Memristor and preparation method thereof, chip and electronic equipment

By using a combination of copper indium phosphorus sulfide (CIPS) materials and electrodes with different work functions in memristors, the problem of creeping current in memristor arrays is solved, achieving high rectification ratio and high resistive switching ratio, simplifying the process and reducing costs, making it suitable for highly integrated applications.

CN119031827APending Publication Date: 2024-11-26WUHAN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411046110.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing memristor cross arrays suffer from creeping current issues, leading to incorrect readings of device resistance states and high power consumption, hindering large-scale applications. Furthermore, existing solutions are complex in process, costly, and have low integration.

Method used

Copper indium phosphorus sulfide (CuInP2S6) is used as the resistive layer material. Combined with the first and second electrodes with different work functions, a Schottky barrier is formed, introducing self-rectification characteristics. The rectification ratio and resistive switching ratio are adjusted by controlling the proportion of copper elements, and the creeping current is avoided by utilizing the rectification characteristics of the memristor itself.

Benefits of technology

This invention achieves memristors with high rectification ratio and high resistive switching ratio, simplifies manufacturing process, reduces cost, and is suitable for highly integrated array applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031827A_ABST
    Figure CN119031827A_ABST
Patent Text Reader

Abstract

The invention discloses a memristor and a preparation method thereof, a chip and electronic equipment, and belongs to the technical field of microelectronic devices. The memristor comprises a first electrode, a resistive layer and a second electrode which are stacked. Wherein the material of the resistive layer comprises copper, indium, phosphorus and sulfur, and the atomic number ratio of the copper element to the indium element in the copper, indium, phosphorus and sulfur is greater than 0.2. The work functions of the materials of the first electrode and the second electrode are both greater than or equal to 5.0 eV, and the materials of the first electrode and the second electrode are different. According to the memristor, different high-work-function materials are selected as the first electrode and the second electrode respectively, schottky barriers are formed by the first electrode and the second electrode and resistive layer materials respectively, a self-rectification behavior is introduced, meanwhile, resistive behaviors can be introduced through ion movement and ferroelectric polarization characteristics of copper, indium, phosphorus and sulfur of the resistive layer, and the self-rectification performance of the memristor is improved by regulating and controlling the proportion of copper elements in copper, indium, phosphorus and sulfur. Therefore, the memristor obtains a high resistive switching ratio and a high rectification ratio at the same time, and the self-rectification behavior can be realized while the resistive performance is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of microelectronic devices, and in particular relates to a memristor and a preparation method thereof, a chip and an electronic device. Background Art

[0002] With the development of data-centric artificial intelligence and Internet of Things technologies, the speed and energy efficiency of current computing hardware and computing architectures cannot meet the growing demand. Among them, memristors are a key research direction in current computing hardware. However, the problem of sneak current is common in memristor crossbar arrays. The sneak current problem not only leads to incorrect reading of the device resistance state, but also interferes with the precise modulation of the resistance, and also causes high energy consumption, hindering the realization of large-scale memristor arrays. At present, the problem of sneak current is mostly solved by connecting rectifier devices, but this process is complex, the cost is high, the integration is low, and the application scenarios are limited.

[0003] Memristors with self-rectification characteristics can suppress sneak current without other auxiliary components, which can not only simplify the array structure, but also simplify the manufacturing process, reduce manufacturing costs, and facilitate the realization of highly integrated memristor arrays. Therefore, memristors with self-rectification characteristics are currently the focus of research. Summary of the invention

[0004] In order to introduce the self-rectification characteristic, the embodiment of the present application provides a memristor, which includes a first electrode, a resistive layer, and a second electrode arranged in a stacked manner. The material of the resistive layer includes copper indium phosphide, and the atomic number ratio of copper element to indium element in copper indium phosphide is greater than 0.2. The work function of the materials of the first electrode and the second electrode are both greater than or equal to 5.0 eV, and the materials of the first electrode and the second electrode are different.

[0005] In some embodiments, in the material of the resistive layer, the atomic number ratio of copper element to indium element is in the range of 0.4-1.

[0006] In some embodiments, the rectification ratio of the memristor ranges from 50 to 2000, and the resistive switching ratio of the memristor ranges from 2000 to 17000.

[0007] In some embodiments, the material of the first electrode includes at least one of palladium, platinum or gold; the material of the second electrode includes at least one of palladium, platinum or gold.

[0008] In some embodiments, the thickness of the resistive layer ranges from 7 nm to 100 nm.

[0009] In the embodiment of the present application, the memristor uses different high work function materials (work function is greater than or equal to 5.0eV) as the first electrode and the second electrode respectively, and forms a Schottky barrier with the resistive layer material respectively, so as to introduce self-rectification behavior. At the same time, the ion movement and ferroelectric polarization characteristics of the copper indium phosphide of the resistive layer can introduce resistive behavior. By adjusting the proportion of copper in the copper indium phosphide, the resistive switching ratio and rectification ratio of the memristor can also be adjusted, and self-rectification behavior can be achieved while maintaining resistive performance. The memristor cross array formed by the memristor provided by the embodiment of the present application can utilize the rectification characteristics of the memristor itself to avoid the problem of sneak current.

[0010] In a second aspect, the present application also provides a method for preparing a memristor, which specifically includes:

[0011] A first electrode, a resistive layer and a second electrode are formed in sequence. The resistive layer comprises copper indium phosphide, and the atomic number ratio of copper to indium in the copper indium phosphide is greater than 0.2. The work functions of the materials of the first electrode and the second electrode are both greater than or equal to 5 eV, and the metal materials of the first electrode and the second electrode are different.

[0012] In some embodiments, forming the resistive layer specifically includes: transferring the resistive layer to the first electrode using a mechanical stripping process.

[0013] In some embodiments, forming the resistive layer specifically includes: forming the resistive layer by a chemical vapor deposition process, and transferring the resistive layer to the first electrode.

[0014] The memristor prepared by the above preparation method has a high resistive switching ratio and rectification ratio, and can achieve self-rectification while maintaining resistive performance. The memristor cross array formed by the memristor prepared by the above preparation method can utilize the rectification characteristics of the memristor itself to avoid the problem of sneak current.

[0015] In a third aspect, an embodiment of the present application further provides a chip, the chip comprising the memristor mentioned in any embodiment of the first aspect and a packaging layer, wherein the packaging layer covers the memristor. The memristor in the chip has a high resistive switching ratio and rectification ratio, and can achieve self-rectification while maintaining resistive performance.

[0016] In a fourth aspect, an embodiment of the present application further provides an electronic device, which includes the chip and the circuit board mentioned in the third aspect, wherein the chip is electrically connected to the circuit board. The electronic device has the same technical effect as the chip mentioned in the third aspect, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0018] Figure 1a A schematic diagram of a memristor structure provided in an embodiment of the present application;

[0019] Figure 1b for Figure 1a The resistive DC IV curve of the memristor shown;

[0020] Figure 1c For voltage regulation Figure 1a The DC IV resistance curve of the memristor performance is shown;

[0021] Figure 1d For voltage amplitude and quantity control Figure 1a Dynamic curve diagram of memristor performance shown;

[0022] Figure 2a A schematic diagram of the first comparative memristor structure provided for this application;

[0023] Figure 2b for Figure 2a The resistive DC IV curve of the comparative memristor is shown;

[0024] Figure 3a A schematic diagram of the second comparative memristor structure provided in this application;

[0025] Figure 3b for Figure 3a The resistive DC IV curve of the comparative memristor is shown;

[0026] Figure 4a to Figure 4d A schematic diagram of the principle of a ferroelectric ion diode provided in an embodiment of the present application;

[0027] Figure 5a A schematic diagram of the third comparative memristor structure provided for this application;

[0028] Figure 5b for Figure 5a The resistive DC IV curve of the comparative memristor is shown;

[0029] Figure 6a A schematic diagram of the fourth comparative memristor structure provided for this application;

[0030] Figure 6b for Figure 6a The resistive DC IV curve of the comparative memristor is shown;

[0031] Figure 7a A schematic diagram of another memristor structure provided in an embodiment of the present application;

[0032] Figure 7b for Figure 7a The resistive DC IV curve of the memristor shown;

[0033] Figure 8a A schematic diagram of another memristor structure provided in an embodiment of the present application;

[0034] Figure 8b for Figure 8a The resistive DC IV curve of the memristor shown;

[0035] Figure 9a A schematic diagram of another memristor structure provided in an embodiment of the present application;

[0036] Figure 9b for Figure 9a The resistive DC IV curve of the memristor shown;

[0037] Fig.10a A schematic diagram of another memristor structure provided in an embodiment of the present application;

[0038] Fig.10b for Fig.10a The resistive DC IV curve of the memristor shown;

[0039] Fig.11 A method for preparing a memristor provided in an embodiment of the present application;

[0040] Fig.12 A schematic diagram of a chip provided in an embodiment of the present application;

[0041] Fig.13 A schematic diagram of an electronic device provided in an embodiment of the present application. DETAILED DESCRIPTION

[0042] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in some embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments provided by the present application, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present application.

[0043] Unless the context requires otherwise, throughout the specification and claims, the term "comprising" is to be construed in an open, inclusive sense, ie, meaning "including, but not limited to."

[0044] In the following, the terms "first" and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present application, unless otherwise specified, "plurality" means two or more.

[0045] When describing some embodiments, the term "connection" and its derivative expressions may be used. The term "connection" should be understood in a broad sense. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For example, when describing some embodiments, the term "connection" may be used to indicate that two or more components are in direct physical or electrical contact with each other.

[0046] Additionally, the use of “based on” is meant to be open and inclusive, as a process, step, calculation, or other action “based on” one or more stated conditions or values ​​may, in practice, be based on additional conditions or values ​​beyond those stated.

[0047] It will be understood that when a layer or element is referred to as being on another layer or substrate, it can be directly on the other layer or substrate, or intervening layers may be present between the layer or element and the other layer or substrate.

[0048] Exemplary embodiments are described herein with reference to cross-sectional views that are idealized exemplary drawings. In the drawings, the thickness of layers and the area of ​​regions are exaggerated for clarity. Therefore, variations in shape relative to the drawings due to, for example, manufacturing techniques and / or tolerances are conceivable. Therefore, the exemplary embodiments should not be interpreted as being limited to the shapes of the regions shown herein, but include deviations in shape due to, for example, manufacturing. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the actual shape of regions of the device, and are not intended to limit the scope of the exemplary embodiments.

[0049] Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.

[0050] In the relevant research on memristors, rectification ratio and resistive switching ratio are two important parameters for evaluating the performance of memristors. Rectification ratio refers to the current ratio of the memristor under forward bias and reverse bias. A higher rectification ratio means that the memristor allows a larger current to flow under forward bias, but hinders the current flow under reverse bias, showing obvious rectification behavior. Resistive switching ratio refers to the resistance ratio between the high resistance state and the low resistance state of the memristor. A higher resistive switching ratio means that the memristor can achieve a significant resistance change from the high resistance state to the low resistance state. This resistance change, that is, the resistive switching performance, is crucial for information storage and processing in memory and logic devices.

[0051] According to current research, two-dimensional van der Waals materials have shown significant advantages in building memristors with self-rectification functions. Two-dimensional van der Waals materials constitute a huge material library with rich and diverse properties, covering a wide range of electrical properties, including metallic, semiconductor (p-type, n-type and bipolar) and insulating properties, as well as tunable bandgap widths, and exhibiting a variety of properties such as multiferroic and optical properties. Therefore, by selecting two-dimensional van der Waals materials with different properties for design, diode-like behavior can be achieved, that is, rectification characteristics can be introduced.

[0052] According to relevant research, rectification capability can be obtained by constructing different two-dimensional material heterostructures and utilizing ferroelectric polarization. However, most of the devices in most of the current related research are planar structures, which often have large feature sizes (such as 8F2), which limits their application in high-density integration, and these device structures usually do not have resistive switching properties.

[0053] How to achieve self-rectification while maintaining the resistive switching performance of a single device is an urgent problem to be solved in the realization of large-scale memristor arrays.

[0054] To this end, the present application embodiment provides a memristor, such as Figure 1a As shown, Figure 1a A schematic diagram of a memristor structure provided in an embodiment of the present application. The memristor 10 is a three-layer vertical structure, including a first electrode 11, a resistive layer 12, and a second electrode 13 stacked in layers. The material of the resistive layer 12 includes copper indium phosphide, and the atomic number ratio of the copper element to the indium element in the copper indium phosphide is greater than 0.2. The work function of the materials of the first electrode 11 and the second electrode 13 are both greater than or equal to 5.0 eV, and the materials of the first electrode 11 and the second electrode 13 are different.

[0055] Copper indium phosphorus sulfur (CuInP2S6, CIPS for short) in the resistive layer 12 material is a van der Waals layered ferroelectric material. CIPS has a van der Waals layered structure, and its crystal structure is based on ABC closely packed sulfur atoms. Metal cations and phosphorus atoms fill the octahedral vacancies and have monoclinic symmetry. In the single layer material of CIPS, copper atoms, indium atoms and phosphorus atoms are arranged in a triangle, and the vertically stacked multilayer materials form a bulk material through interlayer coupling. Affected by its layered structure and material synthesis process, CIPS may have copper ion defect problems, that is, the ratio of the number of atoms of copper element to indium element is less than 1. CIPS exhibits strong ferroelectricity at room temperature, and there is a complex coupling relationship between ferroelectric polarization and ion conduction in CIPS.

[0056] In the embodiment of the present application, the first electrode 11 contacts the resistive layer 12 and forms a first Schottky barrier, and the second electrode 13 contacts the resistive layer 12 and forms a second Schottky barrier. In the resistive layer 12 material, the copper element in CIPS is one of the key factors affecting the performance of the memristor 10. CIPS has the ferroelectric polarization property of ion motion coupling, and the ferroelectric polarization reversal of ion motion coupling can occur under an applied voltage, which can modify the height of the Schottky barrier, and the change of the barrier and the movement of ions introduce resistive behavior. In a common ferroelectric medium, its polarization comes from the deviation of ions from the positive and negative charge centers, while the copper ions in the CIPS lattice can be transported over long distances. On the one hand, the movement of copper ions to the electrode surface can affect the height of the Schottky barrier. On the other hand, the movement of ions also affects the polarization degree of CIPS, and the polarization degree of CIPS further affects the height of the Schottky barrier. The ease of ion movement is related to the defect concentration of CIPS, or to the proportion of copper elements. The presence of copper ion defects can reduce the barrier of ion movement to a certain extent.

[0057] For example, in a specific embodiment, Figure 1b~1d As shown, Figure 1b for Figure 1a The resistive DC IV curve of the memristor shown in Figure 1 is: Figure 1c For voltage regulation Figure 1a The DC IV resistance curve of the memristor performance is shown in Figure 1. Figure 1d For voltage amplitude and quantity control Figure 1a Dynamic curve diagram of memristor performance shown.

[0058] In the embodiment of the present application, the first electrode 11 is a gold (Au) electrode, specifically, including a 5nm thick chromium (Cr) as an adhesion layer, and a 20nm thick gold (Au) electrode. The resistive layer 12 includes a 35nm thick copper indium phosphorus sulfur (CIPS), in which the ratio of copper element is 0.5, that is, the atomic number ratio of copper element to indium element is 0.5. The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40nm thick palladium (Pd) electrode, and a 40nm thick gold (Au) on the surface as a protective layer.

[0059] like Figure 1b As shown, the memristor 10 exhibits rectification behavior, that is, the current under the positive voltage is significantly greater than the current under the negative voltage, and its rectification ratio can reach more than 1000, about 1400. At the same time, the memristor 10 also exhibits resistive behavior, and the resistive switch can reach more than 2000, about 2300. It can be seen that the memristor 10 has a high rectification ratio and resistive switching ratio, and can achieve self-rectification while maintaining the resistive switching performance, that is, the memristor 10 simultaneously achieves simulated resistive behavior with a high rectification ratio and a high resistive switching ratio.

[0060] Further, such as Figure 1c As shown, the resistive switching ratio and rectification ratio of the memristor 10 can be adjusted by applying voltages of different magnitudes. For example, at a voltage of -4 / 4V, the resistive switching ratio of the memristor 10 is relatively large, and the rectification ratio is also relatively large, while at a voltage of -1.5 / 1.5V, the resistive switching ratio of the memristor 10 is relatively small, and the rectification ratio is also relatively small.

[0061] Further, such as Figure 1d As shown, the number and amplitude of the applied pulses can be gradually adjusted to achieve simulated resistive behavior and adjustable resistance state. For example, taking the pulse with the horizontal axis of 0.1s as an example, the voltage amplitude increases from 3V to 7V from bottom to top, and it can be seen that the resistance state of the memristor 10 is different under different voltage amplitudes. Alternatively, taking the same voltage amplitude, such as 7V, as the number of pulses increases, that is, as the horizontal axis time increases, the resistance state of the memristor 10 is also different.

[0062] Correspondingly, in another specific embodiment, Figure 2a-2b As shown, Figure 2a The first comparative memristor structure diagram provided in this application is as follows: Figure 2b for Figure 2a The resistive DC IV curve of the comparative memristor is shown.

[0063] The first electrode 11 of the comparative memristor 10 is a gold (Au) electrode, specifically, including 5 nm thick chromium (Cr) as an adhesion layer, and 20 nm thick gold (Au) as the first electrode 11. The resistive layer 12 includes 35 nm thick indium phosphorus sulfide (IPS). The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40 nm thick palladium (Pd) electrode, and 40 nm thick gold (Au) on the surface as a protective layer.

[0064] like Figure 2b As shown, the comparative memristor 10 exhibits neither rectifying behavior nor resistive behavior.

[0065] and Figure 1a Compared with the memristor structure shown, the indium phosphide (IPS) material used in the comparative memristor 10 does not contain copper elements and has no ferroelectric properties, relative to copper indium phosphide (CIPS). It can be seen that the ferroelectric properties of CIPS play a key role in achieving self-rectification and resistive behavior.

[0066] Correspondingly, in another specific embodiment, Figure 3a-3b As shown, Figure 3a A schematic diagram of the second comparative memristor structure provided in this application, Figure 3b for Figure 3a The resistive DC IV curve of the comparative memristor is shown.

[0067] The first electrode 11 of the comparative memristor 10 is a gold (Au) electrode, specifically, including 5nm thick chromium (Cr) as an adhesion layer, and 20nm thick gold (Au) as the first electrode 101. The resistive layer 12 includes 35nm thick copper indium phosphorus sulfur (CIPS), in which the ratio of copper element is 0.2, that is, the atomic number ratio of copper element to indium element is 0.2. The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40nm thick palladium (Pd) electrode, and a 40nm thick gold (Au) on the surface as a protective layer.

[0068] like Figure 3b As shown, the comparative memristor 10 does not exhibit obvious rectification behavior, but has a certain resistive window, and the resistive switching ratio is about 35.2.

[0069] and Figure 1a Compared with the memristor structure shown in FIG. 1 , the copper element ratio of CIPS in the comparative memristor 10 is lower, and there is no obvious rectification behavior. It can be seen that the atomic number ratio of copper element to indium element in CIPS should be greater than 0.2, otherwise it is impossible to provide effective copper ion movement to achieve more obvious rectification characteristics and resistive switching performance.

[0070] In addition, the work functions of the materials of the first electrode 11 and the second electrode 13 are both greater than or equal to 5.0 eV, and the materials of the first electrode 11 and the second electrode 13 are different.

[0071] This is because, due to the large difference in work function between high work function materials and CIPS, for example, taking metal materials as an example, that is, the first electrode 11 and the second electrode 13 are both high work function metals, the high work function metal can contact CIPS to form a Schottky diode with a higher barrier. The low work function metal in contact with CIPS will form a diode with a lower barrier, or form an ohmic contact, that is, no diode is formed. Furthermore, among high work function metals, the barrier size of the Schottky diode formed by different high work function metals and CIPS is also different.

[0072] For example, Figure 4a to Figure 4d As shown, Figure 4a to Figure 4d This is a schematic diagram of the principle of a ferroelectric ion diode provided in an embodiment of the present application. The size of the diode in the figure indicates the height of the potential barrier. The larger the diode, the higher the potential barrier.

[0073] like Figure 4a As shown, high work function metal palladium (Pd) and gold (Au) are in contact with CIPS to form Schottky diodes with higher potential barriers. The work function of palladium (Pd) is higher than that of gold (Au), so the barrier height of the Pd / CIPS diode is greater than that of the CIPS / Au diode.

[0074] Similarly, if Figure 4b As shown, both electrodes are palladium (Pd) electrodes, and the barrier height of the Pd / CIPS diode formed thereby is the same as that of the CIPS / Pd diode.

[0075] like Figure 4c As shown in Figure 2, the Cr / CIPS diode barrier formed by the low work function metal chromium (Cr) in contact with CIPS is low, or as Figure 4d As shown, the Cr / CIPS diode barrier is almost negligible, that is, chromium (Cr) forms an ohmic contact with CIPS and does not have a diode behavior.

[0076] like Figure 4a As shown in the figure, when a forward voltage is applied to the palladium (Pd) electrode and the voltage is greater than the threshold voltage, the Pd / CIPS diode is forward-conducted, and the movement of copper ions in CIPS and the ferroelectric polarization lower the CIPS / Au barrier, electrons are injected, and the CIPS / Au diode is reverse-conducted, and the current increases. Correspondingly, when a negative voltage is applied to the palladium (Pd) electrode, due to the large Schottky barrier at the Pd end, the movement of copper ions in CIPS cannot effectively reduce the barrier, electron injection is hindered, and the current is therefore cut off.

[0077] In summary, using different high work function materials as the first electrode 11 and the second electrode 13 respectively can form a rectifying effect, and the polarization relaxation of the copper ion movement and ferroelectric coupling in CIPS also enables the formation of a resistive window.

[0078] When a low work function is used, such as Figure 4c or Figure 4d As shown, due to the low potential barrier at the low work function metal Cr end, the electron injection conditions are similar under positive and negative bias, and it is impossible to achieve a significant rectification effect and regulation of the ferroelectric polarization state of CIPS.

[0079] Similarly, when symmetrical electrodes are used, such as Figure 4b As shown, it is equivalent to two face-to-face diodes. The electron injection conditions are similar, and the electron injection conditions are the same under positive and negative bias voltages, and the rectification effect cannot be achieved.

[0080] Exemplarily, in another specific embodiment, Figure 5a-5b As shown, Figure 5a A schematic diagram of the third comparative memristor structure provided in this application, Figure 5b for Figure 5a The resistive DC IV curve of the comparative memristor is shown.

[0081] The first electrode 11 of the comparative memristor 10 is a gold (Au) electrode, specifically, including 5nm thick chromium (Cr) as an adhesion layer, and 20nm thick gold (Au) as the first electrode 101. The resistive layer 12 includes 35nm thick copper indium phosphorus sulfur (CIPS), in which the ratio of copper element is 0.5, that is, the atomic number ratio of copper element to indium element is 0.5. The second electrode 13 is a chromium (Cr) electrode, specifically, including a 40nm thick chromium (Cr) electrode, and 40nm thick gold (Au) on the surface as a protective layer.

[0082] like Figure 5b As shown, the comparative memristor 10 does not exhibit obvious rectifying behavior and resistive behavior.

[0083] and Figure 1a Compared with the memristor structure shown in the figure, the second electrode 13 in the comparative memristor 10 is a chromium (Cr) electrode, and the chromium (Cr) metal work function is relatively low, about 4.5 eV. The second Schottky barrier formed by the contact between the chromium and the CIPS of the resistive layer 12 is relatively low. Under positive and negative bias voltages, the injection conditions of electrons are similar. Therefore, it is impossible to achieve an obvious rectification effect and regulation of the ferroelectric polarization state of CIPS.

[0084] Exemplarily, in another specific embodiment, Figure 6a-6b As shown, Figure 6a A schematic diagram of the fourth comparative memristor structure provided in this application, Figure 6b for Figure 6aThe resistive DC IV curve of the comparative memristor is shown.

[0085] The first electrode 11 of the comparative memristor 10 is a palladium (Pd) electrode, specifically, including 5 nm thick chromium (Cr) as an adhesion layer, and 20 nm thick palladium (Pd) as the first electrode 101. The resistive layer 12 includes 35 nm thick copper indium phosphorus sulfur (CIPS), wherein the ratio of copper element is 0.5, that is, the atomic number ratio of copper element to indium element is 0.5. The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40 nm thick palladium (Pd) electrode, and a 40 nm thick gold (Au) on the surface as a protective layer.

[0086] like Figure 6b As shown, the comparative memristor 10 has obvious resistive behavior, and the resistive switching ratio is about 2640, which is similar to Figure 1a The memristor structure shown, i.e., the memristor structure in which the first electrode 11 is a gold (Au) electrode, has a comparable resistive switch ratio. However, the rectification behavior of the comparative memristor 10 is not obvious, and the rectification ratio is about 2. Since the comparative memristor 10 adopts a symmetrical electrode design, i.e., the first electrode 11 and the second electrode 13 are both palladium (Pd) electrodes, the heights of the first Schottky barrier and the second Schottky barrier formed thereby are equal, and no asymmetric barrier is formed at both ends of the memristor, so the current level difference is not large under positive and negative polarity voltages, that is, there is no obvious rectification characteristic.

[0087] In summary, the asymmetric high work function material used as the first electrode 11 and the second electrode 13 is a key factor in achieving the self-rectifying behavior and the resistive behavior.

[0088] In some embodiments, in the material of the resistive layer, the atomic ratio of copper element to indium element is in the range of 0.4 to 1. Exemplarily, the atomic ratio of copper element to indium element is 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1.

[0089] By adjusting the proportion of copper elements and utilizing the ion movement and polarization characteristics of copper indium phosphide (CIPS) to adjust the resistive switching ratio and rectification ratio of the memristor 10, a memristor 10 with a high rectification ratio and a high resistive switching ratio can be finally obtained.

[0090] For example, in a specific embodiment, Figure 7a-7b As shown, Figure 7a A schematic diagram of another memristor structure provided in an embodiment of the present application, Figure 7b for Figure 7a The resistive DC IV curve of the memristor is shown.

[0091] In the embodiment of the present application, the first electrode 11 is a gold (Au) electrode, specifically, including a 5nm thick chromium (Cr) as an adhesion layer, and a 20nm thick gold (Au) electrode. The resistive layer 12 includes a 35nm thick copper indium phosphorus sulfur (CIPS), in which the ratio of copper element is 0.8, that is, the atomic number ratio of copper element to indium element is 0.8. The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40nm thick palladium (Pd) electrode, and a 40nm thick gold (Au) on the surface as a protective layer.

[0092] like Figure 7b As shown, the memristor 10 exhibits certain rectification behavior and resistive behavior, with a rectification ratio of about 50 and a resistive switching ratio of about 10,000.

[0093] and Figure 1a Compared with the memristor structure shown in FIG. 1 , the copper element ratio of CIPS is increased from 0.5 to 0.8 in this embodiment. After the copper element ratio is increased, the rectification ratio decreases and the resistive switching ratio increases. In general, the memristor 10 has a high rectification ratio and resistive switching ratio, and can achieve self-rectification while maintaining resistive switching performance. That is, the memristor 10 simultaneously achieves simulated resistive behavior with a high rectification ratio and a high resistive switching ratio.

[0094] In some embodiments, the rectification ratio of the memristor 10 ranges from 50 to 2000, and the resistive switching ratio of the memristor 10 ranges from 2000 to 17000. For example, the rectification ratio is 50, 100, 200, ... 2000, etc., and the resistive switching ratio is 2000, 2500, 3000, ... 17000, etc.

[0095] The rectification ratio and resistive switching ratio of the memristor 10 can be adjusted by the proportion of copper elements in CIPS to eventually achieve the required ratio.

[0096] In some embodiments, the material of the first electrode 11 includes at least one of palladium, platinum or gold, and the material of the second electrode 13 includes at least one of palladium, platinum or gold. The work function of palladium (Pd) is about 5.12eV, the work function of platinum (Pt) is about 5.65eV, and the work function of gold (Au) is about 5.10eV, all of which can be used as electrodes of the memristor 10 to form a Schottky barrier with copper indium phosphide (CIPS) of the resistive layer 12, and the Schottky barrier has a relatively high height.

[0097] In some embodiments, the thickness of the resistive layer 12 ranges from 7 nm to 100 nm. For example, the thickness of the resistive layer 12 can be 7 nm, 12 nm, 22 nm, 35 nm, 55 nm, ... 100 nm, etc. The thickness of the resistive layer 12 also affects the rectification ratio and resistive switching ratio of the memristor 10 to a certain extent.

[0098] For example, in a specific embodiment, Figure 8a-8b As shown, Figure 8a A schematic diagram of another memristor structure provided in an embodiment of the present application is shown in FIG. Figure 8b for Figure 8a The resistive DC IV curve of the memristor is shown.

[0099] In the embodiment of the present application, the first electrode 11 is a gold (Au) electrode, specifically, including 5nm thick chromium (Cr) as an adhesion layer, and a 20nm thick gold (Au) electrode. The resistive layer 12 includes 12nm thick copper indium phosphorus sulfur (CIPS), in which the ratio of copper element is 0.5, that is, the atomic number ratio of copper element to indium element is 0.5. The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40nm thick palladium (Pd) electrode, and a 40nm thick gold (Au) on the surface as a protective layer.

[0100] like Figure 8b As shown, the memristor 10 exhibits rectification behavior and resistive behavior, with a rectification ratio of about 200 and a resistive switching ratio greater than 2000, about 2700.

[0101] and Figure 1a Compared with the memristor structure shown in FIG. 1 , in this embodiment, the resistive layer 12 adopts a thin layer of CIPS, that is, the CIPS thickness of the resistive layer 12 is changed from 35nm to 12nm. After the thin layer of CIPS is adopted, the rectification ratio is reduced, and the resistive switching ratio is equivalent. In general, the memristor 10 has a high rectification ratio and resistive switching ratio, and can realize self-rectification while maintaining the resistive switching performance, that is, the memristor 10 simultaneously realizes the simulated resistive behavior of high rectification ratio and high resistive switching ratio.

[0102] For example, in a specific embodiment, Figure 9a-9b As shown, Figure 9a A schematic diagram of another memristor structure provided in an embodiment of the present application is shown in FIG. Figure 9b for Figure 9a The resistive DC IV curve of the memristor is shown.

[0103] In the embodiment of the present application, the first electrode 11 is a gold (Au) electrode, specifically, including 5nm thick chromium (Cr) as an adhesion layer, and a 20nm thick gold (Au) electrode. The resistive layer 12 includes 22nm thick copper indium phosphorus sulfur (CIPS), in which the ratio of copper element is 0.5, that is, the atomic number ratio of copper element to indium element is 0.5. The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40nm thick palladium (Pd) electrode, and a 40nm thick gold (Au) on the surface as a protective layer.

[0104] like Figure 9bAs shown, the memristor 10 exhibits rectification behavior and resistive behavior, with a rectification ratio of more than 2000 and a resistive switching ratio of more than 4000.

[0105] and Figure 1a Compared with the memristor structure shown in FIG. 1 , the CIPS thickness of the resistive layer 12 in the memristor 10 in this embodiment is changed from 35 nm to 22 nm. After the CIPS is thinned, the rectification ratio and the resistive switching ratio are improved. Figure 8a Compared with the memristor structure shown in FIG. 1 , the CIPS thickness of the resistive layer 12 in the memristor 10 in this embodiment is changed from 12 nm to 22 nm. After the CIPS is thickened, the rectification ratio and the resistive switching ratio are improved. Overall, the memristor 10 still has a relatively high rectification ratio and resistive switching ratio, and can achieve self-rectification while maintaining the resistive switching performance. That is, the memristor 10 simultaneously achieves the simulated resistive behavior of high rectification ratio and high resistive switching ratio.

[0106] For example, in a specific embodiment, Figures 10a to 10b As shown, Fig.10a A schematic diagram of another memristor structure provided in an embodiment of the present application is shown below. Fig.10b for Fig.10a The resistive DC IV curve of the memristor is shown.

[0107] In the embodiment of the present application, the first electrode 11 is a gold (Au) electrode, specifically, including a 5nm thick chromium (Cr) as an adhesion layer, and a 20nm thick gold (Au) electrode. The resistive layer 12 includes a 55nm thick copper indium phosphorus sulfur (CIPS), in which the ratio of copper element is 0.8, that is, the atomic number ratio of copper element to indium element is 0.8. The second electrode 13 is a palladium (Pd) electrode, specifically, including a 40nm thick palladium (Pd) electrode, and a 40nm thick gold (Au) on the surface as a protective layer.

[0108] like Fig.10b As shown, the memristor 10 exhibits rectification behavior and resistive behavior, with a rectification ratio of about 100 and a resistive switching ratio greater than 10,000, about 17,000.

[0109] and Figure 7a Compared with the memristor structure shown in FIG. 1 , the CIPS thickness of the resistive layer 12 in the memristor 10 in this embodiment is increased from 35 nm to 55 nm, the rectification ratio is improved, and the resistive switching ratio is equivalent. Overall, the memristor 10 still has a relatively high rectification ratio and resistive switching ratio, and can achieve self-rectification while maintaining the resistive switching performance, that is, the memristor 10 simultaneously achieves the simulated resistive behavior of high rectification ratio and high resistive switching ratio.

[0110] According to the above embodiments, the memristor 10 provided in the present application can realize gradual resistance state adjustment, providing a new solution for the research and development of new high-performance information storage devices in the "post-Moore era".

[0111] In a second aspect, the present application also provides a method for preparing a memristor, such as Fig.11 As shown, Fig.11 A method for preparing a memristor provided in an embodiment of the present application specifically includes:

[0112] The first electrode 11, the resistive layer 12 and the second electrode 13 are formed in sequence. The resistive layer 12 is made of copper indium phosphide, and the atomic ratio of copper to indium in copper indium phosphide is greater than 0.2. The work functions of the materials of the first electrode 11 and the second electrode 13 are both greater than or equal to 5 eV, and the metal materials of the first electrode 11 and the second electrode 13 are different.

[0113] Specifically, taking the case where the first electrode 11 is a gold (Au) electrode and the second electrode 13 is a palladium (Pd) electrode as an example, a photoresist can be spin-coated on a silicon or silicon oxide substrate. After the photoresist coating is completed, ultraviolet photolithography is used for exposure to form a pre-designed pattern required for the first electrode 11. Afterwards, a thermal evaporation or electron beam evaporation process is used to sequentially generate a 5 nm thick chromium (Cr) as an adhesion layer and a 20 nm thick gold (Au) electrode. Thus, the first electrode 11 is formed.

[0114] In the above-mentioned process of spin coating photoresist, in some preparation processes, the first layer of photoresist LOR5A (purchased from Kayaku Advanced Materials) is firstly spin coated at a speed of 2000r / min by a spin coater, and then baked at 150°C for 5min, and then the second layer of photoresist AZ5214 is spin coated at a speed of 5000r / min by a spin coater, and then baked at 100°C for 1min, and the photoresist coating is completed. Alternatively, in some preparation processes, a layer of photoresist AZ5214 is spin coated at a speed of 5000r / min by a spin coater, and then baked at 100°C for 1min, and the photoresist coating is completed.

[0115] After forming the first electrode 11, it is also necessary to form a copper indium phosphide sulfur (CIPS) nanosheet, and transfer the copper indium phosphide sulfur (CIPS) nanosheet material onto the first electrode 11. Thus, the resistive layer 12 is formed.

[0116] Next, a photoresist is spin-coated on the transferred copper indium phosphide (CIPS). The process of spin-coating the photoresist is as described above and will not be repeated here.

[0117] Then, ultraviolet photolithography is used for exposure to form the pre-designed pattern required for the second electrode 13. After that, a 40nm thick palladium (Pd) electrode is evaporated by electron beam evaporation, and a 40nm thick gold (Au) is evaporated by thermal evaporation as a protective layer. Thus, the second electrode 13 is formed.

[0118] Finally, the photoresist is removed. For devices that have been subjected to two spin coating processes, N-methylpyrrolidone (NMP) can be used to remove the photoresist LOR5A first, and then acetone can be used to remove the photoresist AZ5214; for devices that have only been subjected to one spin coating process, acetone can be used to directly remove the photoresist AZ5214.

[0119] After the stripping is completed, the designed pattern is left on the substrate, thereby obtaining the required memristor 10.

[0120] The memristor prepared by the above preparation method has a high resistive switching ratio and rectification ratio, and can achieve self-rectification while maintaining resistive performance. The memristor cross array formed by the memristor prepared by the above preparation method can utilize the rectification characteristics of the memristor itself to avoid the problem of sneak current.

[0121] When the first electrode 11 and the second electrode 13 are made of other materials, the preparation process is the same as above and will not be repeated here.

[0122] In some embodiments, forming the resistive layer 12 specifically includes: transferring the resistive layer 12 onto the first electrode 11 by using a mechanical stripping process.

[0123] Illustratively, in some preparation processes, copper indium phosphosulfide (CIPS) nanosheets are obtained by a tape mechanical stripping method, copper indium phosphosulfide (CIPS) is adhered to polypropylene carbonate (PPC), and then transferred to the prefabricated first electrode 11 through a two-dimensional material transfer station.

[0124] Alternatively, in some preparation processes, copper indium phosphosulfide (CIPS) nanosheets are obtained by a tape mechanical stripping method, copper indium phosphosulfide (CIPS) is pasted onto dimethyl polysiloxane (PDMS), and then transferred to the prefabricated first electrode 11 through a two-dimensional material transfer station.

[0125] In some embodiments, forming the resistive layer 12 specifically includes: forming the resistive layer 12 by a chemical vapor deposition process, and transferring the resistive layer 12 onto the first electrode 11 .

[0126] Exemplarily, in some preparation processes, copper indium phosphide sulfur (CIPS) nanosheets are obtained by chemical vapor deposition (CVD), a layer of polystyrene (PS) is coated on the CVD-grown copper indium phosphide sulfur (CIPS), baked at 80°C for 10 minutes, and then the PS layer is peeled off in water and transferred to the prefabricated first electrode 11.

[0127] The thickness of the copper indium phosphide (CIPS) nanosheet and the proportion of the copper element mentioned in the above embodiment can be selected according to the needs, and CIPS with different copper element proportions can be obtained through different growth processes. For example, the copper indium phosphide (CIPS) nanosheet is 12nm, 20nm, 35nm thick, etc. The atomic number ratio of the copper element to the indium element is 0.5, 0.6, 0.8, etc. Different thicknesses and copper element proportions make the finally prepared memristor 10 have different resistive switching ratios and rectification ratios.

[0128] In a third aspect, the present application also provides a chip 20, such as Fig.12 As shown, Fig.12 A schematic diagram of a chip provided in an embodiment of the present application, wherein the chip 20 comprises the memristor 10 of any embodiment of the first aspect described above and a packaging layer 201, wherein the packaging layer 201 covers the memristor 10, and plays a role in protecting and isolating the memristor. The chip has the same structure and beneficial technical effects as the above-mentioned memristor, has a higher resistive switching ratio and self-rectification ratio, and can achieve self-rectification behavior while maintaining resistive performance.

[0129] In a fourth aspect, the present application also provides an electronic device 30, such as Fig.13 As shown, Fig.13 A schematic diagram of an electronic device provided in an embodiment of the present application, the electronic device 30 includes the chip 20 mentioned in the third aspect above, and a circuit board 301, wherein the chip 20 is electrically connected to the circuit board 301. The electronic device has the same structure and beneficial technical effects as the above-mentioned memristor and chip, has a higher resistive switching ratio and self-rectification ratio, and can achieve self-rectification behavior while maintaining resistive performance.

[0130] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that a person skilled in the art can think of within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A memristor, characterized in that: The memristor comprises a first electrode, a resistive layer and a second electrode which are stacked; The material of the resistive layer includes copper indium phosphide, and the atomic number ratio of copper element to indium element in the copper indium phosphide is greater than 0.2; The work functions of the materials of the first electrode and the second electrode are both greater than or equal to 5.0 eV, and the materials of the first electrode and the second electrode are different.

2. The memristor according to claim 1, characterized in that In the material of the resistive layer, the atomic number ratio of copper element to indium element is in the range of 0.4-1.

3. The memristor according to claim 1, characterized in that The rectification ratio of the memristor ranges from 50 to 2000, and the resistive switch ratio of the memristor ranges from 2000 to 17000.

4. The memristor according to claim 1, characterized in that The material of the first electrode includes at least one of palladium, platinum or gold; The material of the second electrode includes at least one of palladium, platinum or gold.

5. The memristor according to claim 1, characterized in that: The thickness of the resistive layer ranges from 7 nm to 100 nm.

6. A method for preparing a memristor, characterized in that: include: forming a first electrode, a resistive layer and a second electrode in sequence; The material of the resistive layer includes copper indium phosphide, and the atomic number ratio of copper element to indium element in the copper indium phosphide is greater than 0.2; The work functions of the materials of the first electrode and the second electrode are both greater than or equal to 5 eV, and the metal materials of the first electrode and the second electrode are different.

7. The preparation method according to claim 6, characterized in that: Forming the resistive layer comprises: The resistive layer is transferred onto the first electrode by a mechanical stripping process.

8. The preparation method according to claim 6, characterized in that: Forming the resistive layer comprises: The resistive layer is formed by a chemical vapor deposition process, and the resistive layer is transferred to the first electrode.

9. A chip, characterized in that: include: The memristor according to any one of claims 1 to 5; A packaging layer covers the memristor.

10. An electronic device, characterized in that: include: The chip as claimed in claim 9; A circuit board, the chip is electrically connected to the circuit board.

Citation Information

Cited By

  • Self-rectification memristor with adaptivity and preparation method thereof

    CN120813234A

  • Self-adapting self-rectifying memristor and preparation method thereof

    CN120813234B