Production method of glass fiber reinforced polyester resin composition

By adjusting parameters such as shear viscosity, die pressure, and temperature of the twin-screw extruder, the problem of wire breakage in the production of high glass fiber content polyester resin compositions was solved, achieving stable and efficient production of high-quality granules.

CN119032004APending Publication Date: 2024-11-26MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034594.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-22
Filing Date
2023-03-10
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When using a twin-screw extruder to produce glass fiber reinforced polyester resin compositions with high glass fiber content, the filament is prone to breakage, leading to unstable production, the generation of long granules and fragments, and affecting productivity.

Method used

By adjusting parameters such as shear viscosity, die pressure, die holder temperature, and wire cutting temperature, and combining these with the temperature settings of different mixing sections of the twin-screw extruder, the uniform mixing and extrusion of glass fiber and resin are ensured. Water cooling and wire cutting are used to obtain high-quality granules.

Benefits of technology

It has enabled the continuous and stable production of polyester resin compositions with high glass fiber content, significantly reducing wire breakage and the generation of long particles and fragments, and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032004A_ABST
    Figure CN119032004A_ABST
Patent Text Reader

Abstract

A method for producing a glass fiber-reinforced polyester resin composition comprising (A) 10 to 60 mass% of a polyester resin, (B) 40 to 70 mass% of glass fibers, and (C) 0 to 50 mass% of another polymer or additive using a twin screw extruder, the method being characterized in that: the resin composition has a shear viscosity of 400 to 2000 Pa.s at 265 DEG C and 91 / sec; the method comprises a first step of kneading (A) and (C) using a first kneading unit; a second step of adding (B) glass fibers and mixing using a second mixing unit; 3, reducing the pressure of an exhaust port, removing volatile matters, pressurizing, and extruding from a die mounted on a die holder; and 4, cooling the wire material leaving the mold by using water, and cutting the wire material by using a granulator, and extruding in a manner that the pressure of the resin in the mold in the third step is 2-9 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a glass fiber reinforced polyester resin composition, and more particularly to a method for producing a glass fiber reinforced polyester resin composition containing a high concentration of glass fibers by using a twin-screw extruder to produce pellets having a good pellet shape, wherein the method can suppress strand breakage, enable continuous and stable production, and have high productivity. Background Art

[0002] Polyester resins, such as polybutylene terephthalate resins and polyethylene terephthalate resins, are widely used in various electrical and electronic parts, mechanical parts, automobile parts, etc., mainly through injection molding. In particular, glass fiber-reinforced polyester resin compositions having a high glass fiber content have excellent mechanical strength, heat resistance, chemical resistance, etc., and are used as parts in the automotive field, the electrical and electronic equipment field, etc.

[0003] PTL 1 describes a resin composition in which glass fiber is mixed with a polybutylene terephthalate resin at a ratio of 5% to 80%, and PTL 2 describes a glass fiber reinforced polyester resin composition in which 10 to 150 parts by mass of glass fiber are mixed with 100 parts by mass of polyester resin.

[0004] However, polyester resin compositions mixed with high concentrations of glass fibers (e.g., 40% by mass or higher) are prone to strand breakage when extruded from a mold when produced with a twin-screw extruder. This reduces productivity, and when the broken strands enter the granulator, the strands tend to overlap each other, disrupting the flow of the strands and producing long pellets. In addition, the strands are not easy to cut, the cross-section of the pellets is not sharp, and more fragments are produced. This trend becomes more obvious as the concentration of glass fibers increases. Long pellets and fragments are prone to poor plasticization when molded with an injection molding machine, increasing metering time, causing the injection molding machine to shut down, and reducing productivity. Wire cut pellets are usually cylindrical or elliptical, but if the flattening rate of the ellipse becomes larger, plasticization may become unstable.

[0005] [Citation List]

[0006] [Patent Document]

[0007] [PTL 1] JP 1976-7702B

[0008] [PTL 2] JP 2006-16577A Summary of the invention

[0009] [Technical issues]

[0010] The problem (object) of the present invention is to suppress the breakage of strands coming out of a die, achieve continuous stable production, suppress the generation of long pellets, and suppress the generation of chips when producing a glass fiber reinforced polyester resin composition having a high glass fiber content using a twin-screw extruder.

[0011] [Technical solution]

[0012] In order to solve the above problems, the present inventors conducted extensive research and found that when a polyester resin composition having a glass fiber content of 40 to 70% by mass is produced using a twin-screw extruder, the viscosity of the resin composition becomes high, but by setting the shear viscosity to 400 Pa·s to 2000 Pa·s (265°C, 91 / sec) and setting the die pressure when extruding from a die to a range of 2 MPa to 9 MPa, strand breakage can be suppressed, continuous and stable production can be achieved, and the generation of long pellets and chips can be significantly suppressed. This discovery led to the creation of the present invention.

[0013] Furthermore, it was found that, in this case, it is preferred to set the die base temperature to a high temperature of 260°C to 340°C, and it is also preferred to set the temperature of the second kneading section (wherein the glass fiber (B) is kneaded after side feeding) to a low temperature of 150°C to 220°C, and to set the strand temperature when the strand is cut with a pelletizer to 100°C to 150°C.

[0014] The present invention relates to the following production method.

[0015] 1. A method for producing a glass fiber reinforced polyester resin composition using a twin-screw extruder, wherein the resin composition comprises (A) 10% to 60% by mass of a polyester resin, (B) 40% to 70% by mass of glass fibers, and (C) 0% to 50% by mass of other polymers or additives, wherein the sum of the components is 100% by mass,

[0016] The shear viscosity of the resin composition at 265° C. and 91 / s is 400 Pa·s to 2000 Pa·s.

[0017] The method comprises: a first step of mixing the polyester resin (A) and the other polymer or additive (C) in a first mixing section; a second step of adding the glass fiber (B) to be mixed in a second mixing section downstream of the first mixing section; a third step of decompressing the exhaust port downstream of the second mixing section to remove volatiles and increase the pressure, and then extruding from a die attached to a die base; and a fourth step of water cooling the strands coming out of the die and cutting the strands with a pelletizer,

[0018] In the third step, the pressure at the screw tip is increased and extrusion is performed, so that when the resin composition comes out of the mold, the resin pressure in the mold is 2 MPa to 9 MPa.

[0019] 2. The production method according to item 1 above, wherein the mold base temperature in the third step is 260°C to 340°C.

[0020] 3. The production method according to 1 or 2 above, wherein the barrel temperature in the second kneading zone in the second step is 150°C to 220°C.

[0021] 4. The production method according to item 1 above, wherein the strand temperature when the strand is cut by a pelletizer in the fourth step is 100°C to 150°C.

[0022] [Beneficial Effects of the Invention]

[0023] According to the production method of the present invention, a glass fiber reinforced polyester resin composition (pellets) having a high glass fiber content can be produced while suppressing strand breakage, achieving continuous stable production, and significantly suppressing the generation of long pellets and chips. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a conceptual diagram showing an example of the steps from the twin-screw extruder to the pelletizer used in the present invention.

[0025] Figure 2 This is a conceptual diagram of the screw configuration of the extruder used in Examples and Comparative Examples. DETAILED DESCRIPTION

[0026] The present invention will be described in detail below with reference to embodiments, exemplary products, etc., but the present invention is not limited to the embodiments, exemplary products, etc. shown below, and can be freely modified without departing from the gist of the present invention. The word "to" in this specification, when referring to a range, means including the values ​​before and after it as the lower limit and upper limit.

[0027] In the production method of the present invention, a twin-screw extruder is used to produce a glass fiber reinforced polyester resin composition, which comprises (A) 10% to 60% by mass of a polyester resin, (B) 40% to 70% by mass of glass fibers, and (C) 0% to 50% by mass of other polymers or additives.

[0028] The extruder used in the present invention is a vented twin-screw extruder, preferably a co-rotating twin-screw extruder having two co-rotating screws in a barrel, and preferably a mixing section composed of a plurality of mixing disks intermeshing with each other in the middle of the screws.

[0029] like Figure 1As shown, the venting twin-screw extruder has a die base 8 at the end of the barrel, and the barrel is provided with a main raw material hopper 1, an open exhaust port 2, a side feed hopper 3 and a decompression exhaust port 4. A flange 6 is provided between the barrel and the die base. The screw in the barrel is driven to rotate by a motor 16 through a screw connection 14 and a gear box 15. A ring plate or a crushing plate is connected between the flange 6 and the die base 8 to prevent resin leakage. With the die base, the resin is diffused and discharged from the mold (having multiple nozzles) in the form of strands. Usually, the resin diffuses horizontally in the die base part and is discharged in the form of strands 10 from multiple nozzles (called flat dies) arranged horizontally side by side.

[0030] The flange 6 is sometimes also called a hinge plate. In addition, the die base is sometimes also called a template. The flange 6 (or hinge plate) and the die base 8 (or template) are usually called a die head. In order to stably produce the glass fiber reinforced polyester resin composition, that is, to suppress the breakage of the strand, the die base temperature is also important.

[0031] The polyester resin (A) and other polymers or additives (C) are supplied from the main raw material hopper 1 and mixed in the first mixing section (the first step). The glass fiber (B) is side-fed from the side feed hopper 3 located downstream of the first mixing section and mixed in the second mixing section (the second step). Next, the exhaust port 4 is decompressed downstream of the second mixing section to remove volatiles and increase the pressure, and extruded from a die attached to a die base 8 (the third step). The strands 10 coming out of the die are water-cooled and cut by a pelletizer 11 (the fourth step) to obtain pellets 12 of the resin composition.

[0032] In step 1, polyester resin (A) and other polymers or additives (C) are fed from the main raw material hopper 1 into the extruder, and heated, mixed and melted by the screw. The first mixing section composed of multiple mixing discs is formed in the middle of the screw. The first mixing section is a mixing section where the polyester resin (A) and other polymers or additives (C) are mixed after they are introduced, and refers to the mixing section before the glass fiber (B) is added. The screw structure is preferably a combination of two or more of R mixing discs, N mixing discs, L mixing discs, L screws, sealing rings, mixing screws or rotor screws, and the screw length is preferably 5.0D to 9.0D (D is the barrel diameter). The first mixing section is a mixing section where the polyester resin (A) and other polymers or additives (C) are mixed when they are introduced, and this mixing section is before the glass fiber (B) is added.

[0033] The first kneading section may be a single integrated section or may be divided into several sections. That is, the first kneading section may also be divided, and a feed screw may be inserted between the divided sections. Even if there are divided sections, the total length of the kneading section is preferably in the range of 5.0D to 9.0D.

[0034] The R mixing disk (hereinafter sometimes referred to as R) is a forward feeding mixing disk element, which generally has two or more blades, and the blade twist angle θ is preferably 10 degrees to 75 degrees. By setting the blades at a predetermined angle offset in this way, a pseudo screw structure is formed, and a strong shear force is applied while the resin is sent out in the feeding direction, thereby forming an area for mixing.

[0035] The L mixing disk (hereinafter sometimes referred to as L) is a reverse feeding mixing disk element, which generally has two or more blades, and its blade twist angle θ is preferably -10 degrees to -75 degrees. The reverse mixing disk element can block the resin being fed, or increase the pressure acting in the direction of sending the resin back. By installing the reverse mixing disk downstream of the element that promotes mixing, the resin is blocked and a strong mixing effect is exhibited.

[0036] The N mixing disk (hereinafter sometimes referred to as N) is an orthogonal mixing disk element, usually having two or more blades, and the blade twist angle θ is 75 to 105 degrees. Since the blades are installed with an offset of about 90 degrees, the force for sending out the resin is weak, but the mixing force is strong.

[0037] The L screw is a reverse feed screw, the sealing ring restricts the flow of the upstream section through the gap of the sealing ring section, the mixing screw is a screw element with the top of the screw (thread section) cut off, and the rotor screw is a screw element with one or more threads on the outer circumference.

[0038] Among them, the R kneading disk, the N kneading disk, and the L kneading disk are preferred, and a configuration having a combination of a plurality of these kneading disks is preferred.

[0039] The screw configuration of the first kneading section of the first step is preferably such that an element that promotes kneading is placed on the upstream side, and an element having a pressurizing capability is placed on the downstream side. Therefore, in the first kneading section, it is preferred to place two or more kneading disks selected from R, N, and L in the order of R→N→L from the upstream side, and it is also preferred to place a plurality of R, N, and L, respectively. It is particularly preferred to place R upstream, then place a plurality of N, and then place L.

[0040] The screw length of the first mixing section is preferably in the range of 5.0D to 9.0D, where D is the barrel diameter. By using such a screw length, the melt plasticization of the polyester resin (A) is sufficient, and the decomposition of the resin composition can be suppressed. When the screw length of the first mixing section is less than 5.0D, the melt plasticization of the resin is likely to be insufficient due to insufficient shearing, and when the screw length of the first mixing section exceeds 9.0D, due to excessive mixing, local decomposition of the resin composition is likely to proceed, and the mechanical properties of the composition are likely to decrease.

[0041] In the first step, after the polyester resin (A) is kneaded and melted, it is preferably exhausted using the exhaust port 2. A seal ring is preferably provided downstream of the exhaust port 2.

[0042] In the second step, after the first step, glass fiber (B) is fed from the side feed hopper 3 located downstream of the first kneading section, and the glass fiber (B) is kneaded with the molten polyester resin (A) in the second kneading section.

[0043] The second mixing section refers to the mixing section where the glass fiber (B) enters and is opened and mixed. The screw structure of the second mixing section preferably has one or a combination of two or more of an R mixing disk, an N mixing disk, an L mixing disk, an L screw, a sealing ring and a mixing screw. By mixing with such a screw structure, the glass fiber (B) is easily opened and dispersed. Among them, it is preferred to have at least a mixing screw structure, especially a forward feeding grooved mixing screw and a reverse feeding grooved mixing screw.

[0044] The screw length of the second mixing section is preferably in the range of 2.5D to 5.0D. The second mixing section can be integrated into one section or divided into several sections. That is, the second mixing section can also be divided and the feed screw can be inserted between the divided sections. Regardless of the structure, the total length of the mixing section is preferably in the range of 2.5D to 5.0D. By setting the screw length of the second mixing section in this way, the fiber opening and dispersion of the glass fiber (B) are improved, and the strength of the resin composition may also be improved.

[0045] The resin temperature (barrel temperature) in the second step is usually set to about 260°C, but in the method of the present invention, it is preferably set to a lower temperature than usual, for example, 150°C to 220°C. In the step implemented in the second mixing section, the glass fiber (B) is introduced and mixed with the polyester resin (A) and other polymers or additives (C), and the resin temperature may increase. Setting the barrel temperature in this section to a temperature range lower than the usual temperature, for example, 150°C to 220°C, can effectively suppress the breakage of the strand 10 when it comes out of the die base 8. When the temperature is lower than 150°C, the viscosity of the resin increases, resulting in poor impregnation of the glass fiber (B), uneven mixing, and easy breakage of the strand. At the same time, when the temperature is higher than 220°C, the resin temperature tends to increase, thermal decomposition gas is easily generated, and the strand is easily broken. The resin temperature (barrel temperature) in the second step is more preferably above 160°C and below 210°C.

[0046] The screw speed of the twin-screw extruder is preferably 250 rpm to 800 rpm, more preferably 300 rpm to 700 rpm. For TEX44αIII, the discharge is preferably 200 kg / h to 650 kg / h, more preferably 250 kg / h to 630 kg / h. For extruders of different sizes, the preferred range of discharge is proportional to the 2.5th power of the barrel diameter ratio.

[0047] In the third step after the second step, the pressure reduction vent 4 is decompressed downstream of the second kneading section to remove volatiles and increase the pressure, and extruded from a die attached to a die holder 8. The vacuum degree when reducing pressure and removing volatiles at the pressure reduction vent 4 is preferably -0.097 MPa to -0.07 MPa. Here, the vacuum degree refers to the gauge pressure.

[0048] In the third step, the pressure is increased at the screw tip, and extrusion is performed so that the resin pressure in the mold is 2 MPa to 9 MPa when the resin comes out of the mold.

[0049] The resin pressure in the mold (also referred to as mold pressure) refers to the resin pressure at the position of the screw tip portion. The pressure at this position is the highest. Usually, a flange is provided at this position, and a resin pressure gauge 7 is installed so that the pressure can be measured over time. The resin pressure in the mold is preferably above 2MPa and below 9MPa. The glass fiber (B) is usually supplied in a bundle. By setting the resin pressure in the mold to above 2MPa and below 9MPa, the glass fiber is mixed with the resin. By applying appropriate pressure, the resin is easily impregnated into the glass fiber (B) bundle, so that uniform mixing can be achieved, and it is easier to suppress the occurrence of strand breakage. When the resin pressure in the mold is less than 2MPa, the mixing state of the resin and the glass fiber (B) is uneven, and the strand is easy to break when it comes out of the mold. The resin pressure in the mold is more preferably above 2.5MPa, and even more preferably above 3MPa. On the other hand, when the resin pressure is too high, the retention area of ​​the screw tip becomes longer, and it is easy to generate gas due to thermal decomposition, and the strand is easy to break due to gas when it comes out of the mold. The resin pressure is more preferably 8 MPa or less, and even more preferably 7 MPa or less.

[0050] The temperature of the die base 8 is preferably higher than usual, preferably 260°C or higher and 340°C or lower. By setting such a temperature, it is easier to suppress the strands from breaking. If the die base temperature is lower than 260°C, the mold temperature is lower than the resin temperature of the resin composition, and the temperature of the strands at both ends of the mold is lower than the temperature of the strands in the center. This causes a difference in viscosity between the strands, making them more likely to break. The temperature of the die base 8 is more preferably 270°C or higher, and even more preferably 280°C or higher. If the die base temperature exceeds 340°C, gas is more likely to be generated due to heat retention inside the mold, and the strands are also more likely to break. The temperature of the die base 8 is more preferably 330°C or lower. Even more preferably 320°C or lower.

[0051] The second kneading section thermocouple 5 and the die base thermocouple 9 are respectively inserted into the barrel and die base 8 of the extruder, so that the temperature of the barrel and the die base can be measured. In addition, a heater is built into the barrel and the die base to control the temperature. The temperature of the barrel and the die base is the temperature measured by the inserted thermocouple.

[0052] In the fourth step, the strand 10 coming out of the mold is cooled with water and cut with a pelletizer 11. The strand temperature when the strand is cut is preferably above 100°C and below 150°C. By setting the temperature at such a level, it is easier to prevent the generation of fragments and poorly shaped pellets. If the temperature is lower than 100°C, the strand will become hard and fragments will easily be generated when cut with a pelletizer. This makes plasticization unstable during molding processes such as injection molding. If the temperature exceeds 150°C, the flatness of the elliptical cylindrical shape of the cut pellets becomes large, which can also lead to poor plasticization. The strand temperature when the strand is cut is more preferably above 110°C and below 140°C.

[0053] The glass fiber reinforced polyester resin composition containing a high concentration of glass fiber is easy to break after coming out of the mold and before cooling and strand cutting. In this case, the amount of the resin component is small, the viscoelasticity becomes weak, and the strand loses toughness, becomes brittle and easily breaks. In addition, due to the large amount of glass fiber, a fiber bundle with poor fiber opening tends to be produced. The fiber bundle with poor fiber opening is easy to become the starting point of the break during the stretching (extension) of the strand. In addition, when there is little resin filled in the fiber bundle, this part can become the starting point of the break (insufficient resin impregnation of the glass fiber bundle). In addition, due to the high concentration of glass fiber, the viscosity of the resin increases, and the resin temperature is easy to rise. This will produce thermal decomposition gas, causing the strand to break when it comes out of the mold. Therefore, it is difficult to stably cut the strand due to the decrease in strand toughness, insufficient fiber opening of the glass fiber bundle, insufficient resin impregnation of the glass fiber bundle, gas generation, etc. When the strand breaks, the strand must be manually put back into the pelletizer. At this time, the flow of all strands will be disturbed, and the strand will enter the cutter at a certain angle, so longer pellets may be produced. In addition, due to the high concentration of glass fibers and the hardness of the strands, the cut surface produced by the granulator will become blunt instead of sharp, and cut fragments will be produced. In order to suppress the generation of cut fragments, the strand cutting temperature must be increased. This will make the cutting sharp and reduce fragments. However, if the strand cutting temperature is too high, the strand will become soft and be crushed by the winding roller of the granulator, increasing the eccentricity of the elliptical rod-shaped pellets. The more long pellets and fragments there are, the greater the flatness, and the more likely it is that poor plasticization will occur when the pellets are used for injection molding, resulting in reduced productivity. The number of long pellets (usually with a length equal to or greater than twice the length of the pellets) is preferably 5 or less per 1kg. The amount of fragments is preferably 300 mass ppm or less of the total mass (pellets + fragments). The flatness (major axis / minor axis) is preferably 1.30 or less.

[0054] The shape of the extrusion die is not particularly limited, and a known die can be used. The die aperture depends on the desired pellet size, but is generally about 2 to 5 mm, preferably about 3 to 4 mm.

[0055] The strand 10 is taken up by the take-up roller, and is cooled by contact with water. The method of contacting with water may be cooling by water stored in the cooling water tank 13, cooling by contacting the strand 10 with water, pulling the strand with a mesh belt conveyor, and spraying water on it with a water spray device. The time from the strand being extruded from the die to being cooled with water or immersed in water is preferably short. Generally, it is preferred to immerse the strand in water within 1 second after being extruded from the die.

[0056] The cooled strands are sent to the pelletizer via a take-up roller, cut and made into pellets.

[0057] In the method of the present invention, the shear viscosity of the glass fiber reinforced polyester resin composition at 265°C and 91 / second is 400Pa·s or more and 2000Pa·s or less. By setting the viscosity within the range of 400Pa·s to 2000Pa·s and combining it with the above steps, it is possible to suppress the breakage of the strands and achieve continuous and stable production. When the viscosity is lower than 400Pa·s, the elasticity of the strands is weak and the strands are prone to breakage. In addition, when the viscosity exceeds 2000Pa·s, shear heat generation increases, the resin temperature rises, thermal decomposition occurs, and the strands are prone to breakage. A more preferred range is 500Pa·s or more and 1700Pa·s or less, a more preferred range is 600Pa·s or more, and preferably 1400Pa·s or less.

[0058] The shear viscosity is a value measured at 265° C. and a shear rate of 9 1 / sec in accordance with JIS K7199 using a capillograph having an orifice of 1 mm in capillary diameter and 3 mm in capillary length (Capillograph 1D2 manufactured by Toyo Seiki Co., Ltd.).

[0059] In order to adjust the shear viscosity to the above range, the shear viscosity can be increased by increasing the amount of glass fiber (B), and the shear viscosity can be reduced by reducing the amount of glass fiber. Another method is to adjust the amount and viscosity of other polymers (C) to be mixed, such as styrene polymers and polycarbonate resins. The shear viscosity can also be adjusted by changing the viscosity of the polyester resin (A).

[0060] Next, the raw material components used in the present invention will be described.

[0061] Polyester resin (A)

[0062] The polyester resin (A) is a thermoplastic polyester resin which is a polyester obtained by polycondensation of a dicarboxylic acid compound and a dihydroxy compound, polycondensation of a hydroxycarboxylic acid compound, or polycondensation of these compounds, and may be a homopolyester or a copolyester.

[0063] As the dicarboxylic acid compound constituting the polyester resin (A), an aromatic dicarboxylic acid or an ester-forming derivative thereof is preferably used.

[0064] Examples of the aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, 1,5-naphthalene dicarboxylic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, biphenyl-2,2′-dicarboxylic acid, biphenyl-3,3′-dicarboxylic acid, biphenyl-4,4′-dicarboxylic acid, diphenyl ether-4,4′-dicarboxylic acid, diphenylmethane-4,4′-dicarboxylic acid, diphenyl sulfone-4,4′-dicarboxylic acid, diphenylisopropylmethylene-4,4′-dicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4′-dicarboxylic acid, anthracene-2,5-dicarboxylic acid, anthracene-2,6-dicarboxylic acid, p-terphenyl-4,4′-dicarboxylic acid and pyridine-2,5-dicarboxylic acid, among which terephthalic acid is preferably used.

[0065] Two or more of these aromatic dicarboxylic acids may be used in combination. It is well known that, in addition to the free acid, dimethyl esters and the like can be used as ester-forming derivatives in polycondensation reactions.

[0066] One or more of aliphatic dicarboxylic acids such as adipic acid, azelaic acid, dodecanedioic acid and sebacic acid and one or more of alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid may be used in combination with these aromatic dicarboxylic acids, but in a smaller amount.

[0067] Examples of the dihydroxy compound constituting the polyester resin (A) include aliphatic diols such as ethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, 2-methylpropane-1,3-diol, diethylene glycol and triethylene glycol, alicyclic diols such as cyclohexane-1,4-dimethanol, and mixtures thereof.

[0068] It is also possible to copolymerize one or more long-chain diols having a molecular weight of 400 to 6,000, such as polyethylene glycol, poly-1,3-propylene glycol, and polytetramethylene glycol, as long as the amount thereof is small.

[0069] Furthermore, aromatic diols such as hydroquinone, resorcinol, naphthalene diol, dihydroxydiphenyl ether, and 2,2-bis(4-hydroxyphenyl)propane may be used.

[0070] In addition to the above-mentioned bifunctional monomers, a small amount of trifunctional monomers such as trimellitic acid, trimesic acid, pyromellitic acid, pentaerythritol and trimethylolpropane can be used to introduce a branched structure, or monofunctional compounds such as fatty acids can be used to adjust the molecular weight.

[0071] Usually, as the polyester resin (A), a polyester resin mainly composed of a polycondensate of a dicarboxylic acid and a diol is used, i.e., 50% by mass or more, preferably 70% by mass or more of the entire polyester resin is composed of the polycondensate. The dicarboxylic acid is preferably an aromatic dicarboxylic acid, and the diol is preferably an aliphatic diol.

[0072] Among them, polyalkyl terephthalate in which 95 mol% or more of the acid component is terephthalic acid and 95 mass% or more of the alcohol component is aliphatic diol is preferred. Representative examples thereof include polybutylene terephthalate resin and polyethylene terephthalate resin. These are preferably close to homopolyesters, that is, 95 mass% or more of the entire resin is composed of terephthalic acid component and 1,4-butanediol or ethylene glycol component.

[0073] The main component (ie, 50% by mass or more) of the polyester resin (A) is preferably a polybutylene terephthalate resin or a polyethylene terephthalate resin, and particularly preferably a polybutylene terephthalate resin.

[0074] The intrinsic viscosity of the polyester resin (A) is preferably 0.60 dl / g or more and less than 1.0 dl / g, more preferably 0.60 dl / g or more and less than 0.95 dl / g, and even more preferably 0.65 dl / g or more and less than 0.95 dl / g. When a polyester resin having an intrinsic viscosity of less than 0.60 dl / g is used, the mechanical strength of the resulting resin composition tends to be low, the hydrolysis resistance tends to be poor, and the thermal shock resistance tends to be low. When the intrinsic viscosity is 1.0 dl / g or more, good fluidity is unlikely to be obtained.

[0075] The intrinsic viscosity of the polyester resin is a value measured at 30° C. in a mixed solvent of 1,1,2,2-tetrachloroethane and phenol at a ratio of 1:1 (mass ratio).

[0076] In addition, the amount of terminal carboxyl groups of the polyester resin (A) can be appropriately selected and determined, but is generally 60 equivalents / ton or less, preferably 50 equivalents / ton or less, and more preferably 30 equivalents / ton or less. When the amount exceeds 60 equivalents / ton, gas is easily generated during the melt molding process of the resin composition. The lower limit of the amount of terminal carboxyl groups is not particularly limited, but is generally 10 equivalents / ton in consideration of the production efficiency in the production of the polyester resin.

[0077] The amount of terminal carboxyl groups of the polyester resin refers to the value measured by dissolving 0.5 g of the polyalkylene terephthalate resin in 25 mL of benzyl alcohol and titrating with a 0.01 mol / L sodium hydroxide benzyl alcohol solution. The amount of terminal carboxyl groups can be adjusted by a freely selected conventional method, for example, by adjusting polymerization conditions such as the raw material feed ratio, polymerization temperature, and decompression method during polymerization, or by reacting with a terminal blocking agent.

[0078] Glass fiber(B)

[0079] As the glass fiber (B), any known glass fiber can be used as long as such fiber is generally used in polyester resins regardless of the form of the glass fiber when blended, such as A glass, E glass, an alkali-resistant glass composition containing a zirconium oxide component, chopped strands, roving glass, a masterbatch of a thermoplastic resin and glass fiber, etc. Among them, as the glass fiber (B) used in the present invention, alkali-free glass (E glass) is preferred for the purpose of improving the thermal stability of the resin composition.

[0080] It is also preferable to use glass fibers (B) having a longitudinal cross-sectional profile ratio within a range of 2.0 to 6.0.

[0081] The irregularity ratio of the longitudinal section is the ratio of the major diameter to the minor diameter when a minimum area rectangle is assumed to enclose the cross section perpendicular to the longitudinal direction of the glass fiber, with the length of the long side of the rectangle as the major diameter and the length of the short side as the minor diameter.

[0082] The cross-sectional area of ​​the glass fiber (B) in the longitudinal direction is preferably greater than 90 μm 2 And not more than 300μm 2 With such a cross-sectional area, the polyester resin can be easily made into a matrix, and as a result, the heat resistance can be easily improved. More preferably, the cross-sectional area is larger than 90 μm 2 And not more than 250μm 2 , even more preferably greater than 90 μm 2 And not more than 200μm 2 .

[0083] The thickness of the glass fiber (B) is not particularly limited, but it is preferred that the minor diameter is about 2 to 20 μm and the major diameter is about 5 to 50 μm.

[0084] The glass fiber (B) may be treated with a sizing agent or a surface treatment agent. In addition, in the production of the resin composition of the present invention, a sizing agent or a surface treatment agent may be added separately from the untreated glass fiber to perform surface treatment.

[0085] Examples of the sizing agent include resin emulsions such as vinyl acetate resins, ethylene / vinyl acetate copolymers, acrylic resins, epoxy resins, polyurethane resins, and polyester resins.

[0086] Examples of the surface treatment agent include aminosilane compounds such as γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane and γ-(2-aminoethyl)aminopropyltrimethoxysilane; chlorosilane compounds such as vinyltrichlorosilane and methylvinyldichlorosilane; alkoxysilane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane and γ-methacryloxypropyltrimethoxysilane; epoxysilane compounds such as β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane, acrylic compounds, isocyanate compounds, titanate compounds and epoxy compounds.

[0087] Two or more of these sizing agents and surface treatment agents may be used in combination, and their usage (attachment amount) is usually 10% by mass or less, preferably 0.05% by mass to 5% by mass, of the mass of the glass fiber (B). By setting the attachment amount to 10% by mass or less, necessary and sufficient effects can be obtained, and cost efficiency is achieved.

[0088] Two or more types of glass fibers (B) may be used in combination depending on the desired properties.

[0089] The content of the glass fiber (B) is set to 40% to 70% by mass relative to the total amount of the polyester resin (A), the glass fiber (B) and other polymers or additives (C) as 100% by mass. If the content of the glass fiber (B) is less than 40% by mass, the rigidity may be insufficient, and conversely, if the content of the glass fiber exceeds 70% by mass, the impact resistance and fluidity may be insufficient, and production problems may occur. The content of the glass fiber (B) is more preferably 42% by mass or more, more preferably 65% ​​by mass or less, and even more preferably 60% by mass or less.

[0090] The other polymer or additive (C) is other polymer different from the polyester resin (A) and / or various other additives.

[0091] Examples of other additives include various resin additives, such as fillers other than the glass fiber (B) (talc, glass flakes, mica, kaolin, ceramic beads, clay, zeolite, barium sulfate, titanium oxide, silicon oxide, aluminum oxide, magnesium hydroxide, zinc sulfide, etc.), flame retardants, flame retardant aids, stabilizers, antioxidants, mold release agents, ultraviolet absorbers, weather stabilizers, lubricants, colorants such as dyes and pigments, catalyst deactivators, antistatic agents, foaming agents, plasticizers, crystal nucleating agents, crystallization accelerators, etc.

[0092] Examples of other polymers include various elastomers, styrene polymers described below, polycarbonate, polyolefins such as polyethylene and polypropylene, polyamide, polyimide, polyetherimide, polyphenylene ether, polyphenylene sulfide, polysulfone, polymethacrylate resin, and the like.

[0093] One other type of resin may be included, or two or more types of resins may be included in freely selected combinations and ratios.

[0094] The amount of other polymers or additives (C) is 0 to 50% by mass based on 100% by mass of the total amount of (A) to (C), and is preferably 45% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less, and is preferably 1% by mass or more, more preferably 2% by mass or more, and within this range is 3% by mass or more and 4% by mass or more, and particularly preferably 5% by mass or more.

[0095] Examples of styrene-based polymers include homopolymers of styrene, graft copolymers obtained by polymerizing styrene in the presence of rubber, copolymers of styrene and (meth)acrylonitrile, copolymers of styrene and alkyl (meth)acrylates, copolymers of styrene, (meth)acrylonitrile and other copolymerizable monomers, graft copolymers obtained by graft polymerization of styrene and (meth)acrylonitrile in the presence of rubber, and the like. Specifically, polystyrene (general purpose polystyrene, GPPS), impact-resistant polystyrene (high impact polystyrene, HIPS), acrylonitrile-styrene copolymer (AS resin), acrylonitrile-butadiene-styrene copolymer (ABS resin), styrene-butadiene-styrene copolymer (SBS resin), hydrogenated styrene-butadiene-styrene copolymer (hydrogenated SBS), hydrogenated styrene-isoprene-styrene copolymer (SEPS), styrene-maleic anhydride copolymer (SMA resin), acrylonitrile-styrene-acrylic rubber copolymer (ASA resin), methyl methacrylate-butadiene-styrene copolymer (MBS resin), methyl methacrylate-acrylonitrile-butadiene-styrene copolymer (MABS resin), acrylonitrile-acrylic rubber-styrene copolymer (AAS resin), acrylonitrile-ethylene propylene rubber-styrene copolymer (AES resin) and styrene-IPN rubber copolymer, and mixtures thereof.

[0096] Among them, acrylonitrile-styrene copolymer (AS resin), polystyrene (GPPS), high impact polystyrene (HIPS) and acrylonitrile-butadiene-styrene copolymer (ABS resin) are preferred, and acrylonitrile-styrene copolymer (AS resin), polystyrene (GPPS), high impact polystyrene (HIPS) and acrylonitrile-butadiene-styrene copolymer (ABS resin) are particularly preferred.

[0097] As the styrene-based polymer, a styrene-based elastomer may also be used.

[0098] As the styrene-based polymer, a block copolymer composed of a polymer block having a vinyl aromatic compound as a polymerization component and a polymer block having a conjugated diene as a polymerization component, and a hydrogenated product thereof are preferred.

[0099] Examples of the vinyl aromatic compound constituting the polymer block of the vinyl aromatic hydrocarbon include styrene and its derivatives, such as styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 1,3-dimethylstyrene, lower alkyl-substituted styrene, vinylnaphthalene, vinylanthracene, etc. These may be used alone or in combination of two or more.

[0100] Examples of the conjugated diene constituting the conjugated diene block include butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, and the like.

[0101] The styrene-based polymers may be used alone or in combination of two or more.

[0102] The amount of the styrene-based polymer is preferably 5 to 45% by mass based on 100% by mass of the total amount of (A) to (C).

[0103] The polycarbonate resin is preferably an aromatic polycarbonate resin, specifically a thermoplastic aromatic polycarbonate polymer or copolymer obtained by reacting an aromatic dihydroxy compound with phosgene or a carbonic acid diester.

[0104] Examples of the aromatic dihydroxy compound include 2,2-bis(4-hydroxyphenyl)propane (bisphenol A) and tetramethylbisphenol A.

[0105] In a preferred example of the polycarbonate resin, the dihydroxy compound is 2,2-bis(4-hydroxyphenyl)propane or a combination of 2,2-bis(4-hydroxyphenyl)propane and other aromatic dihydroxy compounds.

[0106] The polycarbonate resin may be a homopolymer composed of one repeating unit, or a copolymer having two or more repeating units. In this case, the copolymer may be selected from various copolymerization forms such as a random copolymer and a block copolymer.

[0107] The molecular weight of the polycarbonate resin is not limited, but the viscosity average molecular weight (Mv) is generally about 10,000 to 100,000, preferably about 12,000 to 35,000. By setting the viscosity average molecular weight to be greater than the lower limit of the above range, the mechanical strength can be further improved, making it more suitable for applications requiring high mechanical strength.

[0108] The viscosity average molecular weight (Mv) of the polycarbonate resin is a value calculated by measuring the viscosity of a dichloromethane solution of the polycarbonate resin at 25° C. using an Ubbelohde viscometer to determine the limiting viscosity ([η]), and then using the following Schnell viscosity formula.

[0109] [η] = 1.23 × 10 -4 Mv 0.83

[0110] The production method of the polycarbonate resin is not particularly limited, and polycarbonate resins produced by the phosgene method (interfacial polymerization method) or the melt method (ester exchange method) can be used. In addition, polycarbonate resins produced by the melt method and post-treated to adjust the amount of terminal OH groups are also preferred.

[0111] In addition, the polycarbonate resin can be made not only from virgin raw materials, but also aromatic polycarbonate resins regenerated from waste products, i.e., so-called material-recycled aromatic polycarbonate resins. Examples of waste products include optical recording media such as optical discs and light guide plates, transparent vehicle parts such as automobile window glass, automobile headlight lenses, and windshields, containers such as water bottles and eyeglass lenses, and building parts such as soundproof walls, glass windows, and corrugated boards. In addition, as the recycled polycarbonate resin, crushed products obtained by rejecting products, gates, or runners, or pellets obtained by melting them can also be used.

[0112] When the polycarbonate resin is contained, the content thereof is preferably 5 to 45% by mass based on 100% by mass of the total amount of (A) to (C).

[0113] The glass fiber reinforced polyester resin composition produced by the method of the present invention can be molded into high-strength products, so it can fully meet the performance requirements of lightweight, thin, and strong, and can be widely used in molded products or parts in various industrial fields such as electrical and electronic equipment, office automation equipment such as computers, precision equipment, optical equipment, and automobiles.

[0114] [Example]

[0115] The present invention will be described in more detail below in conjunction with the following embodiments. However, the present invention is not limited to the following embodiments and can be modified as needed without departing from the scope of the present invention.

[0116] The polyester resin (A), glass fiber (B) and other polymers (C) used as raw materials in the examples and comparative examples are shown in Table 1 below.

[0117] [Table 1]

[0118]

[0119] In the following Examples and Comparative Examples, a vented intermeshing co-rotating twin-screw extruder (manufactured by Japan Steel Works Ltd., "TEX44αIII", barrel diameter D = 47 mm) was used as the extruder.

[0120] Screw configuration such as Figure 2 shown.

[0121] C1 is a feed barrel, C7 and C12 are exhaust barrels, C7 is an open exhaust port, C12 is a reduced pressure exhaust port, and C9 is a side feed barrel. The first mixing section for melt mixing polyester resin (A) and other polymers (C) is arranged from C5 to C6, and the screw has a 5-blade RRNNL configuration, each blade has 1D (1D = 44mm). Glass fiber (B) is fed from the side of C9. In the second mixing section for mixing glass fiber (B), as shown in Figure 2 As shown, 5 blades R (1D) and 3 anti-mixing screws of the same 1D (lead 0.25D) are configured.

[0122] The mixing section where the polyester resin (A) and other polymers (C) are added and extends to where the glass fiber (B) is fed is the first mixing section, and the first step is C1 to C9.

[0123] Next, the mixing section where the glass fiber (B) enters the extruder and extends to the reduced pressure exhaust port is the second mixing section, and the second step is C10 to C11. The third step is C12 to C14, and the mixed resin comes out of the mold, including the mold base. In addition, in the fourth step, the strands coming out of the mold are cooled with water and cut with a pelletizer to obtain pellets.

[0124] The following Examples 1 to 11 and Comparative Examples 1 and 2 were used to produce resin compositions according to the raw material ratios shown in Formulation 1 of Table 1 above.

[0125] Example 1

[0126] The total amount of 57.5 kg / h of polybutylene terephthalate resin (PBT2), 45 kg / h of polyethylene terephthalate resin (PET) and 10 kg / h of elastomer (EL) was fed from the main raw material hopper into the feed barrel C1 of the twin screw extruder "TEX44αIII", and 137.5 kg / h of glass fiber (GF) was fed from the side feed hopper into the side feed barrel C9. The total feed amount of raw materials was 250 kg / h, and the screw speed was 300 rpm.

[0127] The set temperature of barrels C2-C9, C12-C14 is 250℃. The set temperature of barrels C10 and C11 in the second mixing stage is 170℃. The set temperature of the die base in the third step is 300℃. The temperature of the flange is also set to 300℃, the same as the die base. The mold used is a flat mold with 10 holes arranged horizontally side by side, the hole diameter is 3.8mm, and the flange length is 20mm. At this time, the resin pressure in the mold is 5.2MPa.

[0128] In the following embodiments and comparative examples, the temperature of the flange is the same as that of the mold base.

[0129] The strands coming out of the die were cooled in a water bath and cut into strands by a pelletizer to obtain 3 mm long elliptical cylindrical pellets. The strand pulling speed of the pelletizer was 40 m / min. At this time, the water cooling distance of the strands was adjusted, and the strand temperature when cutting was set to 130°C. The temperature of the strands was measured with an infrared thermometer. The extrusion lasted for 1 hour. Within 1 hour, no strands broke.

[0130] The dimensions of the obtained elliptical columnar pellets were as follows: the average length of 20 pellets was 3.0 mm, the major axis was 3.0 mm, and the minor axis was 2.4 mm (flattening ratio: 1.25).

[0131] A total of 1 kg of pellets were collected and the amount of fragments was measured using a 1 mm mesh sieve to determine the fragment rate (ppm by mass). The pellets remaining on the sieve (about 1 kg) were visually inspected and the number of long pellets (pellets with a length equal to or greater than 6 mm) was calculated. These results are shown in the table.

[0132] The amount of debris was very small, and there were no long particles. The flatness of the elliptical columnar particles was 1.25, which was good.

[0133] The obtained pellets were dried at 120°C for 5 hours, and the shear viscosity was measured at a temperature of 265°C and a shear rate of 91 / sec using a "Capilograph 1D2" (manufactured by Toyo Seiki Seisakusho Co., Ltd.) with an orifice having a capillary diameter of 1 mm and a capillary length of 3 mm. The shear viscosity was 1020 Pa·s.

[0134] The results are shown in Table 2.

[0135] The strand breakage evaluation was performed according to the following criteria.

[0136] A: Wire breakage 0 times / hour

[0137] B: Wire breakage 1-2 times / hour

[0138] C: Wire breakage 3 to 9 times / hour

[0139] D: Wire breakage more than 10 times / hour

[0140] The pellet shape was evaluated according to the following criteria.

[0141] A: Fragments ≤300ppm, flatness ≤1.30 and long pellets ≤5 / kg

[0142] B: Fragments>300ppm or flatness>1.30 or long particles>5 / kg

[0143] Example 2

[0144] The same operation as in Example 1 was performed except that the mold working zone length was set to 10 mm. The resin pressure in the mold section was 2.8 MPa at this time. The results are shown in Table 2.

[0145] Example 3

[0146] The same operation as in Example 1 was performed except that the mold working zone length was set to 30 mm. The resin pressure in the mold segment was 7.2 MPa at this time. The results are shown in Table 2.

[0147] Example 4

[0148] The same operation as in Example 1 was performed except that the die base temperature was set to 270° C. The results are shown in Table 2.

[0149] Example 5

[0150] The same operation as in Example 1 was performed except that the die base temperature was set to 330° C. The results are shown in Table 2.

[0151] Example 6

[0152] The same operation as in Example 1 was performed except that the die base temperature was set to 250° C. The results are shown in Table 2.

[0153] Example 7

[0154] The same operation as in Example 1 was performed except that the die base temperature was set to 350° C. The results are shown in Table 2.

[0155] Example 8

[0156] The same operation as in Example 1 was carried out except that the temperature of the second kneading zone was set to 140°C. The results are shown in Table 2.

[0157] Example 9

[0158] The same operation as in Example 1 was carried out except that the temperature of the second kneading zone was set to 240°C. The results are shown in Table 2.

[0159] Example 10

[0160] The same operation as in Example 1 was performed except that the strand cutting temperature was set to 95° C. The results are shown in Table 2. The strand cutting temperature was low, and a large amount of fragments were generated.

[0161] Embodiment 11

[0162] The same operation as in Example 1 was performed except that the strand cutting temperature was set to 155° C. The results are shown in Table 2. The amount of chips was small, but the flattening rate of the elliptical columnar pellets was large.

[0163] Comparative Example 1

[0164] The die working zone length was set to 5 mm, and the operation was carried out in the same manner as in Example 1. The resin pressure in the die section was 1.7 MPa. Strand breakage occurred 16 times in the 1-hour test. This situation did not allow stable production.

[0165] Comparative Example 2

[0166] The die working zone length was set to 40 mm, and the operation was carried out in the same manner as in Example 1. The resin pressure in the die section was 9.4 MPa. During the 1-hour test, 19 strand breaks occurred. This situation did not allow stable production.

[0167] The results are shown in Table 2 below.

[0168] [Table 2]

[0169]

[0170]

[0171] The following Examples 12 to 22 and Comparative Examples 3 and 4 produce resin compositions according to the raw material ratios shown in Formulation 2 of Table 1 above.

[0172] Example 12

[0173] 50.0 kg / h of PBT1, 75 kg / h of PS, and 12.5 kg / h of PC were fed from the main raw material hopper into the feed barrel C1 of the twin screw extruder "TEX44αIII", and 112.5 kg / h of glass fiber was fed from the side feed hopper into the side feed barrel C9. The total feed amount of raw materials was 250 kg / h. The operation was carried out in the same manner as in Example 1, except that the screw speed was set to 370 rpm.

[0174] The results are shown in Table 3 below.

[0175] The obtained pellets were dried at 120°C for 5 hours, and the shear viscosity was measured at 265°C and a shear rate of 91 / sec using a "Capilograph 1D2" (manufactured by Toyo Seiki Seisakusho Co., Ltd.) with a capillary diameter of 1 mm and an orifice of 3 mm in capillary length. The shear viscosity was 720 Pa·s.

[0176] Embodiment 13

[0177] The same operation as in Example 12 was performed except that the mold working zone length was set to 10 mm. The resin pressure in the mold section was 2.6 MPa at this time. The results are shown in Table 3.

[0178] Embodiment 14

[0179] The same operation as in Example 12 was performed except that the mold working zone length was set to 30 mm. The resin pressure in the mold segment at this time was 7.1 MPa. The results are shown in Table 3.

[0180] Embodiment 15

[0181] The same operation as in Example 12 was performed except that the die base temperature was set to 270°C. The results are shown in Table 3.

[0182] Example 16

[0183] The same operation as in Example 12 was performed except that the die base temperature was set to 330°C. The results are shown in Table 3.

[0184] Embodiment 17

[0185] The same operation as in Example 12 was performed except that the die base temperature was set to 250°C. The results are shown in Table 3.

[0186] Embodiment 18

[0187] The same operation as in Example 12 was performed except that the die base temperature was set to 350°C. The results are shown in Table 3.

[0188] Embodiment 19

[0189] The same operation as in Example 12 was carried out except that the temperature of the second kneading zone was set to 140°C. The results are shown in Table 3.

[0190] Embodiment 20

[0191] The same operation as in Example 12 was carried out except that the temperature of the second kneading zone was set to 240°C. The results are shown in Table 3.

[0192] Embodiment 21

[0193] The operation was performed in the same manner as in Example 12 except that the strand cutting temperature was set to 95°C. The results are shown in Table 3. The strand cutting temperature was low, and a large amount of fragments were generated.

[0194] Embodiment 22

[0195] The same operation as in Example 12 was performed except that the strand cutting temperature was set to 155° C. The results are shown in Table 3. The amount of chips was small, but the flattening rate of the elliptical columnar pellets was large.

[0196] Comparative Example 3

[0197] The die working zone length was set to 5 mm, and the operation was carried out in the same manner as in Example 12. The resin pressure in the die section was set to 1.6 MPa. Wire breakage occurred 14 times in the 1 h test. This situation did not allow stable production.

[0198] Comparative Example 4

[0199] The die working zone length was set to 40 mm, and the operation was performed in the same manner as in Example 12. The resin pressure in the die section was set to 9.1 MPa. Wire rods occurred 21 times in the 1 h test. This situation did not allow stable production.

[0200] [Table 3]

[0201]

[0202] [Industrial Applicability]

[0203] The production method of the present invention can stably produce high-quality pellets of a glass fiber-reinforced polyester resin composition containing a high concentration of glass fibers.

[0204] [Reference Symbol List]

[0205] 1 Main raw material hopper

[0206] 2 open exhaust ports

[0207] 3 side feed hopper

[0208] 4 Pressure relief exhaust port

[0209] 5 Thermocouple in the second mixing section

[0210] 6 Flange

[0211] 7. Resin pressure gauge

[0212] 8 mold base

[0213] 9 Die base thermocouple

[0214] 10 wire material

[0215] 11 Granulator

[0216] 12 pellets

[0217] 13 cooling water tank

[0218] 14 Threaded connection part

[0219] 15 Gear Box

[0220] 16 Motor

Claims

1. A method for producing a glass fiber reinforced polyester resin composition using a twin-screw extruder, wherein the resin composition comprises (A) 10% to 60% by mass of a polyester resin, (B) 40% to 70% by mass of glass fibers, and (C) 0% to 50% by mass of other polymers or additives, wherein: The total of each component is 100% by mass. The shear viscosity of the resin composition at 265° C. and 91 / s is 400 Pa·s to 2000 Pa·s. The method comprises: a first step of mixing the polyester resin (A) and the other polymer or additive (C) in a first mixing section; a second step of adding the glass fiber (B) to be mixed in a second mixing section downstream of the first mixing section; a third step of decompressing the exhaust port downstream of the second mixing section to remove volatiles and increase the pressure, and then extruding from a die attached to a die base; and a fourth step of water cooling the strands coming out of the die and cutting the strands with a pelletizer, In the third step, the pressure at the screw tip is increased and extrusion is performed, so that when the resin composition comes out of the mold, the resin pressure in the mold is 2 MPa to 9 MPa.

2. The production method according to claim 1, wherein The mold base temperature in the third step is 260°C to 340°C.

3. The production method according to claim 1, wherein The barrel temperature in the second mixing zone in the second step is 150°C to 220°C.

4. The production method according to claim 1, wherein The strand temperature when the strand is cut by a pelletizer in the fourth step is 100°C to 150°C.