0252] By comparing Example 6 and Example 7 with Example 1, it can be seen that Example 6 and Example 7 respectively introduce compounds represented by Formula (II-XXXII) and Formula (II-XVII) into the electrolyte as the first additive, and the cycle performance of the lithium secondary batteries in Example 6 and Example 7 is significantly better than that of the lithium secondary battery in Example 1 and the volume expansion rate is smaller than that of the lithium secondary battery in Example 1. Therefore, it is shown that the introduction of the first additive into the electrolyte can effectively reduce the side reaction of the electrolyte on the surface of the negative electrode active material layer while improving the lithium ion conductivity of the electrolyte, thereby improving the cycle performance and safety performance of the lithium secondary battery.

[0253] By comparing Example 8 with Example 6, it can be seen that when W1 increases, W2 increases in Example 8. The volume expansion rate of the lithium secondary battery in Example 8 is lower than that of the lithium secondary battery in Example 6. Therefore, by controlling W2 to be positively correlated with W1, it is helpful to further improve the safety performance of the lithium secondary battery.

[0254] By comparing Example 9 and Example 1 with Example 1, it can be seen that Example 9 and Example 10 respectively introduce LiDFOB and LiBODFP as the second additive into the electrolyte, and the cycle performance of the lithium secondary battery in Example 9 and Example 10 is significantly better than that of the lithium secondary battery in Example 1, and the volume expansion rate is smaller than that of the lithium secondary battery in Example 1. Therefore, it is explained that the introduction of the second additive into the electrolyte can effectively reduce the side reaction of the electrolyte on the surface of the negative electrode active material layer while improving the lithium ion conductivity of the electrolyte, thereby improving the cycle performance and safety performance of the lithium secondary battery.

[0255] By comparing Example 11 with Example 9, it can be seen that when W1 increases, W3 increases in Example 11. The volume expansion rate of the lithium secondary battery in Example 11 is lower than the volume expansion rate of the lithium secondary battery in Example 9. Therefore, by controlling W3 to be positively correlated with W1, it is helpful to further improve the safety performance of the lithium secondary battery.

[0256] By comparing Example 12 with Example 6 and Example 9, it can be seen that Example 12 introduces the first additive and the second additive into the electrolyte at the same time, and the cycle performance of the lithium secondary battery in Example 12 is significantly improved, and the volume expansion rate is significantly reduced. Therefore, it can be seen that the first additive and the second additive have a synergistic effect in the electrolyte, which can further improve the cycle performance and safety performance of the lithium secondary battery.

[0257] By comparing Example 13 with Example 1, it can be seen that the second positive electrode active material with a smaller Dv502 is introduced into the positive electrode active material layer of Example 13, which increases the powder compaction density of the positive electrode plate. Compared with Example 1, the discharge capacity of the lithium secondary battery in Example 13 is improved. Therefore, it is shown that by matching positive electrode active materials with different particle sizes, it is helpful to increase the powder compaction density of the positive electrode active material layer, thereby helping to improve the discharge capacity of the lithium secondary battery.

[0258] By comparing Example 14 with Example 13, it can be seen that in Example 14, the mass fraction W4 of the second positive electrode active material with a smaller Dv502 in the positive electrode active material layer is reduced, the powder compaction density of the positive electrode sheet is reduced, and the discharge capacity of the lithium secondary battery is also reduced. Therefore, it is shown that by controlling the mass fraction W4 of the second positive electrode active material with a smaller average volume particle size in the positive electrode active material layer, the powder compaction density of the positive electrode sheet can be affected, thereby affecting the energy density of the lithium secondary battery, and further affecting the discharge capacity of the lithium secondary battery.

[0259] It should be understood that the average volume particle size of a material and its specific surface area are interrelated physical quantities. The larger the average volume particle size of a material, the smaller its BET is generally; and the smaller the average volume particle size of a material, the larger its BET is generally.

[0260] By comparing Example 15 with Example 1, it can be seen that Example 15 uses a negative electrode active material with a smaller Dv503 and a larger BET, and the discharge capacity, fast charging performance and cycle performance of the lithium secondary battery in Example 1 are better than those of the lithium secondary battery in Example 15, and the volume expansion rate of the lithium secondary battery in Example 1 is smaller. Therefore, it can be seen that the average volume particle size or specific surface area of ​​the negative electrode active material has an impact on the performance of the lithium secondary battery, and the negative electrode active material with a larger Dv503 and a smaller BET has a smaller contact area with the electrolyte, which can reduce the probability of the electrolyte having side reactions on the surface of the negative electrode active material layer, thereby helping to improve the various performances of the lithium secondary battery.

[0261] Next, the testing methods of the physical parameters and performance parameters mentioned in the embodiments of the present application are briefly introduced.

[0262] 1. Test method for lithium ion diffusion coefficient

[0263] The diffusion coefficient of lithium ions can be tested by conventional methods in the art, such as cyclic voltammetry (CV method), electrochemical impedance spectroscopy (EIS method), constant potential intermittent titration (PITT method), constant current intermittent titration (GITT method), and calculated according to Fick's first law and Fick's second law.

[0264] Taking the electrochemical impedance method as an example, the steps for testing the lithium ion diffusion coefficient of the positive electrode active material layer are as follows: the positive electrode active material, acetylene black conductive agent, and polyvinylidene fluoride binder prepared in the embodiment of the present application and the comparative example are mixed uniformly in a mass ratio of 85:10:5, N-methylpyrrolidone is added to prepare a slurry, which is coated on an aluminum sheet, and vacuum dried at 60°C for 5 hours to prepare a positive electrode sheet sample, and the prepared sample is used as the positive electrode, the metal lithium sheet is used as the negative electrode, and Celgard2400 polypropylene microporous The membrane is a diaphragm, and 1 mol / L LiPF6, ethylene carbonate (EC) and diethyl carbonate (DEC) solution are mixed in a volume ratio of 1:1 as an electrolyte. They are assembled into CR2032 button-type half-cell samples in a high argon environment. The battery's AC impedance (EIS) test is performed using Shanghai Chenhua CHI660b electrochemical workstation, with an amplitude of 5mV and a frequency range of 10mHz-100KHz. The electrochemical impedance spectrum (Nyquist spectrum) of the battery sample can be obtained. By curve fitting the electrochemical impedance spectrum, the Warburg constant of the battery sample can be calculated according to Fick's second law and the Nernst equation. Combined with the Butler-Volmer equation, the lithium ion diffusion coefficient of the positive electrode active material layer can be calculated by the following formula.

[0265]

[0266] Where σ is the Warburg constant, F is the Faraday constant, and S is the surface area of ​​the positive electrode (unit: cm 2 ), V m is the molar volume of the positive electrode active material (unit: cm 2 / mol), dE / dx is the slope of the positive electrode coulometric titration line. The coulometric titration line can be obtained by testing by methods known in the art. For example, the coulometric titration line can be obtained by testing with a constant current electrolysis device.

[0267] 2. Test method for average (volume) particle size

[0268] In the present application, the average volume particle size Dv50 of the active material has a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a laser powder analyzer (e.g., Master Size 3000) with reference to the particle size distribution laser diffraction method of GB / T 19077-2016.

[0269] 3.BET’s testing method

[0270] The test method refers to the standard GB / T19587-2004 "Determination of specific surface area of ​​solid substances by gas adsorption BET method".

[0271] Take 8g-15g of the sample to be tested and put it into the sample tube, and record the initial mass of the sample to be tested. Load the weighed sample to be tested into the equipment NOVA2000e. Then start degassing, and heat the sample to be tested to 200℃ and keep it for 2h. Then record the mass of the sample to be tested after degassing. Then reload the degassed sample to be tested into the equipment, pour in liquid nitrogen for BET test. Set the nitrogen pressure to 0.08MPa-0.12MPa and the heating temperature to 40℃-350℃. After the test, read the specific surface area from the test results.

[0272] 4. Test method for compacted powder density

[0273] The area is 1540.25mm 2 The circular positive electrode sheet of size is taken as the basic unit, where the total weight of the positive electrode sheet coated with positive electrode active material on both sides is A (g), the weight of the positive electrode collector is B (g), the thickness of the positive electrode collector is T (mm), and the thickness of the aluminum foil is U (mm). The powder compacted density (PD) of the positive electrode sheet can be calculated using the following formula.

[0274]

[0275] 5. Battery capacity test

[0276] At 25°C, the lithium secondary battery was charged at a constant current of 0.5C to 3.65V, then charged at a constant voltage of 3.65V to a current less than 0.05C, and then discharged at a constant current of 0.5C to 2.5V to obtain a discharge capacity at 0.5C.

[0277] 6. Fast charging time test

[0278] Charge at 0.33C to 10% state of charge (SOC) at 25°C, charge for s minutes according to the given fast-charging process, charge to 80% SOC, let stand for 30 minutes, then discharge at 1C, then let stand for 30 minutes, after 20 cycles, disassemble the lithium secondary battery after full charge, observe whether lithium is deposited at the negative electrode, if there is no lithium deposition, it indicates that the lithium secondary battery has a fast charging capability of s minutes.

[0279] 7. Cycle performance test

[0280] At 60°C, the lithium secondary battery is charged to 3.65V at 0.5C constant current, then charged to less than 0.05C at 3.65V constant voltage, and then discharged to 2.5V at 0.5C constant current. This is a charge and discharge process. Repeat the charge and discharge process and calculate the number of cycles after the lithium secondary battery decays to 80%.

[0281] 8. Volume expansion rate test

[0282] At 25°C, the prepared lithium secondary batteries were first charged to 3.65V at a constant current of 0.33C, and then further charged to a current of 0.05C at a constant voltage of 3.65V, and then discharged to 2.5V at a constant current of 0.33C. The discharge capacity this time is the discharge capacity of the lithium secondary battery before high-temperature storage; then the lithium secondary battery was charged to 3.65V at a constant current of 0.33C, and charged to a current of 0.05C at a constant voltage of 3.65V to fully charge the lithium secondary battery. The volume of the battery was tested by the drainage method. After that, the lithium secondary battery was stored at 60°C for 60 days. After the storage was completed, the lithium secondary battery was placed in an environment of 25°C, and the volume of the battery was tested by the drainage method. Battery volume expansion rate = (volume after storage / volume before storage-1)%.

[0283] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A lithium secondary battery, wherein: The lithium secondary battery comprises: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, wherein the lithium ion diffusion coefficient Ds of the positive electrode active material layer is within 10 -16 cm 2 / s-10 -5 cm 2 / s range; An electrolyte, the electrolyte comprising a solvent, the solvent comprising at least one of the compounds of the following formula (I), wherein the mass fraction W1 of the compound of the formula (I) in the solvent is in the range of 20%-80%; Wherein, R1 and R2 independently include at least one of an alkyl group having 1 to 3 carbon atoms and a halogenated alkyl group having 1 to 3 carbon atoms.

2. The lithium secondary battery according to claim 1, wherein R1 and R2 independently include at least one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl, and fluoropropyl.

3. The lithium secondary battery according to claim 1 or 2, wherein: 10 -14 cm 2 / s≤Ds≤10 -9 cm 2 / s。 4. The lithium secondary battery according to any one of claims 1 to 3, wherein: 30%≤W1≤70%。 5. The lithium secondary battery according to any one of claims 1 to 4, wherein: The compound of formula (I) comprises at least one of the following compounds: Optionally, the compound of formula (I) includes at least one of a compound of formula (II), a compound of formula (I-II), a compound of formula (IV), and a compound of formula (I-VIII); Alternatively, the compound of formula (I) includes the compound of formula (II) and the compound of formula (I-II).

6. The lithium secondary battery according to any one of claims 1 to 5, wherein: The electrolyte includes a first additive, the first additive including at least one of the compounds of formula (II): Wherein, R3 includes at least one of an alkylene group having 2-10 carbon atoms which is substituted or unsubstituted by Ra, a heteroalkylene group having 2-10 carbon atoms which is substituted or unsubstituted by Ra, an arylene group having 6-18 carbon atoms which is substituted or unsubstituted by Ra, a heteroarylene group having 6-18 carbon atoms which is substituted or unsubstituted by Ra, an alicyclic group having 3-18 carbon atoms which is substituted or unsubstituted by Ra, and a heteroalicyclic group having 3-18 carbon atoms which is substituted or unsubstituted by Ra; Ra includes at least one of a halogen atom, a cyano group, an isocyanate group, a hydroxyl group, a carboxyl group, a sulfonic acid group, an ester group, an alkyl group having 2 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, and an oxaalkyl group having 2 to 10 carbon atoms.

7. The lithium secondary battery according to claim 6, wherein: The mass fraction W2 of the first additive in the electrolyte satisfies: 0.01%≤W2≤20%; optionally, 0.1%≤W2≤10%; optionally, 0.2%≤W2≤5%; optionally, 0.50%≤W2≤1.50%.

8. The lithium secondary battery according to claim 6 or 7, wherein: The first additive comprises at least one of the following compounds: Optionally, the first additive comprises at least one of Formulae II-XXXII and II-XVII.

9. The lithium secondary battery according to any one of claims 1 to 8, wherein: The electrolyte includes a second additive, wherein the second additive includes M a+ [F w PO t ] b- 、M a+ [BF4] - a 、M a+ [FSO3] - a and at least one of the compounds of formula (III): Among them, M a+ Including at least one of lithium ion, sodium ion, potassium ion, rubidium ion, cesium ion, magnesium ion, calcium ion, barium ion, aluminum ion, iron ion, copper ion, nickel ion, and organic cation, and a, b, and c all represent natural numbers; t represents an integer from 0 to 3, and w represents an integer from 1 to 6; X includes at least one halogen atom, and n represents an integer of 0 to 4; Y includes at least one of a boron atom and a phosphorus atom; R4 includes substituted or unsubstituted alkylene having 1 to 10 carbon atoms, substituted or unsubstituted halogenated alkylene having 1 to 10 carbon atoms, substituted or unsubstituted arylene having 6 to 20 carbon atoms, substituted or unsubstituted halogenated arylene having 6 to 20 carbon atoms, q represents an integer of 0 to 1, m represents an integer of 1 to 3, Optionally, the compound of formula (III) includes at least one of lithium difluorooxalatoborate LiDFOB and lithium difluorooxalatophosphate LiBODFP.

10. The lithium secondary battery according to claim 9, wherein: The mass fraction W3 of the second additive in the electrolyte satisfies: 0.01%≤W3≤20%; optionally, 0.1%≤W3≤10%; optionally, 0.2%≤W3≤5%; optionally, 0.05%≤W3≤1.0%.

11. The lithium secondary battery according to claim 9 or 10, wherein: In M a+ [FSO3] - a In, M a+ Including Li + , Na + , K + , Rb + , Cs + ,Mg 2+ , Ca 2+ , Ba 2+ , Al 3+ , Fe 2+ , Cu 2+ , Fe 3+ , Ni 2+ , Ni 3+ At least one of .

12. The lithium secondary battery according to any one of claims 1 to 11, wherein: The solvent of the electrolyte further comprises at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone; Optionally, the solvent further comprises ethylene carbonate and ethyl methyl carbonate.

13. The lithium secondary battery according to any one of claims 1 to 12, wherein: The electrolyte also includes a solute, and the solute includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate and lithium tetrafluorooxalatophosphate.

14. The lithium secondary battery according to any one of claims 1 to 13, wherein: The positive electrode active material layer includes a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material and the second positive electrode active material are the same type of material or different types of materials. The average particle size Dv501 of the first positive electrode active material satisfies: 8 μm ≤ Dv501 ≤ 50 μm, The average particle size Dv502 of the second positive electrode active material satisfies: 0.02 μm≤Dv502≤8 μm; Optionally, the first positive electrode active material includes one or more of a lithium transition metal oxide and an olivine-structured lithium-containing phosphate, and optionally includes lithium nickel cobalt manganese oxide and / or lithium iron phosphate. The second positive electrode active material includes one or more of lithium transition metal oxides and lithium phosphates with an olivine structure, and optionally includes one or more of lithium nickel cobalt manganese oxide, lithium iron phosphate, and lithium manganese iron phosphate; Further optionally, the first positive electrode active material is lithium iron phosphate with an average volume particle size of micrometers, and the second positive electrode active material is lithium iron phosphate with an average volume particle size of nanometers; Further optionally, the first positive electrode active material is lithium iron phosphate with an average particle size of micrometer level, and the second positive electrode active material is lithium manganese iron phosphate with an average volume particle size of nanometer level.

15. The lithium secondary battery according to claim 14, wherein: The mass fraction W4 of the second positive electrode active material in the positive electrode active material layer satisfies: 0%≤W4≤60%; optionally, 20%≤W4≤40%.

16. The lithium secondary battery according to any one of claims 1 to 15, wherein: The lithium secondary battery comprises: A negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material; The average particle size Dv503 of the negative electrode active material satisfies: 6μm≤Dv503; optionally, 8μm≤Dv503≤20μm; further optionally, 8μm≤Dv503≤18μm; further optionally, 15μm≤Dv503≤20μm.

17. The lithium secondary battery according to claim 16, wherein: The specific surface area of ​​the negative electrode active material meets the following requirements: 0.5 m 2 / g≤BET≤2.0m 2 / g; optionally, 0.8m 2 / g≤BET≤1.5m 2 / g.

18. The lithium secondary battery according to claim 16 or 17, wherein: The lithium secondary battery includes an electrode assembly contained in an outer package and the electrolyte, the electrode assembly includes a separator, the positive electrode sheet and the negative electrode sheet, and the separator, the positive electrode sheet and the negative electrode sheet are formed into the electrode assembly through a winding process or a lamination process.

19. An electrical device, wherein: The electrical device comprises a lithium secondary battery as claimed in any one of claims 1 to 18.

Citation Information

Patent Citations

  • Electrolyte and lithium ion battery containing same

    CN101740822A

  • Low-temperature electrolyte of lithium iron phosphate power battery and preparation method thereof

    CN101841061A

  • Low-temperature rate lithium ion battery electrolyte

    CN103078136A

  • Low-temperature type lithium ion battery electrolyte and lithium ion battery

    CN103107364A

  • Lithium ion battery electrolyte and lithium ion battery containing same

    CN103855426A