Solar cell and preparation method thereof

By using the adaptive PEDOT:F material and processing technology in organic/silicon heterojunction solar cells, an efficient hole transport layer is formed, which solves the problem of poor acidity and wettability of PEDOT:PSS materials and improves the solar cell's Photoelectric conversion efficiency and stability.

CN119031728APending Publication Date: 2024-11-26LONGI GREEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411103049.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The PEDOT:PSS materials used in existing organic/silicon heterojunction solar cells have problems such as strong acidity, easy to absorb moisture and poor surface wetting, which limits the photoelectric conversion efficiency and stability.

Method used

A mixed solution of PEDOT:F with a mass concentration ratio of 0.1:9.9 to 7:3 was used to prepare a hole transport layer, and a variable speed spin coating and annealing treatment, combined with cleaning and UV/O3 treatment, a suitable PEDOT was formed: F film, add a p-type passivation material layer to improve photoelectric conversion efficiency and stability.

Benefits of technology

The photoelectric conversion efficiency and stability of solar cells are improved, efficient photoelectric conversion and a long-life hole transport layer are achieved, and the passivation performance of the battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031728A_ABST
    Figure CN119031728A_ABST
Patent Text Reader

Abstract

The invention provides a solar cell, the solar cell comprises a crystalline silicon substrate and a hole transport layer, the hole transport layer is formed on the front surface or the back surface of the crystalline silicon substrate, the hole transport layer is prepared from a mixed solution of PEDOT: F and a solvent according to a mass concentration ratio of 0.1: 9.9-7: 3, and the hole transport layer is formed on the front surface or the back surface of the crystalline silicon substrate. Wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butyl alcohol or ethyl acetate. The solar cell is high in photoelectric conversion efficiency and good in stability. The invention also provides a method for preparing the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar photovoltaic technology, and in particular to a solar cell and a preparation method thereof. Background Art

[0002] The current organic / silicon heterojunction solar cells mainly use PEDOT:PSS as an organic material to form a heterojunction with silicon. PEDOT:PSS has the disadvantages of strong acidity, easy hygroscopicity, and poor wettability on the surface of the active layer, which limits the photoelectric conversion efficiency and stability of PEDOT:PSS / Si heterojunction solar cells.

[0003] Therefore, it is necessary to provide an improved solar cell and a method for preparing the same to overcome or reduce at least a portion of the disadvantages of the above-mentioned prior art. Summary of the invention

[0004] In a first aspect of the present invention, a solar cell is provided, wherein the solar cell comprises: a crystalline silicon substrate and a hole transport layer, the hole transport layer being formed on the front side or the back side of the crystalline silicon substrate, wherein the hole transport layer is prepared from a mixture of PEDOT:F and a solvent having a mass concentration ratio of 0.1:9.9 to 7:3, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate.

[0005] The solar cell of the present invention comprises a crystalline silicon substrate and a hole transport layer, wherein the hole transport layer is formed on the front side or the back side of the crystalline silicon substrate, and is prepared by setting the hole transport layer to be a mixed solution of PEDOT:F and a solvent with a mass concentration ratio of 0.1:9.9 to 7:3, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate, so that the solar cell has high photoelectric conversion efficiency and good stability.

[0006] Optionally, the mixed solution is subjected to variable speed spin coating and annealing to obtain a hole transport layer. By using variable speed spin coating and annealing, a PEDOT:F film having suitable thickness, contact resistance, minority carrier lifetime, etc. can be obtained.

[0007] Optionally, the variable speed spin coating is firstly spin coating at 10-1000 rpm for 1-10 s, and then spin coating at 3400-3600 rpm for >30 s; and / or

[0008] Annealing treatment is annealing at a temperature of <150°C for >10 min; and / or

[0009] The thickness of the hole transport layer is 4-50 nm.

[0010] Optionally, the hole transport layer is prepared from a mixture of PEDOT:F and ethanol in a mass concentration ratio of 4:10, and the thickness of the hole transport layer is 18.4-20 nm.

[0011] Optionally, the hole transport layer is formed on the back side of the crystalline silicon substrate, and the hole transport layer directly contacts the crystalline silicon substrate; or

[0012] The hole transport layer is formed on the back of the crystalline silicon substrate, and a p-type passivation material layer is provided between the hole transport layer and the crystalline silicon substrate, wherein the p-type passivation material layer is selected from an aluminum oxide layer, a silicon oxide layer, a P-doped silicon oxide layer, or a titanium oxide layer. By adding a p-type passivation material layer, surface recombination can be effectively reduced and photoelectric conversion efficiency can be improved.

[0013] Optionally, before forming the hole transport layer on the back side of the crystalline silicon substrate, the back side of the crystalline silicon substrate is cleaned with a cleaning solvent, wherein the cleaning solvent is selected from hydrofluoric acid, a mixture of hydrofluoric acid and nitric acid, a mixture of ammonia water and hydrogen peroxide, or phosphoric acid. By cleaning the back side of the crystalline silicon substrate with a cleaning solvent, the oxide layer can be effectively removed.

[0014] Optionally, after cleaning the back side of the crystalline silicon substrate, UV / O3 treatment is performed for >10 min, and then a hole transport layer is formed on the back side of the crystalline silicon substrate. By continuing to perform UV / O3 treatment, a strong oxidation environment can be constructed to remove impurities on the surface of the crystalline silicon substrate.

[0015] Optionally, the solar cell includes:

[0016] An anti-reflection layer, wherein the anti-reflection layer is a silicon nitride layer with a thickness of 50-80 nm, or the anti-reflection layer is a titanium oxide layer with a thickness of 50-100 nm;

[0017] A passivation layer, wherein the passivation layer is a silicon oxide layer and has a thickness of 1-10 nm;

[0018] A crystalline silicon substrate, wherein the crystalline silicon substrate is a p-type silicon wafer;

[0019] A p-type passivation material layer, wherein the p-type passivation material layer is a PE-ALD aluminum oxide layer and has a thickness of 1.10-1.15 nm; and

[0020] The hole transport layer is prepared from a mixture of PEDOT:F and ethanol in a mass concentration ratio of 4:10 and has a thickness of 18.4-20 nm.

[0021] Optionally, the hole transport layer is formed on the front side of the crystalline silicon substrate, and the hole transport layer directly contacts the crystalline silicon substrate; or

[0022] The hole transport layer is formed on the front side of the crystalline silicon substrate, and there is a passivation layer between the hole transport layer and the crystalline silicon substrate. By adding the passivation layer, the passivation performance of the battery can be improved, thereby further improving the photoelectric conversion efficiency.

[0023] Optionally, the solar cell includes: an anti-reflection layer, a hole transport layer, a first passivation layer, a crystalline silicon substrate, a second passivation layer, and an electron selective contact layer stacked in sequence; wherein the crystalline silicon substrate is a p-type silicon wafer or an n-type silicon wafer.

[0024] Optionally, the solar cell includes: an anti-reflection layer, a first electron selective contact layer, a top cell, a hole transport layer, a first passivation layer, a crystalline silicon substrate, a second passivation layer, and a second electron selective contact layer stacked in sequence; wherein the crystalline silicon substrate is a p-type silicon wafer or an n-type silicon wafer.

[0025] In a second aspect of the present invention, a method for preparing the aforementioned solar cell is provided, the method comprising the steps of:

[0026] providing a crystalline silicon substrate; and

[0027] A hole transport layer is formed on the front or back side of a crystalline silicon substrate, wherein the hole transport layer is formed by: performing variable speed spin coating on a mixture of PEDOT:F and a solvent having a mass concentration ratio of 0.1:9.9 to 7:3, followed by annealing to obtain the hole transport layer, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate.

[0028] The method for preparing a solar cell of the present invention has simple steps and is easy to implement, and can obtain a solar cell with high photoelectric conversion efficiency and good stability.

[0029] Optionally, before forming the hole transport layer on the back side of the crystalline silicon substrate, the method further comprises:

[0030] Cleaning the back side of the crystalline silicon substrate with a cleaning solvent, wherein the cleaning solvent is selected from hydrofluoric acid, a mixture of hydrofluoric acid and nitric acid, a mixture of ammonia water and hydrogen peroxide, or phosphoric acid; and

[0031] Treat with UV / O3 for >10 min.

[0032] Optionally, before forming the hole transport layer on the front surface of the crystalline silicon substrate, the method further comprises: texturing the front surface of the crystalline silicon substrate to form a pyramid-like structure.

[0033] Based on the following detailed description of specific embodiments of the present invention in conjunction with the accompanying drawings, those skilled in the art will become more aware of the above and other objects, advantages and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Features, advantages, and exemplary embodiments of the present invention will be described below with reference to the accompanying drawings, in which like reference numerals refer to like elements, and in which:

[0035] Figure 1 Schematic diagram of the structure of a solar cell according to an embodiment of the present invention.

[0036] Figure 2 It is a schematic structural diagram of a solar cell according to another embodiment of the present invention.

[0037] Figure 3 It is a schematic structural diagram of a solar cell according to another embodiment of the present invention.

[0038] Figure 4 It is a schematic structural diagram of a solar cell according to another embodiment of the present invention.

[0039] Figure 5 This is the contact resistance test result diagram.

[0040] Figure 6 This is a graph of minority carrier lifetime test results.

[0041] Figure 7 This is a SEM electron microscope image of the crystalline silicon substrate plane.

[0042] Figure 8 This is a SEM electron microscope image of the crystalline silicon substrate texture.

[0043] Fig. 9 This is a graph showing battery performance test results.

[0044] Fig.10 This is a graph showing the effect of battery structure on battery performance.

[0045] Fig.11 This is a graph showing the battery performance test results of Example 2.

[0046] Fig.12 This is a diagram of the stability test results of Example 2.

[0047] Fig.13 This is the structural diagram of the back junction battery.

[0048] Fig.14 This is the structural diagram of the positive junction battery. DETAILED DESCRIPTION

[0049] The exemplary embodiments of the present invention are described in detail below with reference to the accompanying drawings. The description of the exemplary embodiments is merely exemplary and is by no means a limitation of the present invention and its application or usage. Moreover, the sizes and proportions of the components in the drawings are merely schematic and do not strictly correspond to actual products.

[0050] The present invention provides a solar cell, which includes: a crystalline silicon substrate 10 and a hole transport layer 20, the hole transport layer 20 is formed on the front or back of the crystalline silicon substrate 10, wherein the hole transport layer 20 is prepared from a mixed solution of PEDOT:F and a solvent with a mass concentration ratio of 0.1:9.9 to 7:3, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate. The solar cell of an embodiment of the present invention includes a crystalline silicon substrate 10 and a hole transport layer 20, the hole transport layer 20 is formed on the front or back of the crystalline silicon substrate 10, and the hole transport layer 20 is set to be prepared from a mixed solution of PEDOT:F and a solvent with a mass concentration ratio of 0.1:9.9 to 7:3, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate, so that the solar cell has high photoelectric conversion efficiency and good stability.

[0051] The present invention also provides a method for preparing the aforementioned solar cell, the method comprising the steps of:

[0052] providing a crystalline silicon substrate 10; and

[0053] A hole transport layer 20 is formed on the front or back side of the crystalline silicon substrate 10, wherein the hole transport layer 20 is formed by: performing variable speed spin coating on a mixture of PEDOT:F and a solvent having a mass concentration ratio of 0.1:9.9 to 7:3, followed by annealing to obtain the hole transport layer 20, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate.

[0054] The method for preparing a solar cell according to the embodiment of the present invention has simple steps and is easy to implement, and can obtain a solar cell with high photoelectric conversion efficiency and good stability.

[0055] In this article, "solar cell" and "battery" can be used interchangeably. In this article, "hole transport layer" and "PEDOT:F film" can be used interchangeably. As mentioned above, the hole transport layer 20 can be formed on the front or back of the crystalline silicon substrate 10. In this article, for the convenience of description, the solar cell in which the hole transport layer 20 is formed on the back of the crystalline silicon substrate 10 is referred to as a "back junction cell"; the solar cell in which the hole transport layer 20 is formed on the front of the crystalline silicon substrate 10 is referred to as a "front junction cell".

[0056] The Chinese name of PEDOT:F is poly(3,4-ethylenedioxythiophene):perfluorosulfonic acid ion polymer. In the present invention, the PEDOT:F used can be a commercially available product, such as a commercially available product of Feiyimande Technology Co., Ltd.

[0057] The current heterojunction technology (HJT) uses amorphous silicon (a-Si) as the hole transport layer 20 material, which has a low hole mobility (~10 -4 cm 2 / Vs) is one of the reasons why its photoelectric conversion efficiency cannot be further improved. The inventors found that PEDOT:F film has a high hole mobility of 0.02cm 2 / Vs, the work function is 5.6eV, which is beneficial to improve the photoelectric conversion efficiency and stability of the battery. In addition, experiments show that the PEDOT:F film has a transmittance of more than 95%, making the PEDOT:F film suitable for use in PEDOT:F positive junction batteries. When the PEDOT:F film is on the polished surface of crystalline silicon, the square resistance is 1.15kΩ / □, the resistivity is 0.11Ω.mm, and the conductivity is 8.6S / cm; when the PEDOT:F film is on the velvet surface of crystalline silicon, the square resistance is 21.95kΩ / □, the resistivity is 2.2Ω.mm, and the conductivity is 4.68S / cm.

[0058] In some embodiments, the mixed solution is subjected to variable speed spin coating and annealing to obtain the hole transport layer 20. By using variable speed spin coating and annealing, a PEDOT:F film with suitable thickness, contact resistance, minority carrier lifetime, etc. can be obtained.

[0059] Variable speed spin coating is usually performed by first slow and then fast spin coating. That is, in the variable speed spin coating process, first, slow spin coating is used to evenly disperse the PEDOT:F-solvent solution on the surface of the battery cell, and then fast spin coating is used to obtain a PEDOT:F film of a specific thickness. Among them, the rotation speed of slow spin coating can be 10-1000rmp, such as 10rmp, 100rmp, 300rmp, 500rmp, 800rmp, 1000rmp, and the time can be 1-10s, such as 1s, 3s, 5s, 7s, 10s; the rotation speed of fast spin coating can be 3400-3600rmp, such as 3400rmp, 3500rmp, 3600rmp, and the time is >30s, such as 31s, 40s, 50s. The variable speed spin coating process can be carried out in an air atmosphere. For example, in an air atmosphere, the coating is first performed at 1500 rpm for 5 seconds and then at 3500 rpm for 35 seconds.

[0060] The specific annealing temperature, time, atmosphere, etc. of the annealing treatment can be determined according to the parameters such as the specific contact resistance and minority carrier lifetime of the PEDOT:F film to be obtained. Generally, the annealing treatment can be annealing for >10min at a temperature of <150°C. For example, the annealing temperature can be 145°C, 140°C, 130°C, 125°C, and the annealing time can be 12min, 15min, 18min, 20min. The annealing treatment can be carried out in an air atmosphere, or an inert gas atmosphere such as nitrogen and argon. For example, annealing is performed at a temperature of 130°C for 15min in an air atmosphere.

[0061] The thickness of the hole transport layer 20 affects the contact resistance, minority carrier lifetime, etc. The thickness of the hole transport layer 20 can be 4-50nm. For example, the thickness of the hole transport layer 20 can be 4nm, 10nm, 18.4nm, 20nm, 30nm, 40nm, 50nm. Herein, the thickness of the hole transport layer 20 is the thickness obtained after spin coating and annealing.

[0062] In a preferred embodiment, the hole transport layer 20 is obtained by spin coating and annealing a mixture of PEDOT:F and ethanol with a mass concentration ratio of 4:10, and the thickness of the hole transport layer 20 is about 18.4-20nm. Experiments show that the hole transport layer 20 prepared under the above conditions has low contact resistance, long minority carrier lifetime, and high photoelectric conversion efficiency.

[0063] In some embodiments, the hole transport layer 20 is formed on the back side of the crystalline silicon substrate 10, and the hole transport layer 20 directly contacts the crystalline silicon substrate 10. Figure 1 In another embodiment, the hole transport layer 20 is formed on the back side of the crystalline silicon substrate 10, and a p-type passivation material layer 30 is provided between the hole transport layer 20 and the crystalline silicon substrate 10, wherein the p-type passivation material layer 30 is selected from an aluminum oxide layer, a silicon oxide layer, a P-doped silicon oxide layer, or a titanium oxide layer, Figure 2 . By adding a p-type passivation material layer 30, surface recombination can be effectively reduced and the photoelectric conversion efficiency can be improved. The p-type passivation material layer 30 can be an aluminum oxide layer, a silicon oxide layer, a P-doped silicon oxide layer, a titanium oxide layer, etc. For example, the p-type passivation material layer 30 is an aluminum oxide layer. In particular, the aluminum oxide layer can be an aluminum oxide layer prepared by thermal oxidation, referred to herein as "thermal oxidation aluminum oxide layer"; the aluminum oxide layer can also be an aluminum oxide layer prepared by PE-ALD, referred to herein as "PE-ALD aluminum oxide layer". The aluminum oxide layer is preferably an aluminum oxide layer prepared by PE-ALD. Experiments show that the use of PE-ALD aluminum oxide layer has better battery performance and device efficiency.

[0064] When the hole transport layer 20 is formed on the back side of the crystalline silicon substrate 10, before the hole transport layer 20 is formed on the back side of the crystalline silicon substrate 10, the back side of the crystalline silicon substrate 10 is cleaned with a cleaning solvent, wherein the cleaning solvent is selected from hydrofluoric acid, a mixture of hydrofluoric acid and nitric acid, a mixture of ammonia water and hydrogen peroxide, or phosphoric acid. By cleaning the back side of the crystalline silicon substrate 10 with a cleaning solvent, the oxide layer can be effectively removed. The cleaning solvent is usually a relatively low concentration of hydrofluoric acid, such as 1%-10% HF, and the relatively low concentration of hydrofluoric acid can effectively clean the silicon oxide naturally formed on the surface of the crystalline silicon substrate 10, facilitating the subsequent addition of a passivation material layer 30 for p-type such as aluminum oxide, while reducing damage to the crystalline silicon substrate 10.

[0065] In addition, after cleaning the back side of the crystalline silicon substrate 10, UV / O3 treatment is performed for >10 min, and then a hole transport layer 20 is formed on the back side of the crystalline silicon substrate 10. By continuing to perform treatment with UV / O3, a strong oxidation environment can be constructed to remove impurities on the surface of the crystalline silicon substrate 10. The time of UV / O3 treatment can be set according to the desired effect, for example, the UV / O3 treatment time can be generally >10 min, for example, 10 min, 15 min, 20 min.

[0066] In some embodiments, the hole transport layer 20 is formed on the front side of the crystalline silicon substrate 10, and the hole transport layer 20 directly contacts the crystalline silicon substrate 10. In other embodiments, the hole transport layer 20 is formed on the front side of the crystalline silicon substrate 10, and a passivation layer is provided between the hole transport layer 20 and the crystalline silicon substrate 10. For a positive junction cell, there is usually a first passivation layer 51 between the hole transport layer 20 and the crystalline silicon substrate 10, and a second passivation layer 52 between the crystalline silicon substrate 10 and the electron selective contact layer 70. PEDOT:F can be directly spin-coated on the front side of the crystalline silicon velvet as a hole selective contact material, and has excellent coating. However, in order to improve the passivation performance of the cell, thereby further improving the photoelectric conversion efficiency, it is preferred that a passivation layer is deposited on the front side of the crystalline silicon substrate 10. The material types and preparation methods of the passivation layer can adopt the material types and preparation methods in the prior art. For example, the material types of the passivation layer can be silicon oxide, amorphous silicon, aluminum oxide, etc. The silicon oxide layer can be prepared by exposing the silicon wafer to oxygen at high temperature for thermal oxidation or chemical vapor deposition CVD, and amorphous silicon can be prepared by plasma enhanced chemical vapor deposition PE-CVD.

[0067] When the hole transport layer 20 is formed on the front surface of the crystalline silicon substrate 10 , the front surface of the crystalline silicon substrate 10 is textured before the hole transport layer 20 is formed on the front surface of the crystalline silicon substrate 10 to form a pyramid-like structure.

[0068] Reference below Figure 1 and Figure 2 The optimized structure of the back-junction battery is described in detail.

[0069] Figure 1 Schematic diagram of the structure of a back junction cell of an embodiment, wherein the hole transport layer 20 is formed on the back side of the crystalline silicon substrate 10, and the hole transport layer 20 directly contacts the crystalline silicon substrate 10. Figure 1 The solar cell may include: an anti-reflection layer 60, a passivation layer 50, a crystalline silicon substrate 10, and a hole transport layer 20 stacked in sequence. The solar cell may also include a metal electrode 40, wherein the metal electrode 40 may be a silver electrode.

[0070] Figure 2 is a schematic structural diagram of a back-junction cell of another embodiment, wherein a hole transport layer 20 is formed on the back of a crystalline silicon substrate 10, and a p-type passivation material layer 30 is provided between the hole transport layer 20 and the crystalline silicon substrate 10. Figure 2 The solar cell may include: an anti-reflection layer 60, a passivation layer 50, a crystalline silicon substrate 10, a p-type passivation material layer 30, and a hole transport layer 20, which are stacked in sequence. The solar cell may also include a metal electrode 40, wherein the metal electrode 40 may be a silver electrode.

[0071] The material type and preparation method of the anti-reflection layer 60 can adopt the material type and preparation method in the prior art. For example, the material type of the anti-reflection layer 60 can be silicon nitride, titanium oxide, etc. The silicon nitride layer can be prepared by plasma enhanced chemical vapor deposition PE-CVD, and the titanium oxide layer can be prepared by atomic layer deposition ALD or sol-gel method.

[0072] As mentioned above, the material type and preparation method of the passivation layer 50 can adopt the material type and preparation method in the prior art. For example, the material type of the passivation layer 50 can be silicon oxide, amorphous silicon, aluminum oxide, etc.

[0073] As described above, the hole transport layer 20 is prepared from a mixture of PEDOT:F and a solvent with a mass concentration ratio of 0.1:9.9 to 7:3, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate.

[0074] As mentioned above, the p-type passivation material layer 30 may be an aluminum oxide layer, a silicon oxide layer, a P-doped silicon oxide layer, a titanium oxide layer, or the like.

[0075] In a preferred embodiment, the solar cell may include:

[0076] An anti-reflection layer 60, wherein the anti-reflection layer 60 is a silicon nitride layer with a thickness of 50-80 nm, or the anti-reflection layer 60 is a titanium oxide layer with a thickness of 50-100 nm;

[0077] A passivation layer 50, wherein the passivation layer 50 is a silicon oxide layer and has a thickness of 1-10 nm;

[0078] A crystalline silicon substrate 10, wherein the crystalline silicon substrate 10 is a p-type silicon wafer;

[0079] A p-type passivation material layer 30, wherein the p-type passivation material layer 30 is a PE-ALD aluminum oxide layer and has a thickness of 1.10-1.15 nm; and

[0080] A hole transport layer 20, wherein the hole transport layer 20 is prepared from a mixture of PEDOT:F and ethanol in a mass concentration ratio of 4:10 and has a thickness of 18.4-20 nm;

[0081] The solar cell may further include a metal electrode 40 , wherein the metal electrode 40 may be a silver electrode.

[0082] When the anti-reflection layer 60 is a silicon nitride layer, the thickness of the silicon nitride layer can be 50-80nm, for example, 50nm, 60nm, 70nm, 80nm, and is prepared by plasma enhanced chemical vapor deposition PE-CVD. When the anti-reflection layer 60 is a titanium oxide layer, the thickness of the titanium oxide layer can be 50-100nm, for example, 50nm, 60nm, 70nm, 80nm, 100nm, and is prepared by atomic layer deposition ALD or sol-gel method. The passivation layer 50 can be a silicon oxide layer with a thickness of 1-10nm, for example, 1nm, 1.16nm, 4nm, 8nm, 10nm. The p-type passivation material layer 30 can be a PE-ALD aluminum oxide layer with a thickness of 1.10-1.15nm, for example, 1.10nm, 1.13nm, 1.15nm, and is prepared by exposing the silicon wafer to oxygen at high temperature for thermal oxidation or chemical vapor deposition CVD. Experiments show that the photoelectric conversion efficiency of the solar cell manufactured by the above method and structure can be as high as 21.8%, and the stability is good.

[0083] Reference below Figure 3 and Figure 4 The optimized structure of the positive junction battery is described in detail.

[0084] Figure 3The present invention is a schematic structural diagram of a positive junction cell of an embodiment, wherein the solar cell includes: an anti-reflection layer 60, a hole transport layer 20, a first passivation layer 51, a crystalline silicon substrate 10, a second passivation layer 52, and an electron selective contact layer 70 which are stacked in sequence; wherein the crystalline silicon substrate 10 is a p-type silicon wafer or an n-type silicon wafer; the solar cell may also include a metal electrode 40, wherein the metal electrode 40 may be a silver electrode.

[0085] Figure 4 It is a schematic structural diagram of a positive junction cell of another embodiment, wherein the solar cell includes the following stacked in sequence: an anti-reflection layer 60, a first electron selective contact layer 71, a top cell 80, a hole transport layer 20, a first passivation layer 51, a crystalline silicon substrate 10, a second passivation layer 52, and a second electron selective contact layer 72; wherein the crystalline silicon substrate 10 is a p-type silicon wafer or an n-type silicon wafer; the solar cell may also include a metal electrode 40, wherein the metal electrode 40 may be a silver electrode.

[0086] As mentioned above, the material type and preparation method of the anti-reflection layer 60 can adopt the material type and preparation method in the prior art. For example, the material type of the anti-reflection layer 60 can be silicon nitride, titanium oxide, etc.

[0087] The material types and preparation methods of the electron selective contact layer 70, the first electron selective contact layer 71, and the second electron selective contact layer 72 can adopt the material types and preparation methods in the prior art. For example, the material types of the electron selective contact layer 70, the first electron selective contact layer 71, and the second electron selective contact layer 72 can be transition metal oxides, such as TiOx, WOx, ZnO, etc. The transition metal oxide layer can be prepared by atomic layer deposition ALD or solution treatment such as sol-gel method. The electron selective contact layer 70 can be a transition metal oxide with a thickness of 10-50nm. The first electron selective contact layer 71 can be a transition metal oxide with a thickness of 10-50nm, for example, 10nm, 20nm, 30nm, 40nm, 50nm. The second electron selective contact layer 72 can be a transition metal oxide with a thickness of 10-50nm, for example, 10nm, 20nm, 30nm, 40nm, 50nm.

[0088] The material type and preparation method of the top battery 80 can adopt the material type and preparation method in the prior art. For example, the material type of the top battery 80 can be perovskite, OPV, gallium arsenide, CIGS, etc.

[0089] As described above, the hole transport layer 20 is prepared from a mixture of PEDOT:F and a solvent with a mass concentration ratio of 0.1:9.9 to 7:3, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate.

[0090] The material types and preparation methods of the first passivation layer 51 and the second passivation layer 52 can adopt the material types and preparation methods in the prior art. For example, the material types of the first passivation layer 51 and the second passivation layer 52 can be silicon oxide, amorphous silicon, aluminum oxide, etc. The silicon oxide layer can be prepared by exposing the silicon wafer to oxygen at high temperature for thermal oxidation or chemical vapor deposition CVD, and the amorphous silicon can be prepared by plasma enhanced chemical vapor deposition PE-CVD. In some embodiments, the first passivation layer 51 can be a silicon oxide layer with a thickness of 1-5nm, for example, 1nm, 2nm, 3nm, 4nm, 5nm. The first passivation layer 51 can also be an amorphous silicon layer with a thickness of 1-5nm, for example, 1nm, 2nm, 3nm, 4nm, 5nm. The second passivation layer 52 can be a silicon oxide layer with a thickness of 1-5nm, for example, 1nm, 2nm, 3nm, 4nm, 5nm. The second passivation layer 52 may also be an amorphous silicon layer with a thickness of 1-5 nm, for example, 1 nm, 2 nm, 3 nm, 4 nm, or 5 nm.

[0091] The present invention introduces the PEDOT:F material into the crystalline silicon battery system for the first time, and optimizes the materials (including solvents, concentration ratios, etc.), processes (spin coating, annealing, etc.), and battery structure of the PEDOT:F material, thereby obtaining an organic crystalline silicon battery with a photoelectric conversion efficiency of up to 21.8%.

[0092] The contact resistance and the implicit open circuit voltage (iV oc ), minority carrier lifetime, morphology, stability, external quantum efficiency (EQE), open circuit voltage (V oc ), fill factor (FF), short circuit current (I sc ), short-circuit current density (J sc ), photoelectric conversion efficiency (PCE), etc.

[0093] Example 1

[0094] The following steps were used for sample preparation:

[0095] 1) Clean the silicon wafer (e.g., p-type silicon wafer) with 5% HF to remove SiOx on the surface;

[0096] 2) treating with UV / O3 for 15 minutes to obtain a treated crystalline silicon substrate 10;

[0097] 3) Spin coating a mixture of PEDOT:F and ethanol with different mass concentration ratios at variable speeds, specifically, first spin coating at 1500 rpm for 5 seconds, and then spin coating at 3500 rpm for 35 seconds;

[0098] 4) Annealing at 130° C. for 15 min to form a PEDOT:F film on the crystalline silicon substrate 10 .

[0099] 1. Thickness of PEDOT:F films obtained with different PEDOT:F / ethanol mass concentration ratios The thickness of PEDOT:F films obtained with different PEDOT:F / ethanol mass concentration ratios are shown in Table 1.

[0100] Table 1

[0101]

[0102] 2. The influence of the passivation material layer for p-type on the contact resistance

[0103] 1) A PEDOT:F film is directly covered on a p-type silicon wafer and a silver electrode is provided to obtain a p-Si / PEDOT:F / Ag structure.

[0104] 2) A PEDOT:F film and a p-type passivation material layer 30 (aluminum oxide Al2O3 in this embodiment) are sequentially covered on a p-type silicon wafer, and a silver electrode is provided to obtain a p-Si / Al2O3 / PEDOT:F / Ag structure.

[0105] The contact resistance tests of the above two structures were carried out respectively. The test results are shown in Figure 5 .from Figure 5 It can be seen that when the PEDOT:F / ethanol mass concentration ratio is 4:10, the contact resistance is the smallest, and the contact resistance of the structure with aluminum oxide is smaller than the contact resistance of the structure without aluminum oxide.

[0106] 3. Effect of annealing treatment on passivation contact effect

[0107] A mixture of PEDOT:F and ethanol (PEDOT:F / ethanol mass concentration ratio of 4:10) was spin-coated on the front and back of a p-type silicon wafer, and the minority carrier lifetimes before and after annealing were compared. The test results are shown in Figure 6 .from Figure 6 It can be seen that after annealing, the implicit open circuit voltage iV oc Increased, minority carrier lifetime decreased.

[0108] 4. Effect of PEDOT:F film on morphology

[0109] The flat surface and the velvet surface of the crystalline silicon substrate 10 are covered with a PEDOT:F film (wherein the mass concentration ratio of PEDOT:F / ethanol is 4:10), and the obtained SEM electron microscope image is shown in FIG. Figure 7 and Figure 8 .

[0110] Figure 7In the figure, a) is the SEM electron microscope image of the original crystalline silicon substrate plane, b) is the SEM electron microscope image of the PEDOT:F film + crystalline silicon substrate plane, and c) is Figure 7 b) A partial enlarged view.

[0111] Figure 8 In the figure, a) is the SEM electron microscope image of the original crystalline silicon substrate texture, b) is the SEM electron microscope image of the PEDOT:F film + crystalline silicon substrate texture, and c) is a local enlarged image of b).

[0112] from Figure 7 and Figure 8 As can be seen from the figure, the PEDOT:F film has good velvet conformality, so that the PEDOT:F film can be used in positive junction batteries, especially in Figure 4 In the cell shown, the cell includes the following layers stacked in sequence: an anti-reflection layer 60, a first electron selective contact layer 71, a top cell 80, a hole transport layer 20, a first passivation layer 51, a crystalline silicon substrate 10, a second passivation layer 52, and a second electron selective contact layer 72; the cell also includes a silver electrode.

[0113] 5. Effect of PEDOT:F / ethanol mass concentration ratio on battery performance parameter test

[0114] based on Figure 2 The battery structure includes: silicon nitride anti-reflection layer 60, silicon oxide passivation layer 50, p-type silicon wafer crystalline silicon substrate 10, PE-ALD aluminum oxide, hole transport layer 20, which are stacked in sequence; through the aforementioned cleaning treatment, UV / O3 treatment, variable speed spin coating treatment and annealing treatment, and evaporation of Ag electrode. Among them, PEDOT: F film is made of PEDOT: F / ethanol with different mass concentration ratios. The battery performance parameter test results are shown in Fig. 9 .from Fig. 9 It can be seen that the battery performance is best when the PEDOT:F / ethanol mass concentration ratio is 4:10, V oc :0.631V;FF:81.3%;J sc :38.1mA / cm 2 ; PCE: 19.5%.

[0115] 6. Impact of battery structure on battery performance

[0116] The experimental subjects include: conventional batteries without PEDOT:F film ( Fig.10 denoted by p-Si / Ag in the figure), batteries containing PEDOT:F thin films (see Figure 1 , Fig.10) and a battery containing a PEDOT:F film and a p-type passivation material layer 30 (aluminum oxide Al2O3 in this embodiment) (see Figure 2 , Fig.10 denoted by p-Si / Al2O3 / PEDOT:F / Ag).

[0117] Fig.10 In the equation, a) is J sc and V oc Figure 2. (b) shows EQE and J sc The graph shows the change of wavelength, and the corresponding V of the three structures is also recorded in the graph oc , FF, J sc , PCE. Fig.10 It can be seen that the battery containing the PEDOT:F film and the p-type passivation material layer 30 has the best performance, and the battery containing the PEDOT:F film is second.

[0118] Example 2

[0119] In this embodiment, the battery has Figure 2 The structure shown, i.e., the battery includes the following stacked layers: a silicon nitride anti-reflection layer 60 with a thickness of about 70 nm, a silicon oxide passivation layer 50 with a thickness of about 1.16 nm, a p-type silicon wafer crystalline silicon substrate 10, a PE-ALD aluminum oxide layer with a thickness of about 1.13 nm (as a p-type passivation material layer 30), and a hole transport layer 20 (wherein the mass concentration ratio of PEDOT:F / ethanol is 4:10, and the thickness is about 20 nm).

[0120] The preparation process includes: 1) cleaning the p-type silicon wafer with 5% HF; 2) treating with UV / O3 for 15 minutes; 3) preparing aluminum oxide with a thickness of about 1.13nm by PE-ALD method; 4) spin coating a mixture of PEDOT:F and ethanol with a mass concentration ratio of 4:10 at variable speeds, first at 1500rmp for 5s, and then at 3500rmp for 35s; 5) annealing at 130°C for 15 minutes; 6) evaporating an Ag electrode with a thickness of about 300nm.

[0121] The battery performance test was carried out on the battery, and the results are shown in Fig.11 , V oc :0.655V;FF:83.8%;J sc :39.7mA / cm 2 ; PCE: 21.8%.

[0122] The stability test of the battery is shown in Fig.12 . Fig.12 In the figure, a) is the PCE and storage time diagram, and b) is the V corresponding to the three structures.oc ,,J sc , FF and storage time diagram. Fig.12 As can be seen from the figure, the PCE of the device exposed to air (i.e., not encapsulated) dropped from 21.8% to 16.2% after 30 days of standing. oc From 655mV to 635mV; J sc From 39.7mA / cm 2 Down to 38.1mA / cm 2 ; FF dropped from 83.8% to 66.8%. If there is good packaging, the stability can be further improved.

[0123] Example 3

[0124] In this embodiment, the battery has Figure 1 The structure shown, i.e., the battery includes: a silicon nitride anti-reflection layer 60 with a thickness of about 70 nm, a silicon oxide passivation layer 50 with a thickness of about 1.16 nm, a p-type silicon wafer crystalline silicon substrate 10, and a hole transport layer 20, which are stacked in sequence. The cleaning treatment, UV / O3 treatment, variable speed spin coating treatment and annealing treatment in Example 1 are carried out, and the Ag electrode is evaporated. Among them, the PEDOT:F film is prepared with PEDOT:F / ethanol of different mass concentration ratios. The battery performance parameter test results are shown in Table 2.

[0125] Table 2

[0126]

[0127] It can be seen from Table 2 that the battery performance is best when the PEDOT:F / ethanol mass concentration ratio is 4:10.

[0128] Example 4

[0129] In this embodiment, the battery has Figure 2 The structure shown, i.e., the cell includes the following stacked layers: a silicon nitride anti-reflection layer 60 with a thickness of about 70 nm, a silicon oxide passivation layer 50 with a thickness of about 1.16 nm, a p-type silicon wafer crystalline silicon substrate 10, an aluminum oxide layer, and a hole transport layer 20 (wherein the mass concentration ratio of PEDOT:F / ethanol is 4:10, and the thickness is about 20 nm). The aluminum oxide layer is a thermal oxidized aluminum oxide layer, or the aluminum oxide layer is a PE-ALD aluminum oxide layer. The test results of the cell performance parameters are shown in Table 3.

[0130] Table 3

[0131]

[0132] It can be seen from Table 3 that the effect of using PE-ALD aluminum oxide as the p-type passivation material layer 30 is better than the effect of using thermal oxidized aluminum oxide layer as the p-type passivation material layer 30 .

[0133] Example 5

[0134] In this embodiment, the battery is similar to that in Embodiment 2, except that the solvent used in the PEDOT:F mixed solution is methanol.

[0135] Example 6

[0136] In this embodiment, the battery is similar to that in Embodiment 2, except that the solvent used in the PEDOT:F mixed solution is isopropanol.

[0137] Example 7

[0138] In this embodiment, the battery is similar to that in Embodiment 2, except that the solvent used in the PEDOT:F mixed solution is acetone.

[0139] Example 8

[0140] In this embodiment, the battery is similar to that in Embodiment 2, except that the solvent used in the PEDOT:F mixed solution is n-butanol.

[0141] Example 9

[0142] In this embodiment, the battery is similar to that in Embodiment 2, except that the solvent used in the PEDOT:F mixed solution is ethyl acetate.

[0143] Example 10

[0144] In this embodiment, the battery is similar to that in Embodiment 2, the only difference is that the mass concentration ratio of PEDOT:F to ethanol is 0.1:9.9; the thickness of the silicon nitride anti-reflection layer 60 is 50 nm; and the thickness of the silicon oxide passivation layer 50 is 10 nm.

[0145] Embodiment 11

[0146] In this embodiment, the battery is similar to that in Embodiment 2, the only difference is that the mass concentration ratio of PEDOT:F to ethanol is 7:3; the thickness of the silicon nitride anti-reflection layer 60 is 80 nm; and the thickness of the silicon oxide passivation layer 50 is 1 nm.

[0147] Example 12

[0148] In this embodiment, the battery is similar to that in embodiment 2, the only difference is that the variable speed spin coating is firstly 10 rpm for 10 s and then 3400 rpm for 40 s; the annealing treatment is annealing at 140° C. for 20 min.

[0149] Embodiment 13

[0150] In this embodiment, the battery is similar to that in Embodiment 2, the only difference is that the variable speed spin coating is firstly 1000 rpm for 1 second and then 3600 rpm for 50 seconds; and the annealing treatment is annealing at 120° C. for 25 minutes.

[0151] Embodiment 14

[0152] In this embodiment, the battery is similar to that in Embodiment 2, except that the p-type passivation material layer 30 is a silicon oxide layer.

[0153] Embodiment 15

[0154] In this embodiment, the battery is similar to that in Embodiment 2, except that the p-type passivation material layer 30 is a P-doped silicon oxide layer.

[0155] Example 16

[0156] In this embodiment, the battery is similar to that in Embodiment 2, except that the p-type passivation material layer 30 is a titanium oxide layer.

[0157] Embodiment 17

[0158] In this embodiment, the battery structure is shown in Figure 3 , including: an anti-reflection layer 60, a hole transport layer 20, a first passivation layer 51, a crystalline silicon substrate 10, a second passivation layer 52, and an electron selective contact layer 70 stacked in sequence; the battery also includes a silver electrode, wherein the crystalline silicon substrate 10 is an n-type silicon wafer, the anti-reflection layer 60 is titanium oxide, the hole transport layer 20 is a PEDOT:F film prepared from a mixed solution of PEDOT:F and a solvent with a mass concentration ratio of 4:10, the first passivation layer 51 and the second passivation layer 52 are amorphous silicon, and the electron selective contact layer 70 is TiOx.

[0159] Embodiment 18

[0160] In this embodiment, the battery structure is shown in Figure 4 , including: an anti-reflection layer 60, a first electron selective contact layer 71, a top battery 80, a hole transport layer 20, a first passivation layer 51, a crystalline silicon substrate 10, a second passivation layer 52, and a second electron selective contact layer 72, which are stacked in sequence; the battery also includes a silver electrode, wherein the crystalline silicon substrate 10 is a p-type silicon wafer, the anti-reflection layer 60 is silicon nitride, the hole transport layer 20 is a PEDOT:F film prepared from a mixed solution of PEDOT:F and a solvent with a mass concentration ratio of 4:10, the first passivation layer 51 and the second passivation layer 52 are aluminum oxide, the top battery 80 is OPV, and the first electron selective contact layer 71 and the second electron selective contact layer 72 are ZnO.

[0161] Embodiment 19

[0162] Fig.13 The structure diagram of the back-junction battery (a) and the corresponding battery performance parameters (b) are shown. In Figure b), the structure without aluminum oxide is represented by PEDOT:F, and the structure with aluminum oxide as the p-type passivation material layer 30 is represented by Al2O3 / PEDOT:F. The battery performance parameter test results of these two batteries are shown in Table 4.

[0163] Table 4

[0164]

[0165]

[0166] It can be seen from Table 4 that when only the PEDOT:F film is provided, the PCE reaches 22.2%; when the aluminum oxide layer and the PEDOT:F film are provided at the same time, the PCE reaches 23.7%.

[0167] Embodiment 20

[0168] Fig.14 The structure diagram of the positive junction battery (also called PEDOT-HJT battery) (a) and the corresponding battery performance parameters (b) are shown. In Figure b), a is V oc and hole mobility diagram, b is FF and hole mobility diagram, c is J sc and hole mobility, d is the PCE and hole mobility diagram. Fig.14 It can be seen that the PCE reaches 27.5%.

[0169] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "an example", "some embodiments", or "preferred embodiment" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0170] The embodiments of the present invention are described in detail above. However, aspects of the present invention are not limited to the above embodiments. Various modifications and substitutions may be applied to the above embodiments without departing from the scope of the present invention.

Claims

1. A solar cell, wherein: The solar cell comprises: a crystalline silicon substrate and a hole transport layer, wherein the hole transport layer is formed on the front side or the back side of the crystalline silicon substrate, wherein the hole transport layer is prepared from a mixed solution of PEDOT:F and a solvent with a mass concentration ratio of 0.1:9.9 to 7:3, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate.

2. The solar cell according to claim 1, wherein: The mixed solution is subjected to variable speed spin coating and annealing treatment to obtain the hole transport layer.

3. The solar cell according to claim 2, wherein: The variable speed spin coating is firstly spin coating at 10-1000 rpm for 1-10 s, and then spin coating at 3400-3600 rpm for more than 30 s; and / or The annealing treatment is performed at a temperature of <150°C for >10 min; and / or The thickness of the hole transport layer is 4-50 nm.

4. The solar cell according to any one of claims 1 to 3, wherein: The hole transport layer is prepared from a mixed solution of PEDOT:F and ethanol with a mass concentration ratio of 4:10, and the thickness of the hole transport layer is 18.4-20 nm.

5. The solar cell according to any one of claims 1 to 3, wherein: The hole transport layer is formed on the back side of the crystalline silicon substrate, and the hole transport layer directly contacts the crystalline silicon substrate; or The hole transport layer is formed on the back side of the crystalline silicon substrate, and a p-type passivation material layer is provided between the hole transport layer and the crystalline silicon substrate, wherein the p-type passivation material layer is selected from an aluminum oxide layer, a silicon oxide layer, a P-doped silicon oxide layer, or a titanium oxide layer.

6. The solar cell according to claim 5, wherein: Before forming the hole transport layer on the back side of the crystalline silicon substrate, the back side of the crystalline silicon substrate is cleaned with a cleaning solvent, wherein the cleaning solvent is selected from hydrofluoric acid, a mixture of hydrofluoric acid and nitric acid, a mixture of ammonia water and hydrogen peroxide, or phosphoric acid.

7. The solar cell according to claim 6, wherein: After cleaning the back side of the crystalline silicon substrate, UV / O3 treatment is performed for >10 min, and then the hole transport layer is formed on the back side of the crystalline silicon substrate.

8. The solar cell according to claim 5, wherein: The solar cell comprises: An anti-reflection layer, wherein the anti-reflection layer is a silicon nitride layer with a thickness of 50-80 nm, or the anti-reflection layer is a titanium oxide layer with a thickness of 50-100 nm; A passivation layer, wherein the passivation layer is a silicon oxide layer and has a thickness of 1-10 nm; The crystalline silicon substrate, wherein the crystalline silicon substrate is a p-type silicon wafer; The p-type passivation material layer, wherein the p-type passivation material layer is a PE-ALD aluminum oxide layer and has a thickness of 1.10-1.15 nm; and The hole transport layer is prepared from a mixture of PEDOT:F and ethanol in a mass concentration ratio of 4:10 and has a thickness of 18.4-20 nm.

9. The solar cell according to any one of claims 1 to 3, The hole transport layer is formed on the front side of the crystalline silicon substrate, and the hole transport layer directly contacts the crystalline silicon substrate; or The hole transport layer is formed on the front surface of the crystalline silicon substrate, and a passivation layer is provided between the hole transport layer and the crystalline silicon substrate.

10. The solar cell according to claim 9, wherein: The solar cell comprises: an anti-reflection layer, a hole transport layer, a first passivation layer, a crystalline silicon substrate, a second passivation layer, and an electron selective contact layer which are stacked in sequence; wherein the crystalline silicon substrate is a p-type silicon wafer or an n-type silicon wafer.

11. The solar cell according to claim 9, wherein: The solar cell comprises: an anti-reflection layer, a first electron selective contact layer, a top cell, the hole transport layer, a first passivation layer, the crystalline silicon substrate, a second passivation layer, and a second electron selective contact layer, which are stacked in sequence; wherein the crystalline silicon substrate is a p-type silicon wafer or an n-type silicon wafer.

12. A method for preparing a solar cell according to any one of claims 1 to 11, the method comprising the steps of: providing a crystalline silicon substrate; and A hole transport layer is formed on the front or back side of the crystalline silicon substrate, wherein: The step of forming the hole transport layer is: performing variable speed spin coating on a mixture of PEDOT:F and a solvent with a mass concentration ratio of 0.1:9.9 to 7:3, followed by annealing to obtain the hole transport layer, wherein the solvent is selected from at least one of ethanol, methanol, isopropanol, acetone, n-butanol, or ethyl acetate.

13. The method according to claim 12, before forming the hole transport layer on the back side of the crystalline silicon substrate, the method further comprises: Cleaning the back side of the crystalline silicon substrate with a cleaning solvent, wherein the cleaning solvent is selected from hydrofluoric acid, a mixture of hydrofluoric acid and nitric acid, a mixture of ammonia water and hydrogen peroxide, or phosphoric acid; and Treat with UV / O3 for >10 min.

14. The method according to claim 12, before forming the hole transport layer on the front surface of the crystalline silicon substrate, the method further comprises: The front surface of the crystalline silicon substrate is textured to form a pyramid-like structure.