Single-layer graphene conductive paste, preparation method and application thereof, and conductivity evaluation method

By controlling the water content and thermal reduction temperature of graphene oxide, oligolayer graphene powder was prepared, solving the problem of poor conductivity of multilayer graphene. This enabled the preparation of highly conductive graphene conductive slurry, improving the conductivity and fast charge/discharge performance of lithium-ion batteries.

CN119018885AInactive Publication Date: 2024-11-26THE SIXTH ELEMENT CHANGZHOU MATERIALS TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411130736.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare highly conductive graphene conductive agents, especially in lithium-ion batteries. Multilayer graphene leads to poor conductivity, and the presence of dispersants in traditional methods affects battery performance.

Method used

Oligolayer graphene was prepared by redox method. By controlling the water content and thermal reduction temperature of graphene oxide, oligolayer graphene powder was prepared and dispersed in solvent, reducing or eliminating the use of dispersant to form a highly conductive graphene conductive slurry.

Benefits of technology

It significantly improves the conductivity of graphene, reduces the resistivity of the electrode, and enhances the fast charge/discharge performance and high voltage resistance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018885A_ABST
    Figure CN119018885A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a few-layer graphene conductive paste, which comprises the following steps: few-layer graphene is dispersed in a solvent, the number of layers of the few-layer graphene is less than or equal to 4, and the solid content of the few-layer graphene in the few-layer graphene conductive paste is 0.5 wt%-1.5 wt%. The invention also provides the few-layer graphene conductive paste and application thereof, and a conductivity evaluation method of the graphene conductive agent. When the few-layer rGO is used as a conductive agent to be applied to the lithium ion battery, the conductivity and the threshold value have obvious advantages; when the graphene conductive paste is prepared from the few-layer graphene, graphene sheets can be stabilized by adding less or even not adding a dispersing agent, so that the graphene conductive paste can bear large current in the use process of a downstream lithium ion battery without adding the dispersing agent, and the rapid charge and discharge performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material synthesis and application, in particular to the preparation and application of graphene conductive slurry. Background Art

[0002] (1) Introduction to graphene

[0003] Graphene is composed of carbon atoms in the form of sp 2 The hybrid orbital is a planar two-dimensional material with a hexagonal honeycomb lattice, which has the characteristics of high electrical and thermal conductivity. Theoretically, the electrical conductivity of graphene can reach 10^8S / m, and its carrier mobility is as high as 15000cm 2 ·V -1 s -1 , which has the highest known mobility and can reach more than 10 times that of commercial silicon wafers (see literature: Ma Wenshi, Zhou Junwen, Cheng Shunxi, Preparation and Characterization of Graphene, Journal of Chemical Engineering of Universities, 2010, 24(4):719-722).

[0004] Graphene preparation method:

[0005] There are many methods for preparing graphene, including mechanical exfoliation, liquid phase exfoliation, chemical oxidation, crystal epitaxial growth, chemical vapor deposition, organic synthesis and carbon nanotube exfoliation.

[0006] Mechanical stripping is to overcome the interaction between sheets in graphite by mechanical methods (see literature: NOVOSELOV KS, GEIM AK, MOROZOV SV, et al. Electric field effect in atomically thin carbon films. Science, 2004, 306 (5696): 666-669), use photoresist to separate graphite, and successfully obtain single-layer graphene. Although this method can produce a lower number of graphene layers than the general mechanical stripping method, it is still difficult to accurately control the purity of graphene and the yield is extremely low, making it difficult to achieve large-scale preparation of graphene. The currently commercialized mechanical exfoliation method for preparing graphene slurry generally uses a sand mill, homogenizer and other means to break up and exfoliate the graphite. The thickness of the obtained graphene material is generally ≥10 layers, which is a multi-layer graphene material. It is impossible to prepare graphene with few or few layers. In addition, a small amount of dispersant needs to be added to stabilize the graphene while these devices are breaking and exfoliating. The dispersant will have adverse effects during the use of downstream lithium-ion batteries, and higher-end applications of graphene materials cannot be achieved.

[0007] Liquid phase exfoliation is to use ultrasound, heating and other means to exfoliate graphite to prepare a single or multilayer graphene solution (see literature: HERNANDEZ Y, NICOLOSI V, LOTYAM, et al., High-yield production of graphene by liquid-phase exfoliation of graphite. Nature Nanotech, 2008, 3 (9): 563-568). In the process of preparing graphene by this method, a lot of dispersants need to be added. The dispersant has the function of stabilizing the graphene sheet in the graphene solution, but when the downstream lithium-ion battery is prepared, the dispersant on the surface of the graphene present as a conductive agent cannot be separated out, so that when the positive and negative electrodes are assembled, there will be dispersants in the pole piece. The presence of these dispersants will reduce the high-voltage resistance of the battery after the pole piece is assembled into a battery. The fundamental reason is that the dispersant is often some polymer or small molecule materials, which will decompose and produce gas under high voltage and high current to produce adverse reactions such as cycle swelling, so it is difficult to be suitable for charging and discharging under high current. Under the fast-paced rhythm of life, this type of graphene conductive agent is difficult to meet the fast charging demand.

[0008] Chemical vapor deposition (CVD) (see literature: BERGER C, SONG ZM, LI XB, et al., Electronic confinement and coherence in patterned epitaxial graphene. Science, 2006, 312 (5777): 1191-1196), CVD is to decompose carbon-containing chemicals (such as methane, etc.) at high temperature, and the carbon atoms obtained by cracking are deposited on the substrate, and the carbon atoms are combined with carbon atoms to form graphene, which can prepare a few layers or even a single layer of graphene materials. This method is used to prepare transparent graphene films and can be applied to electronic touch screens, sensors, transistors, etc. Its most important barrier is how to peel off graphene from the substrate without damage or pollution, which is still a problem of concern. In addition, the CVD method is not suitable for the preparation of graphene powder materials, and the prepared graphene materials cannot be used as conductive agents in lithium-ion batteries.

[0009] Epitaxial growth, organic synthesis, and carbon tube exfoliation can all produce single-layer and few-layer graphene materials, but their cost and large-scale production are still constraints.

[0010] The redox method uses a chemical method to first oxidize and exfoliate graphene to obtain high-monolayer graphene oxide (GO), and then reduce GO to obtain graphene (strictly speaking, reduced graphene oxide rGO).

[0011] (2) Conductive agent

[0012] Conductive agent is an indispensable part of battery manufacturing. Its function is to improve the conductivity of the electrode, reduce the internal resistance, and improve the charge and discharge performance of the battery. Conductive agent is a key auxiliary material for lithium-ion batteries. It is a reagent to ensure that the electrode has good charge and discharge performance. It collects microcurrents between active substances and between active substances and current collectors, and then collects the microcurrents on current collectors such as aluminum foil and copper foil to form a large current, which is finally transported to electrical appliances. The addition of conductive agent can reduce the contact resistance of the electrode in this way, accelerate the electron movement rate and the migration rate of lithium ions in the electrode material, and improve the electronic conductivity, thereby improving the charge and discharge efficiency of the electrode. Therefore, conductive agent plays an important role in improving conductivity, capacity utilization, rate performance, and cycle performance. Since most of the active substances of positive electrode materials have poor conductivity and large internal resistance, the conductive agent forms a conductive network to improve the conductivity between the active substances of the electrode material and the current collector.

[0013] There are three types of battery conductive agents: carbon black, carbon tubes, graphite, carbon fiber, and graphene. According to the composition of the conductive agent particles and the morphology and structure of the original particles, common conductive agents can be roughly divided into three categories: granular conductive agents, fibrous conductive agents, and lamellar conductive agents. Granular conductive agents mainly include conductive graphite (graphite, mainly some KS series conductive graphite), carbon black (carbon black, CB) and metal powder. Among them, CB can be further subdivided into Super-P (SP), acetylene black (acetylene black, AB) and Ketjen black (Ketjen black, KB). Fibrous conductive agents mainly include metal fibers, vapor grown carbon fiber (vapor grown carbon fiber, VGCF) and carbon nanotubes (carbonnanotubes, CNTs). Lamellar conductive agents mainly include SFG series and most KS series conductive graphites, as well as graphene.

[0014] (3) Electrode resistivity test

[0015] In order to better evaluate the conductive effect of the conductive agent in lithium-ion batteries, the method of testing the resistivity of the pole piece is generally used to evaluate the effect of conductivity. In short, the method is to disperse the graphene powder in water or solvents such as NMP (N-methylpyrrolidone) to form a uniform slurry, and then mix the graphene slurry with the main material (LFP (lithium iron phosphate), NCM (ternary lithium), etc.), and the binder (PTFE (polytetrafluoroethylene), etc.) evenly, and then apply the slurry mixture on the collector (aluminum foil, copper foil, etc.), and obtain the pole piece after drying. The probe film impedance test principle is used to test the resistivity of the slurry film. The conductive effect of the conductive agent when used downstream can be known by the size of the pole piece resistivity. The smaller the pole piece resistivity, the better the conductivity of the graphene material.

[0016] The contents of the background technology section are merely the technologies known to the inventors and do not necessarily represent the prior art in the field. Summary of the invention

[0017] In order to achieve the above-mentioned object, the present invention provides a method for preparing a few-layer graphene conductive paste, comprising the following steps: dispersing the few-layer graphene in a solvent, wherein the number of the few-layer graphene layers is ≤4, and the solid content of the few-layer graphene in the few-layer graphene conductive paste is 0.5wt%-1.5wt%.

[0018] Furthermore, the solid content of the few-layer graphene is 1wt%-1.3wt%;

[0019] And / or, the solvent is NMP or water.

[0020] Furthermore, the dispersion method is preferably homogeneous dispersion, microfluidic dispersion, or sand mill dispersion.

[0021] Furthermore, the dispersion method is to disperse the slurry containing the few-layer graphene by sand grinding, wherein the zirconium beads are 1-3 mm, the grinding power is 1-3 kw, and the grinding time is 1-3 h.

[0022] Furthermore, the dispersion method is to stir the slurry containing the few-layer graphene at a stirring speed of 1000-5000 rpm for 20-40 minutes, and then put the stirred slurry into a homogenizer and homogenize it 2-4 times at a pressure of 800-1000 MPa.

[0023] Furthermore, the method for preparing the few-layer graphene comprises the following steps:

[0024] (1) quantitatively humidifying the graphene oxide powder, wherein the graphene oxide powder satisfies the following conditions:

[0025] The graphene oxide powder is prepared into a 20-100 ppm solution, and then oscillated on an oscillator with a frequency of 10-15 Hz for 10-40 minutes. The oscillated solution is dropped on a silicon dioxide wafer and dried, and then observed under an optical microscope. The observation result shows that the surface of the silicon wafer appears blue, and no other colors exist.

[0026] And / or the moisture content of the humidified graphene oxide powder is 6wt%-25wt%; preferably, the moisture content of the humidified graphene oxide powder is 10wt%-18wt%;

[0027] (2) heat treating the humidified graphene oxide powder under an inert atmosphere, so that the graphene oxide releases gas during the reduction process to cause the graphene oxide to peel off;

[0028] (3) The product of step (2) is subjected to thermal repair treatment under an inert atmosphere to obtain a few-layer graphene powder.

[0029] Furthermore, the production process of the graphene oxide powder in step (1) is to make the graphene oxide raw material into blocks and then dry them, pulverize the dried graphene oxide blocks, and then treat them with a classification wheel; wherein the graphene oxide raw material is preferably made into 0.1-5 cm 3 wherein the graphene oxide raw material is further preferably made into 0.5-3cm 3 wherein the graphene oxide raw material is further preferably made into 1 cm 3 The block shape;

[0030] And / or, the graphene oxide powder in step (1) meets the following conditions: the graphene oxide powder is prepared into a 50 ppm solution, and then oscillated on an oscillator with a frequency of 11 Hz for 20 minutes, the oscillated solution is dropped on a silicon dioxide wafer, dried, and then observed under an optical microscope, and the observation result shows that the surface of the silicon wafer appears blue, without the presence of other colors;

[0031] And / or, the number of graphene oxide layers constituting the graphene oxide powder in the step (1) is ≤3 layers;

[0032] And / or, the particle size of the graphene oxide powder in step (1) is ≤70 μm; preferably 40-60 μm.

[0033] And / or, the quantitative humidification treatment method for the graphene oxide powder in step (1) is to stir the graphene oxide powder at high speed in a closed container and add atomized deionized water at the same time.

[0034] and / or, the gas maintaining the inert atmosphere is nitrogen;

[0035] And / or, the graphene oxide powder in step (1) satisfies the following conditions: the graphene oxide is prepared into a 50 ppm solution, and then oscillated on an oscillator with a frequency of 11 Hz for 20 min, the oscillated solution is dropped on a silicon dioxide wafer, dried, and then observed under an optical microscope. The result of the observation is that the surface of the silicon dioxide wafer appears blue, and no other colors exist;

[0036] And / or, the heat treatment temperature in step (2) is 350°C-700°C, and the treatment time is 5-40 min; preferably, the heat treatment temperature is 375°C-500°C, and the treatment time is 10 min-25 min;

[0037] And / or, in step (3), the thermal repair temperature is 1000°C-1500°C, and the thermal repair time is 1h-6h; preferably, the repair temperature is 1000-1300°C, and the thermal repair time is 2h-6h.

[0038] Furthermore, the few-layer graphene has the following indicators:

[0039] C (wt%) ≥ 98.5, ID / IG ≤ 1.10, BET (m2 / g) ≥ 750, oil absorption value (ml / 100g) is 4000-6000, and conductivity (S / m) ≥ 10^6.

[0040] The present invention also provides a few-layer graphene conductive paste, which is composed of few-layer graphene and a solvent, wherein the few-layer graphene has ≤4 layers, and the solid content of the few-layer graphene in the few-layer graphene conductive paste is 0.5wt%-1.5wt%;

[0041] Wherein, the solid content of the few-layer graphene is preferably 1wt%-1.3wt%;

[0042] And / or, the solvent is NMP or water;

[0043] And / or, the few-layer graphene has the following indicators:

[0044] C (wt%) ≥ 98.5, ID / IG ≤ 1.10, BET (m2 / g) ≥ 750, oil absorption value (ml / 100g) is 4000-6000, and conductivity (S / m) ≥ 10^6.

[0045] The present invention also provides an application of the few-layer graphene conductive slurry in a battery.

[0046] The present invention also provides a method for evaluating the conductivity of a graphene conductive paste, comprising the following steps: uniformly stirring the few-layer graphene conductive paste described in claim 9 with a binder, a solvent, and a main material, then performing vacuum stirring, and finally coating and drying to obtain a pole piece film, and testing the pole piece resistivity thereof by a four-probe method;

[0047] Among them, the binder is preferably PTFE or PVDF, the solvent is preferably NMP, and the main material is preferably LFP or NCM;

[0048] And / or, in the dried electrode film, the mass proportions of graphene, binder and main material are 0.2wt%, 1.2wt% and 98.60wt% respectively.

[0049] The current lithium battery market mainly uses mechanical exfoliation to obtain dozens of layers of graphene, but the exfoliation is not ideal; even if the dry graphene is obtained after drying, its thickness is too large to play the lubricating effect of few-layer or single-layer graphene. Thin-layer powdered graphene is the prerequisite for preparing graphene conductive slurry with better conductivity. The powdered graphene currently prepared on the market is all multi-layered graphene, which cannot play the advantageous characteristics of graphene's own conductivity.

[0050] There are two factors that determine the conductivity of rGO in practical applications: one is its intrinsic conductivity, which is determined by the sheet structure. The main influencing factor is the structural defects within the sheet. The fewer the defects, the more sp carrying π electrons. 2 The higher the carbon content, the better the conductivity of the flakes. The other is the degree of dispersion of graphene in the matrix. This factor is the fundamental factor that directly distinguishes graphene powder from conductive carbon black and conductive graphite. It is precisely because graphene can have a good dispersion form in the matrix and the flakes form a good connection, so as to achieve effective transmission of π electrons in the matrix. The dispersion performance is related to the binding force between graphene sheets in the graphene powder. The smaller the interaction force, the better the dispersion performance of graphene, the lower the conductivity threshold, and the less the addition amount. From another perspective, the fewer the number of single graphene sheets in the powder, the easier it is to disperse.

[0051] Through the relevant research of this patent, it is found that few-layer rGO has many advantages when used as a conductive agent for lithium-ion batteries. First, the electrode resistivity (i.e., conductivity evaluation) is orders of magnitude lower than that of conventional multilayer graphene, and the conductivity is significantly improved. At the same time, it has obvious advantages over the conductivity and threshold of general conductive agents (multilayer graphene, multi-walled carbon tubes, few-walled carbon tubes, carbon black); secondly, when preparing graphene conductive slurry, little or even no dispersant can be added to stabilize the graphene sheets, because few-layer graphene itself has liquid absorption properties and high specific surface area. Without the addition of dispersant, the graphene conductive slurry can withstand large currents during the use of downstream lithium-ion batteries, thereby improving the rapid charging and discharging performance of the battery.

[0052] The redox method is the optimal path to achieve large-scale preparation of high-monolayer graphene powder. However, during the thermal reduction of graphene oxide powder, as the temperature rises and the oxygen-containing functional groups are eliminated, the π-electron conjugated structure on the graphene sheets is restored, and these π-electron clouds can overlap between adjacent graphene sheets to form π-π stacking. The higher the degree of reduction of graphene oxide, the more fully the π-electron conjugated structure is restored, and the stronger the π-π stacking. π-π stacking increases the interaction between graphene sheets, forming a stack of sheets, resulting in the reduced graphene being a multilayer structure.

[0053] In the present invention, the moisture content and instantaneous thermal reduction temperature of GO before thermal reduction are controlled to prepare a few-layer graphene material. The exfoliation of rGO relies on the gases released instantaneously during the reduction process of oxygen-containing functional groups in GO, mainly including H 2 O、CO 2 , CO, etc. The faster the release rate of these gases, the higher the peeling degree of the sheets, and the higher the corresponding monolayer rate. The rate of gas release directly affects the air pressure between the layers. When the air pressure is much greater than the external air pressure, the van der Waals interaction between the layers can be overcome, thereby achieving the purpose of effective peeling. From this perspective, when the amount of gas that can be released from GO during reduction is more, the number of layers of rGO obtained will also be less.

[0054] In the present invention, the water content of graphene oxide powder is controlled to be between 6wt% and 25wt%. When the water content is less than 6wt%, the amount of gas released is insufficient to resist the lamellar folding caused by the reduction. When the water content is too high, greater than 25wt%, the graphene oxide powder will agglomerate, and the particle size of the agglomerated GO powder will increase significantly. During the instantaneous thermal expansion reduction, the pressure generated by the excessively large particles causes the gas to be unable to be released immediately, which in turn leads to a large number of rGO layers after reduction.

[0055] The heat treatment temperature is 350℃-700℃. When the temperature is too high, the carbon material will have a higher requirement for the inert atmosphere. If there is a small amount of flammable gas in the atmosphere (above this temperature range, water gas reaction will occur, and a small amount of O 2 A reaction will occur) and there will be adverse reactions such as sparks. Too low a temperature will cause incomplete reduction of graphene oxide and less gas release, resulting in more reduced rGO layers.

[0056] The rGO powder is repaired at high temperature, and the temperature is controlled at 1000-1500℃. Due to the shedding of oxygen-containing groups, rGO has defects. Within this temperature range, rGO undergoes defect repair and improves its performance. When the temperature is lower than 1000℃, the oxygen-containing functional groups on the surface of rGO are not completely removed, and its conductivity will be poor. When the temperature is higher than 1500℃, a rearrangement reaction of C atoms will occur, and a two-dimensional graphene sheet structure with a complete lattice will be repaired, which will cause overlap between graphene sheets (due to π-π forces).

[0057] The present invention:

[0058] (1) Inventing a graphene conductive agent suitable for high conductivity of lithium-ion batteries

[0059] Conductive agents improve the physical polarization of lithium-ion batteries through their own physical connection by forming a conductive network, increasing the contact between the main materials, or strengthening the conductive network between the main materials. The primary function of the conductive agent is to improve the electronic conductivity. The conductive agent collects microcurrents between the main materials and between the main materials and the current collector to reduce the contact resistance of the electrodes and improve the mobility of electrons in lithium batteries. Secondly, this graphene can effectively reduce the permeation threshold of graphene materials. The addition amount of traditional carbon black conductive agents is generally about 3% of the weight of the positive electrode material, while the addition amount of new conductive agents such as carbon nanotubes and conventional graphene can be reduced to 0.5%-1.0%. The graphene conductive agent in this patent can reduce the permeation threshold to 0.2%, improving the energy density, fast charging and other performance of lithium batteries.

[0060] (2) The preparation of graphene is beneficial to improving the high voltage resistance of lithium batteries

[0061] Since the patent uses a few-layer graphene as raw material, the number of layers of the few-layer graphene itself is ≤4, and the specific surface area can be as high as 900m 2 / g, when it is dispersed to prepare graphene conductive slurry, it has a strong ability to absorb liquid and can be stably dispersed in solvents. It can even stably exist in solvents with high surface energy such as NMP and isopropyl alcohol with only a very small amount of dispersant added or no dispersant added. When no dispersant is added, the graphene conductive slurry is mixed with the main material and the binder and then coated and dried to obtain the pole piece. After being assembled into a battery, due to the absence of dispersant, it has higher high voltage resistance than other materials with poor conductivity. Few-layer graphene powder is used as a conductive agent in lithium battery systems. Its conductivity is significantly better than that of all other carbon material conductive agents, except that it is weaker than single-walled carbon nanotubes, providing favorable support for lithium batteries to achieve high energy density and higher fast charging performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0063] Figure 1 This is a peeling effect diagram of the GO paste raw materials in Example 1 of the present invention after dispersion under an optical microscope;

[0064] Figure 2 is a SEM image of the test electrode in Example 1 of the present invention;

[0065] Figure 3 This is a peeling effect diagram of the GO paste raw materials in Example 2 of the present invention after dispersion under an optical microscope;

[0066] Figure 4 is a SEM image of the test electrode in Example 2 of the present invention;

[0067] Figure 5 This is a peeling effect diagram of the GO paste raw materials after dispersion under an optical microscope in Example 3 of the present invention;

[0068] Figure 6 is a SEM image of the test electrode in Example 3 of the present invention;

[0069] Figure 7 This is a peeling effect diagram of the GO paste raw materials in Example 4 of the present invention after dispersion under an optical microscope;

[0070] Figure 8 is a SEM image of the test electrode in Example 4 of the present invention;

[0071] Fig. 9 This is a peeling effect diagram of the GO paste raw materials in Comparative Example 1 of the present invention after dispersion under an optical microscope;

[0072] Fig.10 is a SEM image of the test electrode in Comparative Example 1 of the present invention;

[0073] Fig.11 This is a peeling effect diagram of the GO paste raw materials in Comparative Example 2 of the present invention after dispersion under an optical microscope;

[0074] Fig.12 is a SEM image of the test electrode in Comparative Example 2 of the present invention;

[0075] Fig.13 It is a peeling effect diagram under an optical microscope after the GO paste raw materials in Comparative Examples 3 and 4 of the present invention are dispersed;

[0076] Fig.14This is the SEM image of the test electrode in Comparative Example 3 of the present invention.

[0077] Fig.15 It is a SEM picture of the test electrode in comparative example 4 of the present invention. DETAILED DESCRIPTION

[0078] In the following description, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.

[0079] This article relates to numerical ranges. Unless otherwise specified, the above numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0080] The temperature parameters herein, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range of instrument control.

[0081] Reduced graphene oxide (rGO) in the present application is graphene obtained by reducing graphene oxide. Therefore, reduced graphene oxide (rGO) in the present application also refers to graphene.

[0082] 1. Preparation of GO Raw Materials

[0083] GO's Choice

[0084] In order to ensure that GO can be fully peeled off during thermal reduction, the raw material GO itself has ≤3 layers. The screening method in the present invention is optical microscopy, and GO is configured into a 20-100ppm solution, such as 20ppm, 25ppm, 30ppm, 35ppm, 40ppm, 45ppm, 50ppm, 55ppm, 60ppm, 65ppm, 70ppm, 75ppm, 80ppm, 85ppm, 90ppm, 95ppm, 100ppm, among which 50ppm is preferred; then at a frequency of 10 to 15H z on an oscillator, for example, 10 Hz, 11 Hz, 12 Hz, 13 Hz, 14 Hz, 15 Hz, preferably 11 Hz; oscillate for 10-40 min, for example, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, preferably 20 min; obtain a light yellow solution, drop the light yellow solution on a silicon dioxide wafer and dry it, then observe it under an optical microscope, when the surface of the silicon wafer appears light blue and there is no other color such as white, yellow, orange, black, etc., then GO is ready.

[0085] This is because silicon dioxide sheets appear light blue under an optical microscope, and single-layer graphene oxide has a high degree of transparency. When GO is less than or equal to 3 layers, it still has a certain degree of transparency, and the color of silicon dioxide sheets will not be affected by scattering and refraction. As the number of graphene oxide layers increases, the color will become darker due to the scattering and absorption effects between layers. When it exists on silicon dioxide sheets, it will form a different color from the silicon dioxide sheets.

[0086] GO moisture content control

[0087] Currently, GO on the market generally has raw materials such as dispersion, powder, and paste. However, paste is a cheaper GO. In this patent, GO paste is used as the raw material and the GO paste is dried. In order to ensure the uniformity of the dried GO, the paste GO is prepared into a uniform 1*1*1cm block and placed in an oven for drying. The size of the block can also be 0.1-5cm 3 , and further preferably made into 0.5-3cm 3The shape of the GO block does not have to be a regular shape, as long as the uniformity of the dried GO can be guaranteed. The dried GO block is placed in a powder machine, air flow mill, stone mill and other equipment for grinding and graded with a grading wheel, and the particle size of the GO powder is taken between ≤70μm. When it is greater than 70μm, it is difficult to prepare a few-layer graphene material. The thicker the graphene layer, the worse the conductivity of the prepared graphene conductive slurry. The reason for the pulverization treatment is that after making it into powder, the specific surface area of ​​the GO material will be large, and it is easier to absorb more water. At the same time, it can make the GO humidification treatment more uniform, and it will not affect the uneven gas generation during its thermal reduction, which will bring about a huge difference in the number of rGO layers, resulting in poor uniformity of the graphene material.

[0088] Test the moisture content of the GO powder. According to the moisture content, a double-mixing device is used. A certain amount of deionized water is placed in an atomizer. The GO powder is stirred at high speed in a closed container, and the atomized deionized water is added to the closed container in the same direction. The GO powder is quantitatively humidified using the above method. The moisture content of the GO powder is controlled between 6wt% and 25wt%, such as 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, wherein 10wt%-18wt% is preferred. Since GO itself is a material rich in oxygen functional groups, it has a strong ability to contain and retain water. Under this moisture content, the GO powder still remains in powder form and no agglomeration occurs.

[0089] 2. Thermal reduction of GO

[0090] This patent adopts a method of preparing rGO by heat treatment GO reduction. By controlling the temperature of heat reduction, the gas gathers enough between GO layers to achieve the effect of instantaneous reduction and gas evaporation. To achieve the effect of generating a large amount of gas, the higher the temperature, the better. However, when the temperature is too high, the carbon material will have a higher requirement for the inert atmosphere. If there is a small amount of flammable gas in the atmosphere (GO will produce CO gas during heat treatment reduction, which will react with the small amount of O at high temperature), the carbon material will have a higher requirement for the inert atmosphere. 2There will be reactions) and there will be adverse reactions such as sparks. Therefore, the temperature of the thermal annealing reduction needs to be controlled within a certain range, preferably 350℃~700℃, such as 350℃, 375℃, 400℃, 425℃, 450℃, 475℃, 500℃, 525℃, 550℃, 575℃, 600℃, 625℃, 650℃, 675℃, 700℃; 375℃-500℃ is preferred. Although GO begins to thermally decompose at 150℃, the higher the temperature, the higher the amount of gas and water vapor generated by instantaneous reduction. In this patent, humidification treatment is performed, and higher heat is required to vaporize water, so the minimum temperature is recommended to be 350℃.

[0091] The specific implementation steps are as follows: pour the GO powder with increased moisture content into a nitrogen-protected heat-conducting vessel (not sealed), place the heat-conducting vessel in a nitrogen atmosphere at a temperature of 350°C to 700°C, and heat treat for 5-40 minutes, for example, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, and 40 minutes, preferably 10 minutes to 25 minutes, to obtain fluffy rGO black powder.

[0092] In the present invention, the inert atmosphere is a controlled environment in which the gas in the air is replaced by a chemically inactive gas. The chemically inactive gas can be an inert gas such as argon (Ar), helium (He), neon (Ne), krypton (kr), xenon (xe), radon (Rn), nitrogen, etc.

[0093] 3. High temperature repair of rGO powder

[0094] The black powder is heat treated in a high temperature furnace under an inert atmosphere, and the temperature is controlled at 1000-1500°C, such as 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, 1500°C; preferably 1000-1300°C; the heat treatment time is between 1h-6h, such as 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h; preferably 2h-6h. After high temperature repair treatment, a few-layer graphene powder is obtained.

[0095] 4. Few-layer graphene selection

[0096] To prepare graphene conductive paste with good conductivity, the number of layers of graphene raw materials itself needs to be small, so the number of layers of graphene raw materials should be ≤4 (the average number of layers is 2 to 3 layers), and the graphene itself has relatively few surface defects. Based on this, the selection indicators of raw material graphene powder are as follows:

[0097]

[0098] Since the number of rGO layers is difficult to measure directly, the specific surface area is usually used instead. The number of layers = 2630 / BET. The calculated specific surface area of ​​5-layer graphene = 2630 / 5 = 526 m 2 / g. Since the BET test is an average value, to ensure that the number of graphene layers of the few-layer graphene powder is within 5 layers, it is necessary to ensure that the BET value is controlled at about 3 layers, that is, the BET value is ≥750m 2 / g.

[0099] 5. Preparation of Few-layer Graphene Conductive Slurry

[0100] The few-layer graphene powder is dispersed in a solvent, preferably NMP as the solvent. Since the oil absorption value and specific surface area of ​​the few-layer graphene are relatively high, the few-layer graphene has strong liquid absorption and liquid retention capabilities, and the few-layer graphene can be dispersed in the solution with very little or no dispersant. At the same time, the disadvantage is that it is impossible to achieve a high-solid graphene conductive slurry, because the higher the solid content, the greater the viscosity of the conductive slurry, and it is difficult to disperse evenly. The dispersion methods include: homogenization, micro-jet, sand mill dispersion and other means, so the solid content of the few-layer graphene slurry is generally 0.5-1.5wt%; for example, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%; among which 1wt%-1.3wt% is preferred.

[0101] 6. Conductivity evaluation of few-layer graphene conductive agents

[0102] The internal resistance of the pole film is generally tested for the evaluation of the conductivity of the lithium battery system. This patent also uses the pole resistivity test method to evaluate the conductivity of the few-layer graphene. The general method is: the prepared graphene conductive slurry is mixed with the binder and the main material in proportion, then vacuum stirred, and finally coated and dried to obtain the pole film, in which the few-layer graphene accounts for 0.2wt% by weight, and the pole resistivity is tested by the four-probe method. The test results are compared with other graphene, multi-walled carbon nanotubes, and the results are as follows:

[0103]

[0104] From the comparison in the table above, under the same amount of conductive agent added, the resistivity of few-layer graphene is obviously lower than that of the current conductive agents with better conductivity in the market (multi-walled carbon tubes, graphene SE1233, few-walled carbon tubes), but the resistivity is still significantly higher than that of single-walled carbon nanotubes. Few-layer graphene powder is still the top 2 material in terms of conductivity, creating a precedent for the application of graphene powder with higher conductivity, and further verifying that it is possible for graphene materials to achieve the theoretical conductivity of graphene.

[0105] The main reason why its conductive performance is superior to other graphene-based conductive agents is that it can remain in a single-layer state in the slurry and can form a single-layer coated conductive network wrapped around the outer surface of the main material.

[0106] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0107] Embodiment 1:

[0108] This embodiment shows a method for preparing a few-layer graphene, a method for preparing a conductive paste thereof, and a method for evaluating conductivity.

[0109] 1. GO’s Choice

[0110] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Figure 1 As shown:

[0111] Figure 1 The whole picture is blue and there are no thick flakes, which means that the GO can be easily peeled off into thin layers.

[0112] 2. Powder preparation with controlled humidity

[0113] The selected GO paste was made into a block of 1*1*1cm in shape and placed in an oven for drying. The dried GO block was pulverized and the particle size of the GO powder was tested after treatment with a grading wheel: D50 = 60μm. The moisture content of the GO powder was then tested to be 3.5wt%. The amount of deionized water required to be added to a moisture content of 6wt% was calculated based on the amount of GO. The above amount of water was added by atomization under high-speed stirring of the GO powder. A GO powder with a moisture content of 6wt% was obtained.

[0114] 3. GO powder thermal reduction and high temperature repair

[0115] The GO powder with a moisture content of 6 wt% was poured into a heat-conducting vessel (not sealed) protected by nitrogen, and the heat-conducting vessel was placed in a nitrogen atmosphere at a temperature of 375°C for 25 minutes to obtain fluffy rGO black powder. The powder was kept at 1000°C for 6 hours to obtain a powder of few-layer graphene.

[0116] The indicators of few-layer graphene powder are as follows:

[0117]

[0118] 4. Preparation of graphene conductive slurry

[0119] The graphene powder is dispersed in a solvent, preferably NMP as a solvent, and the solid content of the graphene slurry is 1.15wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution. Then, the graphene NMP slurry is dispersed by sand milling, with zirconium beads of 1mm, grinding power of 2kw, and grinding time of 2.5h. The solid content of the graphene conductive slurry is 1.20wt%.

[0120] 5. Conductivity evaluation of graphene conductive agent

[0121] Prepare a pole piece with a solid ratio of 0.2wt% graphene content. Add 2.434g of 10% PVDF (polyvinylidene fluoride) glue, 3.381g of 1.20wt% graphene conductive slurry, 20g of positive electrode main material and 4.015g of NMP to the mixing tank of the vacuum mixer according to the ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and dry it after scraping to obtain the pole piece. The pole piece resistivity is measured to be 26.7Ω·cm.

[0122] The calculation method for the graphene solid ratio of 0.2wt% is:

[0123]

[0124] The SEM of the test pole piece is as follows Figure 2 shown.

[0125] Embodiment 2:

[0126] This embodiment shows a method for preparing a few-layer graphene, a method for preparing a conductive paste thereof, and a method for evaluating conductivity.

[0127] 1. GO’s Choice

[0128] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Figure 3 As shown:

[0129] Figure 3 The whole picture is blue, and there are no thick flakes of other colors, indicating that the GO can be easily peeled off into thin layers.

[0130] 2. Powder preparation with controlled humidity

[0131] The selected GO paste was made into a block of 1*1*1cm in shape and placed in an oven for drying. The dried GO block was pulverized and the particle size of the GO powder was tested after treatment with a grading wheel: D50 = 40μm. The moisture content of the GO powder was then tested to be 1.0wt%. The amount of deionized water required to be added to a moisture content of 25wt% was calculated based on the amount of GO. The above amount of water was added by atomization while the GO powder was stirred at high speed. GO powder with a moisture content of 25wt% was obtained.

[0132] 3. GO powder thermal reduction and high temperature repair

[0133] The GO powder with a moisture content of 25 wt% was poured into a heat-conducting vessel (not sealed) protected by nitrogen, and the heat-conducting vessel was placed in a nitrogen atmosphere at a temperature of 415°C for 20 minutes to obtain fluffy rGO black powder. The powder was kept at 1200°C for 2.5 hours to obtain a powder of few-layer graphene.

[0134] The indicators of few-layer graphene powder are as follows:

[0135]

[0136] 4. Preparation of graphene conductive slurry

[0137] The graphene powder is dispersed in a solvent, preferably NMP as the solvent, and the solid content of the graphene slurry is configured to be 1wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution, and then the graphene NMP slurry is poured into a homogenizer and homogenized 3 times at a pressure of 1000MPa. The solid content of the graphene conductive slurry is 1.16wt%.

[0138] 5. Conductivity evaluation of graphene conductive agent

[0139] Prepare a pole piece with a solid ratio of 0.2wt% graphene content. Add 2.434g of 10% PVDF glue, 3.50g of 1.16wt% graphene conductive slurry, 20g of positive electrode main material and 3.256g of NMP to the mixing tank of the vacuum mixer according to the ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and after scraping, dry it to get the pole piece. The pole piece resistivity is measured to be 25.4Ω·cm.

[0140] The SEM of the test pole piece is as follows Figure 4 as shown.

[0141] Embodiment 3:

[0142] This embodiment shows a method for preparing a few-layer graphene, a method for preparing a conductive paste thereof, and a method for evaluating conductivity.

[0143] 1. GO’s Choice

[0144] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Figure 5 As shown:

[0145] Figure 5 The whole picture is blue and there are no thick flakes, which means that the GO can be easily peeled off into thin layers.

[0146] 2. Powder preparation with controlled humidity

[0147] The selected GO paste was made into a block of 1*1*1cm in shape and placed in an oven for drying. The dried GO block was pulverized and the particle size of the GO powder was tested after treatment with a grading wheel: D50 = 60μm. The moisture content of the GO powder was then tested to be 3.5wt%. The amount of deionized water required to be added to a moisture content of 10wt% was calculated based on the amount of GO. The above amount of water was added by atomization while the GO powder was stirred at high speed. GO powder with a moisture content of 10wt% was obtained.

[0148] 3. GO powder thermal reduction and high temperature repair

[0149] The GO powder with a moisture content of 10 wt% was poured into a heat-conducting vessel (not sealed) protected by nitrogen, and the heat-conducting vessel was placed in a nitrogen atmosphere at a temperature of 520°C. After 40 minutes of heat treatment, fluffy rGO black powder was obtained. The powder was kept at 1500°C for 1 hour to obtain a powder of few-layer graphene. The specific surface area of ​​the few-layer graphene powder was 879 m 2 / g.

[0150] The indicators of few-layer graphene powder are as follows:

[0151]

[0152] 4. Preparation of graphene conductive slurry

[0153] The graphene powder is dispersed in a solvent, preferably NMP as the solvent, and the solid content of the graphene slurry is 0.5wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution, and then the graphene NMP slurry is poured into a homogenizer and homogenized 3 times at a pressure of 1000MPa. The graphene conductive slurry has a solid content of 0.5wt%.

[0154] 5. Conductivity evaluation of graphene conductive agent

[0155] Prepare a pole piece with a solid ratio of 0.2wt% graphene content. Add 2.434g of 10% PVDF glue, 8.114g of 0.5wt% of the above graphene conductive slurry, 20g of positive electrode main material and 3.707g of NMP in the mixing tank of the vacuum mixer according to the ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and dry it after scraping to obtain the pole piece. The pole piece resistivity was measured to be 24.7Ω·cm.

[0156] The SEM of the test pole piece is as follows Figure 6 shown.

[0157] Embodiment 4:

[0158] This embodiment shows a method for preparing a few-layer graphene, a method for preparing a conductive paste thereof, and a method for evaluating conductivity.

[0159] 1. GO’s Choice

[0160] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Figure 7 As shown:

[0161] Figure 7 The whole picture is blue and there are no thick flakes, which means that the GO can be easily peeled off into thin layers.

[0162] 2. Powder preparation with controlled humidity

[0163] The selected GO paste was made into a block of 1*1*1cm in shape and placed in an oven for drying. The dried GO block was pulverized and the particle size of the GO powder was tested after treatment with a grading wheel: D50 = 60μm. The moisture content of the GO powder was then tested to be 3.5wt%. The amount of deionized water required to be added to a moisture content of 15wt% was calculated based on the amount of GO. The above amount of water was added by atomization under high-speed stirring of the GO powder. A GO powder with a moisture content of 15wt% was obtained.

[0164] 3. GO powder thermal reduction and high temperature repair

[0165] The GO powder with a moisture content of 15 wt% was poured into a heat-conducting vessel (not sealed) protected by nitrogen, and the heat-conducting vessel was placed in a nitrogen atmosphere at a temperature of 700°C. After 5 minutes of heat treatment, fluffy rGO black powder was obtained. The powder was kept at 1000°C for 6 hours to obtain a powder of few-layer graphene. The specific surface area of ​​the few-layer graphene powder was 923 m 2 / g.

[0166] The indicators of few-layer graphene powder are as follows:

[0167]

[0168] 2. Preparation of graphene conductive slurry

[0169] The graphene powder is dispersed in a solvent, preferably NMP as the solvent, and the solid content of the graphene slurry is 1.4wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution, and then the graphene NMP slurry is poured into a homogenizer and homogenized 3 times at a pressure of 1000MPa. The solid content of the graphene conductive slurry is 1.46wt%.

[0170] 3. Conductivity evaluation of graphene conductive agent

[0171] Prepare a pole piece with a solid ratio of 0.2wt% graphene content. Add 2.434g of 10% PVDF glue, 2.779g of 1.46wt% of the above graphene conductive slurry, 20g of positive electrode main material and 3.298g of NMP in the mixing tank of the vacuum mixer according to the ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and after scraping, dry it to get the pole piece. The pole piece resistivity is measured to be 23.8Ω·cm.

[0172] The SEM of the test pole piece is as follows Figure 8 shown.

[0173] Comparative Example 1:

[0174] This comparative example shows a method for preparing graphene, a method for preparing a conductive paste thereof and a method for evaluating conductivity when the raw material is multilayer GO.

[0175] 1. GO’s Choice

[0176] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Fig. 9 As shown:

[0177] Fig. 9 It is shown that there are a lot of colors other than blue in the picture, indicating that the GO stripping effect is far worse than the demand.

[0178] 2. Powder preparation with controlled humidity

[0179] The selected GO paste was made into a block of 1*1*1cm in shape and placed in an oven for drying. The dried GO block was pulverized and the particle size of the GO powder was tested after treatment with a grading wheel: D50 = 30μm. The moisture content of the GO powder was then tested to be 1.5wt%. The amount of deionized water required to be added to a moisture content of 12wt% was calculated based on the amount of GO. The above amount of water was added by atomization while the GO powder was stirred at high speed. GO powder with a moisture content of 12wt% was obtained.

[0180] 3. GO powder thermal reduction and high temperature repair

[0181] The GO powder with a moisture content of 12 wt % was poured into a heat-conducting container (not sealed) protected by nitrogen, and the heat-conducting container was placed in a nitrogen atmosphere at a temperature of 500° C. After heat treatment for 20 minutes, fluffy rGO black powder was obtained.

[0182] The temperature was kept at 1250°C for 2.5 hours to obtain black multilayer graphene powder.

[0183] The characteristics of the prepared multi-layer graphene material are as follows:

[0184]

[0185] 4. Preparation of graphene conductive slurry

[0186] The graphene powder is dispersed in a solvent, preferably NMP as the solvent, and the solid content of the graphene slurry is configured to be 1wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution, and then the graphene NMP slurry is poured into a homogenizer and homogenized 3 times at a pressure of 1000MPa. The solid content of the graphene conductive slurry is 1.05wt%.

[0187] 5. Conductivity evaluation of graphene conductive agent

[0188] Prepare a pole piece with a solid ratio of 0.2wt% graphene content. Add 2.434g of 10% PVDF glue, 3.864g of 1.05wt% graphene conductive slurry, 20g of positive electrode main material and 3.532g of NMP to the mixing tank of the vacuum mixer according to the ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and dry it after scraping to obtain the pole piece. The pole piece resistivity is measured to be 123Ω·cm.

[0189] The SEM of the test pole piece is as follows Fig.10 shown.

[0190] Comparative Example 2:

[0191] This comparative example shows the preparation method of graphene, the preparation method of its conductive slurry and the conductivity evaluation method under the condition of poor GO exfoliation effect and 1.5wt% water content.

[0192] 1. GO’s Choice

[0193] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Fig.11 As shown:

[0194] Fig.11 It is shown that there are a small number of bright yellow, red, orange, and green thick flakes in the picture except for blue, indicating that the GO exfoliation effect is worse than the demand.

[0195] 2. Powder preparation with controlled humidity

[0196] The selected GO paste was made into blocks of 1*1*1 cm in shape and placed in an oven for drying. The dried GO blocks were powdered and the particle size of the GO powder was tested after being processed by a grading wheel: D50 = 45.7 μm. The moisture content of the GO powder was then tested to be 1.5 wt%.

[0197] 3. GO powder thermal reduction and high temperature repair

[0198] The GO powder with a moisture content of 1.5 wt % was poured into a heat-conducting container (not sealed) protected by nitrogen, and the heat-conducting container was placed in a nitrogen atmosphere at a temperature of 450° C. After a heat treatment for 20 minutes, fluffy rGO black powder was obtained.

[0199] The temperature was kept at 1250°C for 2.5 hours to obtain black multilayer graphene powder.

[0200] The characteristics of the prepared multi-layer graphene material are as follows:

[0201]

[0202] 4. Preparation of graphene conductive agent

[0203] The graphene powder is dispersed in a solvent, preferably NMP as the solvent, and the solid content of the graphene slurry is configured to be 1wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution, and then the graphene NMP slurry is poured into a homogenizer and homogenized 3 times at a pressure of 1000MPa. The graphene conductive slurry has a solid content of 1.10wt%.

[0204] 5. Conductivity evaluation of graphene conductive agent

[0205] Prepare a pole piece with a solid ratio of 0.25wt% graphene content. Add 2.435g of 10% PVDF glue, 3.688g of 1.10wt% graphene slurry, 20g of positive electrode main material and 7.516g of NMP in the mixing tank of the vacuum mixer according to the following ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and after scraping, dry it to get the pole piece. The pole piece resistivity is measured to be 146Ω·cm.

[0206] The SEM of the test pole piece is as follows Fig.12 shown.

[0207] Comparative Example 3:

[0208] This comparative example shows a method for preparing graphene, a method for preparing a conductive slurry thereof and a method for evaluating conductivity when the moisture content of GO is 30 wt%.

[0209] 1. GO’s Choice

[0210] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Fig.13 As shown:

[0211] Fig.13 It shows that only blue and light blue flakes exist in the picture, indicating that the exfoliation effect of GO itself is good.

[0212] 2. Powder preparation with controlled humidity

[0213] The selected GO paste was made into a block of 1*1*1cm in shape and placed in an oven for drying. The dried GO block was pulverized and the particle size of the GO powder was tested after treatment with a grading wheel: D50 = 43.7μm. The moisture content of the GO powder was then tested to be 1.5wt%. The amount of deionized water required to be added to a moisture content of 30wt% was calculated based on the amount of GO. The above amount of water was added by atomization under high-speed stirring of the GO powder. A GO powder with a moisture content of 30wt% was obtained.

[0214] 3. GO powder thermal reduction and high temperature repair

[0215] The GO powder with a moisture content of 30 wt% was poured into a heat-conducting container (not sealed) protected by nitrogen, and the heat-conducting container was placed in a nitrogen atmosphere at a temperature of 500° C. After a heat treatment for 10 minutes, fluffy rGO black powder was obtained.

[0216] The mixture was heated at 1500°C for 2 hours to obtain black multilayer graphene powder.

[0217] The characteristics of the prepared multi-layer graphene material are as follows:

[0218]

[0219] 4. Preparation of graphene conductive slurry

[0220] The graphene powder is dispersed in a solvent, preferably NMP as the solvent, and the solid content of the graphene slurry is configured to be 1wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution, and then the graphene NMP slurry is poured into a homogenizer and homogenized 3 times at a pressure of 1000MPa. The graphene conductive slurry has a solid content of 1.10wt%.

[0221] 5. Conductivity evaluation of graphene conductive agent

[0222] Prepare a pole piece with a solid ratio of 0.25wt% graphene content. Add 2.435g of 10% PVDF glue, 3.688g of 1.10wt% graphene slurry, 20g of positive electrode main material and 6.414g of NMP in the mixing tank of the vacuum mixer according to the following ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and after scraping, dry it to get the pole piece. The pole piece resistivity was measured to be 78.6Ω·cm.

[0223] The SEM of the test pole piece is as follows Fig.14 shown.

[0224] Comparative Example 4

[0225] This comparative example shows the preparation method of graphene, the preparation method of its conductive paste and the conductivity evaluation method when the particle size of GO powder is D50=100 μm.

[0226] 1. GO’s Choice

[0227] Select GO paste raw materials, prepare GO slurry with a solid content of 50 ppm with deionized water, oscillate it in water at an oscillation frequency of 11 Hz for 20 minutes, drop it on a clean and defect-free silicon oxide wafer and dry it, and observe its peeling effect under an optical microscope, as shown in Figure 2. Fig.13 As shown:

[0228] Fig.13 It shows that only blue and light blue flakes exist in the picture, indicating that the exfoliation effect of GO itself is good.

[0229] 2. Powder preparation with controlled humidity

[0230] The selected GO paste was made into a block of 1*1*1cm in shape and placed in an oven for drying. The dried GO block was pulverized and the particle size of the GO powder was tested after treatment with a grading wheel: D50 = 100μm. The moisture content of the GO powder was then tested to be 1.5wt%. The amount of deionized water required to be added to a moisture content of 15wt% was calculated based on the amount of GO. The above amount of water was added by atomization while the GO powder was stirred at high speed. GO powder with a moisture content of 15wt% was obtained.

[0231] 3. GO powder thermal reduction and high temperature repair

[0232] The GO powder with a moisture content of 15 wt % was poured into a heat-conducting container (not sealed) protected by nitrogen, and the heat-conducting container was placed in a nitrogen atmosphere at a temperature of 500° C. After a heat treatment for 10 minutes, fluffy rGO black powder was obtained.

[0233] By keeping the temperature at 1500°C for 2h, black multilayer graphene powder was obtained.

[0234] The characteristics of the prepared multi-layer graphene material are as follows:

[0235]

[0236] 4. Preparation of graphene conductive slurry

[0237] The graphene powder is dispersed in a solvent, preferably NMP as the solvent, and the solid content of the graphene slurry is configured to be 1wt%. First, it is stirred at a stirring speed of 2000rmp for 30min to make it well dispersed in the NMP solution, and then the graphene NMP slurry is poured into a homogenizer and homogenized 3 times at a pressure of 1000MPa. The graphene conductive slurry has a solid content of 1.10wt%.

[0238] 5. Conductivity evaluation of graphene conductive agent

[0239] Prepare a pole piece with a solid ratio of 0.2wt% graphene content. Add 2.435g of 10% PVDF glue, 3.688g of 1.10wt% graphene slurry, 20g of positive electrode main material and 6.818g of NMP in the mixing tank of the vacuum mixer according to the following ratio and order. After preparation, use a feeding spoon to quickly stir the material evenly without obvious particles. Start vacuum mixing (speed 600rpm) for 140min before discharging. Put the PET film on the flat coating machine, turn on the vacuum, attach the PET flatly to the scraper, scrape with a 200μm blade, and dry it after scraping to obtain the pole piece. The pole piece resistivity is measured to be 63.5Ω·cm.

[0240] The SEM of the test pole piece is as follows Fig.15 shown.

[0241] In the present invention

[0242]

[0243]

[0244] It can be seen from the table that when the carbon content of graphene increases, ID / IG decreases, BET increases, and the oil absorption value decreases, its conductivity increases, and the resistivity when made into a pole piece decreases. It can be seen from the embodiments and comparative examples that the conductivity of graphene in the embodiments is increased by 2-3 orders of magnitude compared with the comparative example, and the resistivity when made into a pole piece is reduced by up to 6 times.

[0245] Although the above disclosed content shows exemplary embodiments of the present invention, it should be noted that, without departing from the scope defined in the claims, various changes and modifications may be made. In addition, although elements of the present invention may be described or required in individual form, it is also conceivable to have multiple elements, unless explicitly limited to a single element.

[0246] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a few-layer graphene conductive slurry, It is characterized in that The following steps are involved: Dispersing the few-layer graphene in a solvent, wherein the few-layer graphene has a layer number of ≤4 layers, and the solid content of the few-layer graphene in the few-layer graphene conductive slurry is 0.5wt%-1.5wt%.

2. The method for preparing the few-layer graphene conductive paste according to claim 1, It is characterized in that The solid content of the few-layer graphene is 1wt%-1.3wt%; And / or, the solvent is NMP or water; And / or, the few-layer graphene has the following indicators: C(wt%)≥98.5, ID / IG≤1.10, BET(m 2 / g)≥750, oil absorption value (ml / 100g) is 4000~6000, and electrical conductivity (S / m)≥10^6.

3. The method for preparing the few-layer graphene conductive paste according to claim 2, It is characterized in that The dispersion method is preferably homogeneous dispersion, microfluidic dispersion, or sand mill dispersion.

4. The method for preparing the few-layer graphene conductive paste according to claim 3, It is characterized in that The dispersion method is to disperse the slurry containing the few-layer graphene by sand grinding, wherein the zirconium beads are 1-3 mm, the grinding power is 1-3 kw, and the grinding time is 1-3 h.

5. The method for preparing the few-layer graphene conductive paste according to claim 3, It is characterized in that The dispersion method is to stir the slurry containing the few-layer graphene at a stirring speed of 1000-5000 rpm for 20-40 minutes, and then put the stirred slurry into a homogenizer and homogenize it 2-4 times at a pressure of 800-1000 MPa.

6. The method for preparing the few-layer graphene conductive paste according to claim 1, It is characterized in that The preparation method of the few-layer graphene comprises the following steps: (1) humidifying the graphene oxide powder, wherein the graphene oxide powder satisfies the following conditions: The graphene oxide powder is prepared into a 20-100 ppm solution, and then oscillated on an oscillator with a frequency of 10-15 Hz for 10-40 minutes. The oscillated solution is dropped on a silicon dioxide wafer and dried, and then observed under an optical microscope. The observation result shows that the surface of the silicon dioxide wafer appears blue, and no other colors exist. And / or, the moisture content of the humidified graphene oxide powder is 6wt%-25wt%; preferably, the moisture content of the humidified graphene oxide powder is 10wt%-18wt%; (2) heat treating the humidified graphene oxide powder under an inert atmosphere, so that the graphene oxide releases gas during the reduction process to cause the graphene oxide to peel off; (3) The product of step (2) is subjected to thermal repair treatment under an inert atmosphere to obtain a few-layer graphene powder.

7. The method for preparing the few-layer graphene conductive paste according to claim 6, It is characterized in that The production process of the graphene oxide powder in step (1) is to make the graphene oxide raw material into blocks and then dry them, pulverize the dried graphene oxide blocks, and then treat them with a classification wheel; wherein the graphene oxide raw material is preferably made into 0.1-5 cm 3 wherein the graphene oxide raw material is further preferably made into 0.5-3cm 3 wherein the graphene oxide raw material is further preferably made into 1 cm 3 The block shape; And / or, the graphene oxide powder in step (1) satisfies the following conditions: the graphene oxide powder is prepared into a 50 ppm solution, and then oscillated on an oscillator with a frequency of 11 Hz for 20 minutes, the oscillated solution is dropped on a silicon dioxide wafer, dried, and then observed under an optical microscope, and the observation result shows that the surface of the silicon dioxide wafer appears blue, without the presence of other colors; And / or, the number of graphene oxide layers constituting the graphene oxide powder in the step (1) is ≤3 layers; And / or, the particle size of the graphene oxide powder in step (1) is ≤70 μm; preferably 40-60 μm; And / or, the quantitative humidification treatment method for the graphene oxide powder in step (1) is to stir the graphene oxide powder at high speed in a closed container and add atomized deionized water at the same time; and / or, the gas maintaining the inert atmosphere is nitrogen; And / or, the graphene oxide powder in step (1) satisfies the following conditions: the graphene oxide is prepared into a 50 ppm solution, and then oscillated on an oscillator with a frequency of 11 Hz for 20 min, the oscillated solution is dropped on a silicon dioxide wafer, dried, and then observed under an optical microscope. The observation result shows that the surface of the silicon wafer appears blue, without the presence of other colors; And / or, in step (2), the heat treatment temperature is 350°C-700°C, and the treatment time is 5-40 min; preferably, the heat treatment temperature is 375°C-500°C, and the treatment time is 10 min-25 min; And / or, in step (3), the thermal repair temperature is 1000°C-1500°C, and the thermal repair time is 1h-6h; preferably, the repair temperature is 1000-1300°C, and the thermal repair time is 2h-6h.

8. A few-layer graphene conductive paste, It is characterized in that Composed of a few-layer graphene and a solvent, wherein the few-layer graphene has ≤4 layers, and the solid content of the few-layer graphene in the few-layer graphene conductive slurry is 0.5wt%-1.5wt%; Wherein, the solid content of the few-layer graphene is preferably 1wt%-1.3wt%; And / or, the solvent is NMP or water; And / or, the few-layer graphene has the following indicators: C(wt%)≥98.5, ID / IG≤1.10, BET(m 2 / g)≥750, oil absorption value (ml / 100g) is 4000~6000, and electrical conductivity (S / m)≥10^6.

9. Use of the few-layer graphene conductive slurry according to claim 8 in a battery.

10. A method for evaluating the conductivity of a graphene conductive agent, It is characterized in that The method comprises the following steps: uniformly mixing the few-layer graphene conductive slurry as claimed in claim 9 with a binder, a solvent and a main material, then performing vacuum stirring, and finally coating and drying to obtain an electrode film, and testing the electrode resistivity thereof by a four-probe method; Among them, the binder is preferably PTFE or PVDF, the solvent is preferably NMP, and the main material is preferably LFP or NCM; And / or, in the dried electrode film, the mass proportions of graphene, binder and main material are 0.2wt%, 1.2wt% and 98.60wt% respectively.

Citation Information

Cited By

  • Preparation method and application of sodium ion battery negative electrode material with improved conductivity

    CN119551651B

  • Low-defect few-layer graphene water-based conductive paste and preparation method and application thereof

    CN120748797A