Ultrathin antimony selenide resistive layer memristor and preparation method thereof

Deposition of ultra-thin Sb2Se3 layers by fast thermal evaporation solves the problems of high power consumption and unstable electrical characteristics of memristors, and realizes low power consumption and high stability memristors, suitable for flexible electronic devices and data storage field.

CN119031828APending Publication Date: 2024-11-26CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411182373.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing memristors are difficult to maintain the stability and performance of the device due to high power consumption, unstable electrical characteristics and poor repeatability, especially when designing ultra-thin antimony selenide resistive layer.

Method used

The ultra-thin Sb2Se3 layer is deposited by rapid thermal evaporation (RTE). By controlling the time and temperature during the deposition process, an Sb2Se3 resistive layer with a thickness of 30-100 nm is formed, and an Ag top electrode and an FTO bottom electrode are formed on the substrate. Optimize electronic transport characteristics and electrical properties.

Benefits of technology

It realizes the reduction of power consumption while maintaining device stability, improves device integration and flexibility, improves electrical performance and reliability, and enhances the versatility and storage capabilities of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005012553120000011
    Figure HDA0005012553120000011
  • Figure HDA0005012553120000012
    Figure HDA0005012553120000012
  • Figure HDA0005012553120000021
    Figure HDA0005012553120000021
Patent Text Reader

Abstract

The invention belongs to the field of memristor preparation, and particularly discloses an ultrathin antimony selenide resistive random access layer memristor and a preparation method thereof. The memristor prepared by the invention comprises a substrate, a bottom electrode, a resistive layer and a top electrode which are sequentially arranged from bottom to top, wherein the resistive layer is made of Sb2Se3 materials, the bottom of the resistive layer is in contact with the top of the bottom electrode, and the top of the resistive layer is in contact with the bottom of the top electrode. The resistance change layer is an ultrathin Sb2Se3 layer, the ultrathin Sb2Se3 layer is deposited through a rapid thermal evaporation method (RTE), the thickness of the ultrathin Sb2Se3 layer is 40-60 nm, the stability and uniformity of the memristor are improved, and meanwhile power consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of memristor preparation and relates to an ultra-thin antimony selenide resistive layer memristor. Background Art

[0002] As one of the four basic electronic components, memristor has a unique "memory" function. It is an important component and medium for realizing neuromorphic computing technology, and can be applied to important fields such as artificial neural network synapses, information storage and machine learning. In recent years, with the increasing demand for intelligent and flexible electronic devices, new requirements have been put forward for memristors, such as energy saving, flexibility, high integration and multi-functions.

[0003] Sb2Se3 material can be activated by an external electric field or current to achieve resistance changes over time or voltage, and has a good resistance change effect. This controllability is conducive to realizing a variety of different resistance states in the memristor, providing more possibilities for storage and logical operations. KR20230082068A discloses a memristor with multi-level switching characteristics and a method for manufacturing the same, which discloses the application of antimony selenide (Sb2Se3) as a resistance change layer in a memristor device. Antimony selenide is deposited on the first electrode by a pulsed laser deposition (PLD) method, and the thickness of Sb2Se3 is not specified. However, the cost of pulsed laser deposition for the preparation of thin Sb2Se3 films is too high, and rapid thermal evaporation (RTE) technology stands out for its cost-effectiveness and ease of operation.

[0004] As a semiconductor material with special structure and properties, Sb2Se3 provides favorable conditions for the manufacture of memristors, including excellent electron transmission performance, non-volatile characteristics and adjustable resistive switching effect. Ultrathin Sb2Se3 has high electron mobility and good carrier transport performance, which is conducive to the realization of fast state conversion and stable resistance characteristics in memristors. In addition, ultrathin materials help to improve the integration of devices, improve thermal management, reduce material usage, reduce costs, and may make devices more flexible and suitable for flexible electronic devices. At the same time, precisely controlled antimony selenide thickness helps to optimize electrical properties, such as retention and durability, thereby improving device reliability. Nevertheless, the design also needs to overcome the challenges that may be brought about by ultrathin resistive switching layers, such as reduced retention and stability, to ensure the overall performance of memristors. However, there is currently no application of ultrathin Sb2Se3 in memristors. Summary of the invention

[0005] The purpose of the present invention is to provide an ultra-thin antimony selenide resistive layer memristor and a preparation method thereof. The present invention prepares Sb2Se3 with appropriate thickness as the material of the resistive layer, which can reduce the power consumption of the memristor while maintaining the stability of the memristor.

[0006] To achieve the above-mentioned purpose, the present invention provides a memristor, comprising a substrate, a resistive layer and a top electrode arranged in sequence from bottom to top, wherein the resistive layer is made of Sb2Se3 material, the bottom of the resistive layer contacts the top of the bottom electrode, and the top of the resistive layer contacts the bottom of the top electrode.

[0007] The resistive switching layer is an ultra-thin Sb2Se3 layer, which is deposited by rapid thermal evaporation (RTE). The thickness and density of Sb2Se3 during the deposition process are maintained by controlling the time and temperature during the RTE process.

[0008] Optionally, the thickness of the Sb2Se3 layer is 30 to 100 nm, and more preferably 40 to 60 nm; the top electrode is an Ag layer, and the thickness of the Ag layer is 50 to 70 nm; the bottom electrode is an FTO layer, and the thickness of the FTO layer is 150 nm; and the substrate is a glass substrate coated with an FTO layer.

[0009] Optionally, the dielectric layer Sb2Se3 is formed on the bottom electrode layer by a rapid thermal evaporation method. The rapid thermal evaporation reaction process can be divided into three stages:

[0010] Substrate insulation stage: The RTE system is heated to 300°C and kept warm for 300 to 1200 seconds to achieve the deposition and preferential growth of the seed layer;

[0011] Thin film deposition stage: the heating rate is 10-15°C / s, the RTE system is further heated to 580°C and maintained for 40-90s; an antimony selenide film is grown on the upper surface of the FTO bottom electrode layer, and the thickness of the antimony selenide film is 30-100nm.

[0012] Cooling phase: The program stops and the machine cools naturally to room temperature.

[0013] Optionally, the substrate is a glass substrate coated with a FTO layer, the resistive layer is deposited on the substrate by rapid thermal evaporation, and the top electrode is formed on the resistive layer by evaporation coating.

[0014] The resistive switching layer is made of Sb2Se3 material with a thickness of about 40 to 60 nm. Sb2Se3 has a layered structure similar to graphene and has a multi-layer thickness adjustable layer structure. This structure enables antimony selenide to be better controlled and adjusted in the preparation of memristors, which is conducive to adjusting the electron transport characteristics at a microscopic scale. Antimony selenide also has non-volatile properties, showing good non-volatility in maintaining the resistance state. Once the state is set, it can stably store information for a long time, making it suitable for use in fields such as data storage. Antimony selenide materials can be activated by an external electric field or current to achieve changes in resistance over time or voltage, and have a good resistive switching effect. This controllability is conducive to achieving a variety of different resistance states in memristors, providing more possibilities for storage and logic operations.

[0015] The substrate is a purchased glass substrate coated with an FTO layer; the top electrode is an Ag layer with a thickness of 50 to 70 nm, and the top electrode is formed on the resistive layer by evaporation coating through the openings of a mask plate; the substrate is a glass substrate.

[0016] Among them, the top electrode and the bottom electrode are used to make electrical connections with an external power source, and the resistive switching layer is used to realize the conversion between resistance states. When a voltage is applied to the top electrode of the device, the top electrode Ag promotes the rapid growth of the conductive filaments, reducing the voltage required for the resistance change of the memristor, thereby improving the problems of high power consumption, unstable electrical characteristics, and poor repeatability in current memristors. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Schematic diagram of the structure of the memristor of the present invention.

[0018] Figure 2 This is an IV curve diagram of the memristor of Example 1 after one cycle at a current limit of 1 mA.

[0019] Figure 3 This is an IV curve diagram of the memristor of Example 1 after 30 cycles at 1 mA current limit.

[0020] Figure 4 This is a diagram showing the retention characteristics of the high and low resistance states of the memristor in Example 1 under 1 mA current limiting.

[0021] Figure 5 This is an IV curve diagram of the memristor of Example 2-4 after one cycle at a current limit of 1 mA.

[0022] Figure 6 This is a diagram showing the retention characteristics of the high and low resistance states of the memristor of Example 2 under 1 mA current limiting.

[0023] Figure 7 This is a diagram showing the retention characteristics of the high and low resistance states of the memristor of Example 3 under 1 mA current limiting.

[0024] Figure 8 This is a diagram showing the retention characteristics of the high and low resistance states of the memristor of Example 4 under 1 mA current limiting. DETAILED DESCRIPTION

[0025] like Figure 1 As shown, the present invention discloses a memristor, comprising a substrate, a resistive layer and a top electrode arranged in sequence from bottom to top, wherein the resistive layer is made of Sb2Se3 material, the bottom of the resistive layer contacts the top of the bottom electrode, and the top of the resistive layer contacts the bottom of the top electrode.

[0026] Example 1

[0027] 1) Buy a glass substrate coated with a FTO layer as a substrate;

[0028] 2) Place the glass substrate coated with the FTO layer in a beaker and ultrasonicate it with glass cleaning liquid and deionized water for 30 minutes each. After discarding the waste liquid, ultrasonicate it with deionized water for 3-5 times, each time for 10 minutes. The water temperature should not exceed 40°C during the ultrasonication. Then discard the water and add isopropanol for 30 minutes. Finally, ultrasonicate it with anhydrous ethanol for 30 minutes. Blow it dry with an air pump and put it in a drying cabinet for later use.

[0029] 3) using rapid thermal evaporation (RTE) to grow an antimony selenide resistive switching layer on the upper surface of the FTO bottom electrode layer;

[0030] 4) Put the antimony selenide powder into an oven and set the oven temperature to 90° C. After 24 hours, weigh 0.6-0.8 g of the dried antimony selenide powder on an electronic balance and evenly cover the antimony selenide powder on a glass sheet.

[0031] 5) Open the rapid annealing furnace chamber, install an AlN ceramic sheet on the heating table, and place the glass sheet covered with antimony selenide powder in step 4) on the AlN ceramic sheet.

[0032] 6) The glass substrate coated with the FTO layer after cleaning in step 2) is placed opposite to the antimony selenide powder, with the FTO surface and the antimony selenide powder being 5 to 10 mm apart. A graphite block is covered on the substrate to maintain the substrate temperature.

[0033] 7) Evacuate the rapid annealing furnace chamber to 2.0×10 -3 Torr, the antimony selenide powder and the glass substrate coated with the FTO layer are heated to 300°C and kept warm for 1200s; after the insulation, the antimony selenide powder and the glass substrate deposited with the FTO layer are heated to 580°C, and the growth time is 60s; an antimony selenide film is grown on the upper surface of the FTO bottom electrode layer, and the thickness of the antimony selenide film is 50nm.

[0034] 8) Take the prepared film out of the rapid annealing furnace and evaporate the electrode after cooling. Weigh 0.2 grams of silver (Ag) and place Ag in the evaporation boat of the vacuum coating machine as an evaporation source.

[0035] 9) Start the vacuum system and evacuate the air to reduce the system pressure to 7×10 -4 Pa. Before starting evaporation, the evaporation source is properly preheated to allow the metal to reach an appropriate evaporation temperature. The preheating time is five minutes, and the preheating temperature is adjusted by the current of the boat control. The current size of the preheating stage is 75A.

[0036] 10) After the evaporating Ag is completely melted, the current is adjusted to 85A, and the metal is heated for 10 minutes to evaporate the silver and deposit it on the surface of the antimony selenide resistive layer. After 10 minutes, a silver electrode with a thickness of about 60nm is deposited.

[0037] 11) Stop the evaporation of the metal and close the vacuum system. Ensure that the closing process is smooth to avoid affecting the quality of the film. Allow the system to cool to room temperature, and gradually release the vacuum to restore the chamber pressure to normal pressure and remove the sample.

[0038] Example 2

[0039] 1) Buy a glass substrate coated with a FTO layer as a substrate;

[0040] 2) Place the glass substrate coated with the FTO layer in a beaker and ultrasonicate it with glass cleaning liquid and deionized water for 30 minutes each. After discarding the waste liquid, ultrasonicate it with deionized water for 3-5 times, each time for 10 minutes. The water temperature should not exceed 40°C during the ultrasonication. Then discard the water and add isopropanol for 30 minutes. Finally, ultrasonicate it with anhydrous ethanol for 30 minutes. Blow it dry with an air pump and put it in a drying cabinet for later use.

[0041] 3) using rapid thermal evaporation (RTE) to grow an antimony selenide resistive switching layer on the upper surface of the FTO bottom electrode layer;

[0042] 4) Put the antimony selenide powder into an oven and set the oven temperature to 90° C. After 24 hours, weigh 0.6-0.8 g of the dried antimony selenide powder on an electronic balance and evenly cover the antimony selenide powder on a glass sheet.

[0043] 5) Open the rapid annealing furnace chamber, install an AlN ceramic sheet on the heating table, and place the glass sheet covered with antimony selenide powder in step 4) on the AlN ceramic sheet.

[0044] 6) The glass substrate coated with the FTO layer after cleaning in step 2) is placed opposite to the antimony selenide powder, with the FTO surface and the antimony selenide powder being 5 to 10 mm apart. A graphite block is covered on the substrate to maintain the substrate temperature.

[0045] 7) Evacuate the rapid annealing furnace chamber to 2.0×10 -3 Torr, the antimony selenide powder and the glass substrate coated with the FTO layer are heated to 300°C and kept warm for 1200s; after the insulation, the antimony selenide powder and the glass substrate deposited with the FTO layer are heated to 580°C, and the growth time is 70s; an antimony selenide film is grown on the upper surface of the FTO bottom electrode layer, and the thickness of the antimony selenide film is 80nm.

[0046] 8) Take the prepared film out of the rapid annealing furnace and evaporate the electrode after cooling. Weigh 0.2 grams of silver (Ag) and place Ag in the evaporation boat of the vacuum coating machine as an evaporation source.

[0047] 9) Start the vacuum system and evacuate the air to reduce the system pressure to 7×10 -4 Pa. Before starting evaporation, the evaporation source is properly preheated to allow the metal to reach an appropriate evaporation temperature. The preheating time is five minutes, and the preheating temperature is adjusted by the current of the boat control. The current size of the preheating stage is 75A.

[0048] 10) After the evaporating Ag is completely melted, the current is adjusted to 85A, and the metal is heated for 10 minutes to evaporate the silver and deposit it on the surface of the antimony selenide resistive layer. After 10 minutes, a silver electrode with a thickness of about 60nm is deposited.

[0049] 11) Stop the evaporation of the metal and close the vacuum system. Ensure that the closing process is smooth to avoid affecting the quality of the film. Allow the system to cool to room temperature, and gradually release the vacuum to restore the chamber pressure to normal pressure and remove the sample.

[0050] Example 3

[0051] 1) Buy a glass substrate coated with a FTO layer as a substrate;

[0052] 2) Place the glass substrate coated with the FTO layer in a beaker and ultrasonicate it with glass cleaning liquid and deionized water for 30 minutes each. After discarding the waste liquid, ultrasonicate it with deionized water for 3-5 times, each time for 10 minutes. The water temperature should not exceed 40°C during the ultrasonication. Then discard the water and add isopropanol for 30 minutes. Finally, ultrasonicate it with anhydrous ethanol for 30 minutes. Blow it dry with an air pump and put it in a drying cabinet for later use.

[0053] 3) using rapid thermal evaporation (RTE) to grow an antimony selenide resistive switching layer on the upper surface of the FTO bottom electrode layer;

[0054] 4) Put the antimony selenide powder into an oven and set the oven temperature to 90° C. After 24 hours, weigh 0.6-0.8 g of the dried antimony selenide powder on an electronic balance and evenly cover the antimony selenide powder on a glass sheet.

[0055] 5) Open the rapid annealing furnace chamber, install an AlN ceramic sheet on the heating table, and place the glass sheet covered with antimony selenide powder in step 4) on the AlN ceramic sheet.

[0056] 6) The glass substrate coated with the FTO layer after cleaning in step 2) is placed opposite to the antimony selenide powder, with the FTO surface and the antimony selenide powder being 5 to 10 mm apart. A graphite block is covered on the substrate to maintain the substrate temperature.

[0057] 7) Evacuate the rapid annealing furnace chamber to 2.0×10 -3 Torr, the antimony selenide powder and the glass substrate coated with the FTO layer are heated to 300°C and kept warm for 1200s; after the insulation, the antimony selenide powder and the glass substrate deposited with the FTO layer are heated to 580°C, and the growth time is 90s; an antimony selenide film is grown on the upper surface of the FTO bottom electrode layer, and the thickness of the antimony selenide film is 120nm.

[0058] 8) Take the prepared film out of the rapid annealing furnace and evaporate the electrode after cooling. Weigh 0.2 grams of silver (Ag) and place Ag in the evaporation boat of the vacuum coating machine as an evaporation source.

[0059] 9) Start the vacuum system and evacuate the air to reduce the system pressure to 7×10 -4 Pa. Before starting evaporation, the evaporation source is properly preheated to allow the metal to reach an appropriate evaporation temperature. The preheating time is five minutes, and the preheating temperature is adjusted by the current of the boat control. The current size of the preheating stage is 75A.

[0060] 10) After the evaporating Ag is completely melted, the current is adjusted to 85A, and the metal is heated for 10 minutes to evaporate the silver and deposit it on the surface of the antimony selenide resistive layer. After 10 minutes, a silver electrode with a thickness of about 60nm is deposited.

[0061] 11) Stop the evaporation of the metal and close the vacuum system. Ensure that the closing process is smooth to avoid affecting the quality of the film. Allow the system to cool to room temperature, and gradually release the vacuum to restore the chamber pressure to normal pressure and remove the sample.

[0062] Example 4

[0063] 1) Buy a glass substrate coated with a FTO layer as a substrate;

[0064] 2) Place the glass substrate coated with the FTO layer in a beaker and ultrasonicate it with glass cleaning liquid and deionized water for 30 minutes each. After discarding the waste liquid, ultrasonicate it with deionized water for 3-5 times, each time for 10 minutes. The water temperature should not exceed 40°C during the ultrasonication. Then discard the water and add isopropanol for 30 minutes. Finally, ultrasonicate it with anhydrous ethanol for 30 minutes. Blow it dry with an air pump and put it in a drying cabinet for later use.

[0065] 3) using rapid thermal evaporation (RTE) to grow an antimony selenide resistive switching layer on the upper surface of the FTO bottom electrode layer;

[0066] 4) Put the antimony selenide powder into an oven and set the oven temperature to 90° C. After 24 hours, weigh 0.6-0.8 g of the dried antimony selenide powder on an electronic balance and evenly cover the antimony selenide powder on a glass sheet.

[0067] 5) Open the rapid annealing furnace chamber, install an AlN ceramic sheet on the heating table, and place the glass sheet covered with antimony selenide powder in step 4) on the AlN ceramic sheet.

[0068] 6) The glass substrate coated with the FTO layer after cleaning in step 2) is placed opposite to the antimony selenide powder, with the FTO surface and the antimony selenide powder being 5 to 10 mm apart. A graphite block is covered on the substrate to maintain the substrate temperature.

[0069] 7) Evacuate the rapid annealing furnace chamber to 2.0×10 -3 Torr, the antimony selenide powder and the glass substrate coated with the FTO layer are heated to 300°C and kept warm for 1200s; after the insulation, the antimony selenide powder and the glass substrate deposited with the FTO layer are heated to 580°C, and the growth time is 40s; an antimony selenide film is grown on the upper surface of the FTO bottom electrode layer, and the thickness of the antimony selenide film is 30nm.

[0070] 8) Take the prepared film out of the rapid annealing furnace and evaporate the electrode after cooling. Weigh 0.2 grams of silver (Ag) and place Ag in the evaporation boat of the vacuum coating machine as an evaporation source.

[0071] 9) Start the vacuum system and evacuate the air to reduce the system pressure to 7×10 -4 Pa. Before starting evaporation, the evaporation source is properly preheated to allow the metal to reach an appropriate evaporation temperature. The preheating time is five minutes, and the preheating temperature is adjusted by the current of the boat control. The current size of the preheating stage is 75A.

[0072] 10) After the evaporating Ag is completely melted, the current is adjusted to 85A, and the metal is heated for 10 minutes to evaporate the silver and deposit it on the surface of the antimony selenide resistive layer. After 10 minutes, a silver electrode with a thickness of about 60nm is deposited.

[0073] 11) Stop the evaporation of the metal and close the vacuum system. Ensure that the closing process is smooth to avoid affecting the quality of the film. Allow the system to cool to room temperature, and gradually release the vacuum to restore the chamber pressure to normal pressure and remove the sample.

[0074] When a positive voltage is applied to the memristor, the voltage is swept from 0V to the set positive voltage and then from the set positive voltage back to 0V. During this process, metal conductive filaments are formed in the resistive layer of the memristor device. The conductive filaments connect the top electrode and the bottom electrode, resulting in a resistance transition effect. The device changes from a high-resistance state to a low-resistance state. This is the SET process. In the RESET process, the voltage is swept from 0V to a set negative voltage and then from the set negative voltage to 0V. During this process, the device changes from a low-resistance state back to a high-resistance state due to the breakage of the conductive filaments.

[0075] like Figure 2 As shown, the original device exhibits a high resistance state (HRS) and can be switched to a low resistance state (LRS) by applying a negative DC sweep, where a SET voltage of approximately -0.5 V is observed and a RESET voltage of 0.9 V. The device can then be reset back to HRS.

[0076] like Figure 3 As shown in the figure, the curve shows that the SET voltage of the memristor is low, about -0.25V, and the RESET voltage has a slight fluctuation around -1V, which is lower than other low-power devices (400fW under this current limit), indicating that the device's operating voltage is also very small under 1mA current limit. Both the SET voltage and the RESET voltage fluctuate within a very small range, and the curve overlaps very well, indicating that the device's electrical performance has good stability and repeatability and the stability can last for 10 4 cycle.

[0077] like Figure 4 As shown, the device can remain stable in both high and low resistance states under SET / RSET voltage stimulation without obvious attenuation, which indicates that the device has stable non-volatile storage performance.

[0078] like Figure 5As shown, the current-voltage characteristics of the memristors of Examples 2 to 4 are analyzed, and the switching ratios of these devices are relatively low. Specifically, the difference in resistance between the high resistance state (HRS) and the low resistance state (LRS) is not significant, indicating that the transition between the two resistance states is not obvious enough. The high resistance state of Example 1 reaches 120Ω, while the low resistance state is only 23Ω. This significant switching ratio not only enhances its storage capacity, but also provides great flexibility for data storage and logical operations. In contrast, the resistance value change of Example 2 is not significant, and it fails to provide sufficient resistance state contrast, limiting its potential in storage applications. Although Example 3 has been improved, the high resistance state is 55Ω and the low resistance state is 25Ω, but compared with Example 1, its resistance transition amplitude is smaller, and it may not perform well in some applications that are sensitive to resistance state changes. The high resistance state of Example 4 is 50Ω and the low resistance state is 30Ω. Although the resistance state contrast is improved to a certain extent, there is still a gap compared with Example 1. The results of Examples 2 to 4 may point to the limitations of the device in resistance state control, especially in application scenarios that require precise and significant resistance state differences. The 50 nm antimony selenide layer in Example 1 may provide the best electron transport path, which will neither hinder electron migration due to being too thick nor increase electron leakage due to being too thin.

[0079] like Figure 6-8 As shown, the stability of the high and low resistance states of the memristors of Example 2, Example 3, and Example 4 at different time points was tested. The results show that the resistance state transitions of these devices not only have a low switching ratio, but also show obvious instability over time.

[0080] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention is described in detail with reference to the embodiments, a person skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. An ultra-thin antimony selenide resistive layer memristor, characterized in that: The ultra-thin antimony selenide resistive layer memristor comprises a substrate, a resistive layer and a top electrode; wherein the substrate, the resistive layer and the top electrode are arranged from bottom to top; the resistive layer is a Sb2Se3 layer with a thickness of 30 to 100 nm.

2. The ultra-thin antimony selenide resistive layer memristor according to claim 1, characterized in that: The substrate is a glass substrate coated with a FTO layer.

3. The ultra-thin antimony selenide resistive layer memristor according to claim 1, characterized in that: The top electrode is a Ag layer.

4. The ultra-thin antimony selenide resistive layer memristor according to claim 3, characterized in that: The thickness of the Ag layer is 50 to 70 nm.

5. The ultra-thin antimony selenide resistive layer memristor according to claim 1, characterized in that: The thickness of the resistive layer is 40 to 60 nm.

6. The method for preparing the ultra-thin antimony selenide resistive layer memristor according to any one of claims 1 to 5, characterized in that: After cleaning and pre-treating the substrate, an antimony selenide resistive switching layer is grown on the upper surface of the FTO bottom electrode layer by using a rapid thermal evaporation method, and finally the electrode is evaporated.

7. The method for preparing the ultra-thin antimony selenide resistive layer memristor according to claim 6, characterized in that: The specific steps of growing an antimony selenide resistive switching layer on the surface of a glass substrate coated with an FTO layer by using a rapid thermal evaporation method are as follows: (1) Evenly covering the dried antimony selenide powder on a glass sheet; (2) Open the rapid annealing furnace chamber, install an AIN ceramic sheet on the heating table, and place a glass sheet covered with antimony selenide powder on the AIN ceramic sheet; (3) The glass substrate coated with the FTO layer after cleaning and pretreatment is placed opposite to the antimony selenide powder, and the distance between the FTO surface and the antimony selenide powder is 5 to 10 mm; (4) Evacuate the rapid annealing furnace chamber to 2.0×10 -3 Torr, antimony selenide powder and a glass substrate coated with an FTO layer are heated to 300°C; after a period of insulation, the antimony selenide powder and the glass substrate deposited with the FTO layer are heated to 580°C, and the growth time is 40 to 90 seconds; an antimony selenide film is grown on the upper surface of the FTO bottom electrode layer, and the thickness of the antimony selenide film is 30 to 100 nm.