Graft copolymers for reducing interfacial tension in polymer blends

By adjusting the block molecular weight and graft branching number in the graft copolymer of polymers A and B, the graft copolymer formed serves as a compatibilizer, the problem of excessive interfacial tension in the polymer blend is solved. Improved compatibility and material properties.

CN119032116APending Publication Date: 2024-11-26COVESTRO DEUTSCHLAND AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032428.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2023-03-29
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the phase interfacial tension caused by the difference in polarity of polymers A and B leads to phase separation and instability of the polymer blend, affecting light transmission, mechanical properties and processing stability, and existing connections Branch copolymers are not effective enough in reducing interfacial tension.

Method used

Using graft copolymers with specific structures, polymer A is a polycarbonate, polyester or polyamide, and polymer B is a polymer made of vinyl monomers, by adjusting the block molecular weight and the number of graft branches, The formed graft copolymer acts as a compatibilizer to reduce the interfacial tension between the polymers and improve compatibility.

Benefits of technology

The interfacial tension in the blend of polymers A and B is significantly reduced, compatibility is improved, the light transmittance, mechanical properties and processing stability of the material are improved, and the capacity enhancement effect is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070045200000071
    Figure BDA0005070045200000071
  • Figure BDA0005070045200000072
    Figure BDA0005070045200000072
  • Figure BDA0005070045200000091
    Figure BDA0005070045200000091
Patent Text Reader

Abstract

The invention relates to a graft copolymer having the general structure B-(A) ns, consisting of a block of two polymers A and B having different chemical compositions, one polymer being a polycondensation polymer selected from the group consisting of polycarbonates, polyestercarbonates, polyesters and polyamides, the other polymer being a polymer made from at least one vinyl monomer, the present invention relates to a graft copolymer characterized in that (i) the number average molecular weight Mn (B) of the block of polymer B is at least 13 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy, (ii) the number ns of side chains in the graft copolymer is at least 3 and at most 15, as determined by NMR spectroscopy, (iii) the number average molecular weight Mn (A) of the block of polymer A is at least 1.5 kg / mol and at most 15 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy, and (iv) ns multiplied by Mn (A) is at least 13 kg / mol, to the use of the graft copolymer for reducing the phase interfacial tension in mixtures comprising polymers A and B, to compositions comprising the graft copolymer and polymers A and B, and to mouldings comprising the compositions.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a graft copolymer of a specific structure, which is composed of blocks of two polymers A and B with different chemical compositions, wherein one polymer is a polycondensation polymer selected from polycarbonate, polyester carbonate, polyester, and polyamide, and the other polymer is a polymer made of one or more different vinyl monomers. The present invention also relates to the use of the graft copolymer for reducing the interfacial tension in a mixture containing homopolymers A and B or a mixture of polymers with similar polarity, a composition containing the graft copolymer and homopolymers A and B or polymers with similar polarity, a molding compound made of the composition, and a molded product made of the molding compound.

[0002] Mixtures of immiscible polymers with different chemical compositions are suitable for producing multiphase polymer blends, whose properties sometimes combine the specific application technical advantages of the two polymers in a synergistic manner and type. However, if the polarity difference between polymers A and B is too large, that is, the interfacial tension at the phase interface of the two polymers is too large, the polymer blend tends to phase separate. The resulting coarse dispersion and / or unstable phase morphology or insufficient phase adhesion usually leads to adverse effects at this time, such as insufficient light transmittance, phase separation, insufficient processing stability, insufficient mechanical properties (such as material ductility / toughness, elongation at break, stress cracking resistance or weld strength), appearance surface defects on parts formed by the polymer blend by thermoplastic processing technology, especially injection molded under high shear, or the shedding of the decorative layer applied on the injection molded parts. In these cases, in order to achieve the desired technical performance conditions, it is usually necessary to add a compatibilizer to the polymer blend composition, which reduces the interfacial tension between the polymers forming the blend, thereby reducing the above-mentioned technical problems, or ideally completely eliminating them.

[0003] Mixtures of polymers of different chemical composition are also suitable for producing block copolymers consisting of blocks of chemically different polymer species by reacting two polymers with each other in a multiphase melt of the polymer mixture. Since such reactions naturally can only take place at the phase interfaces of the different polymers in the melt, the reaction rate of such melt reactions depends on the size of the phase interfaces, i.e. the phase dispersion, or the domain size of the different polymers in the molten mixture. Therefore, in order to achieve the thermodynamically stable, finely dispersed phase morphology in the melt required for high conversions within a technically feasible or reasonable reaction residence time, it is usually necessary to reduce the interfacial tension between the different polymers in the molten mixture, i.e. to use a compatibilizer as a process aid.

[0004] As compatibilizers in polymer mixtures consisting of two chemically different polymers A and B, past experience has shown that block copolymers consisting of blocks of polymers A and B are suitable, wherein, according to conventional ideas from experience in emulsifying immiscible low-viscosity liquids, bipolar AB block copolymer structures are particularly attractive to those skilled in the art in terms of achieving a high degree of effectiveness for the intended purpose. However, in the case of block copolymers comprising a polycondensation polymer as block A and a vinyl (co)polymer as block B, such block copolymer structures are difficult to synthesize. It is usually easier to synthesize graft copolymers consisting of blocks of polycondensation polymers and vinyl (co)polymers.

[0005] For example, US 4959411 discloses a process for producing copolymers by reacting glycidyl methacrylate grafted olefin polymers with carboxyl functionalized polycarbonates in organic solution or in melt compounding, and the use of such copolymers (which are obviously graft copolymers) for compatibilizing polymer blends of polycarbonate and polyolefin to reduce their delamination tendency. The application is completely silent on the influence of the spatial arrangement of the grafted branches on the grafted backbone or the number of the grafted branches and the length of the grafted branches and the grafted backbone on the effect of the grafted copolymer as a compatibilizer in polymer blends.

[0006] Prior art graft copolymers are not sufficiently effective in reducing the interphase tension in the blend or melt mixture of polymers A and B from which they are formed.

[0007] US2006 / 063891 A1 discloses a method having B-(A) n A graft copolymer of the structure, which consists of free radical polymers as blocks A and B and consists of preferably n=2-8 grafted branches of polymer A grafted onto the main chain of polymer B, wherein the average molecular weight M of polymer A is n (A) is preferably 20,000 to 100,000 g / mol, and the average molecular weight M of polymer B is n (B) is preferably >50000 g / mol, where the relative block lengths are chosen so that n·M n (A) / (n·M n (A)+M n (B)) is preferably 0.6 to 0.8. The application discloses that these graft copolymers are suitable for impact modification of transparent polymers. The application does not mention their effect as compatibilizers in blends of homopolymers A and B.

[0008] CN 108586668 A discloses a high-toughness polypropylene / polylactic acid ion-grafted copolymer and a preparation method thereof. The method provided by the invention is simple and low-cost, and utilizes the interaction between anions and cations to graft polylactic acid onto the main chain. However, the effect of the copolymer as a compatibilizer is not disclosed.

[0009] US2012 / 071606A1 discloses a method for forming polycarbonate graft copolymers. In particular, an allyl-containing polycarbonate polymer or copolymer constitutes the backbone of the graft copolymer, and the side chains are attached to the copolymer via the allyl groups. The graft copolymer exhibits a combination of high transparency, good grafting level, good scratch resistance and / or good anti-fog properties. The disclosure also does not provide any hint of the effect on phase compatibilization.

[0010] US 488401A discloses an optical resin composition, which mainly comprises a graft copolymer, wherein the graft copolymer comprises a styrene resin and an aromatic polycarbonate, each of which has a specific molecular weight and specific molecular weight and weight conditions, wherein the composition has a microdispersed phase not exceeding 0.5 μm. The resin composition is suitable for optical use. No disclosure is made about phase compatibilization.

[0011] JP H09143293A discloses a film having a layer made of a graft copolymer of polyester and an acryl polymer. This layer ensures good lubricity and printability. The role of the graft copolymer as a phase compatibilizer is not disclosed.

[0012] The present invention seeks to provide specific graft copolymers which, as additives or process aids, show better effects in reducing the interfacial tension in polymer blends and / or reactive melt mixtures consisting of polymers A and B of different chemical compositions under similar conditions, i.e., by using the same molar concentration, wherein one polymer is a polycondensation polymer selected from polycarbonate, polyester carbonate, polyester, polyamide and mixtures thereof, and the other polymer is a polymer made of one or more different vinyl monomers. The vinyl monomer is preferably selected from styrene, styrene derivatives, vinyl cyanide, acrylate, acrylate derivatives, olefins, maleimide and maleimide derivatives. The ultimate purpose is that these graft copolymers can therefore contribute to improving at least one of the above-mentioned technical problems caused by the insufficient compatibility of polymers A and B.

[0013] In the context of the present invention, the variable E=(1-γ / γ0) is used as a measure of the reduction of the interfacial tension and is called the phase compatibilizer efficiency. γ0 here is the interfacial tension of an incompatible polymer blend consisting of homopolymers A and B, i.e. the interfacial tension at the phase interface of such polymers in the absence of a graft copolymer, and γ is the value of the interfacial tension reduced by the addition of the graft copolymer. If the graft copolymer does not work at all as a compatibilizer, then γ=γ0 and therefore E=0. In the other extreme case of the best possible phase compatibilization, in the absence of a graft copolymer, the interfacial tension at the phase interface of homopolymers A and B is reduced to a value of γ=0, i.e. complete miscibility is achieved. Therefore, in this case, E=1. The value of the phase compatibilizer efficiency E naturally depends on the concentration of the graft copolymer used. In the context of the present invention, under the conditions adopted in the experiments on which it is based, a minimum value of 30, preferably a minimum value of 35, further preferably a minimum value of 40, and more preferably a minimum value of 45 are considered ideal. It is also desirable that these graft copolymers exhibit their effective effects at the lowest possible molecular weight of the graft copolymer employed, since graft copolymers having too high a molecular weight have a lower diffusion coefficient in the polymer melt and therefore can only reach the interface of the polymer components in the polymer blend with greater difficulty (i.e., more slowly) for kinetic reasons in order to be able to effectively exert their desired effects there.

[0014] This purpose is achieved by having a general structure B-(A) ns The graft copolymer is realized by a graft copolymer consisting of blocks of two polymers A and B having different chemical compositions, wherein one polymer, preferably polymer A, is a polycondensation polymer selected from polycarbonate, polyester carbonate, polyester and polyamide, and the other polymer, preferably polymer B, is a polymer made from at least one vinyl monomer, characterized in that

[0015] (i) The number average molecular weight M of the block of polymer B n (B) is at least 13 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy,

[0016] (ii) The number of side chains in the graft copolymer n s is at least 3 and at most 15, as determined by NMR spectroscopy,

[0017] (iii) The number average molecular weight M of the block of polymer A n (A) is at least 1.5 kg / mol and at most 15 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy, and

[0018] (iv)n s Multiply by M n (A) is at least 13 kg / mol.

[0019] For different single n s The preferred ranges, embodiments and features of the claims mentioned in the present invention are "n s "Usually refers to the number of n molecules in a single polymer. s The arithmetic mean of the values.

[0020] n s The value of is preferably at least 4, more preferably at least 5, most preferably at least 6.

[0021] M n (A) is preferably at least 3.0 kg / mol, more preferably at least 4.5 kg / mol, most preferably at least 5.3 kg / mol.

[0022] M n (B) is preferably at least 20 kg / mol, more preferably at least 23 kg / mol, most preferably at least 30 kg / mol.

[0023] n s ×M n The value of (A) is preferably at least 20 kg / mol, more preferably at least 30 kg / mol, most preferably at least 35 kg / mol.

[0024] n s The value of is preferably at most 12, more preferably at most 10, and even more preferably at most 8.

[0025] M n The value of (B) is preferably at most 200 kg / mol, more preferably at most 100 kg / mol, and even more preferably at most 50 kg / mol.

[0026] M n The value of (A) is preferably at most 12 kg / mol, preferably at most 9 kg / mol, more preferably at most 8 kg / mol.

[0027] n s Multiply by M n The value of (A) is preferably at most 120 kg / mol, more preferably 80 kg / mol, and even more preferably 50 kg / mol.

[0028] M n (A)×n s / [M n (B)+M n (A)×n s ] is preferably 0.25 to 0.75, further preferably 0.40 to 0.70, more preferably 0.40 to 0.60.

[0029] n s 、Mn (A), M n (B) and n s ×M n (A) The upper and lower limits and M n (A)×n s / [M n (B)+M n (A)×n s ] ranges can be combined with each other arbitrarily.

[0030] Particularly preferred are graft copolymers having a combination of the following features:

[0031] (i)M n (B) is at least 23 kg / mol,

[0032] (ii)n s is at least 5,

[0033] (iii)M n (A) is at least 3.0 kg / mol,

[0034] (iv)n s Multiply by M n (A) is at least 13 kg / mol.

[0035] Particularly preferred are graft copolymers having a combination of the following features:

[0036] (i)M n (B) is at least 23 kg / mol,

[0037] (ii)n s is at least 6,

[0038] (iii)M n (A) is at least 4.5 kg / mol,

[0039] (iv)n s Multiply by M n (A) is at least 13 kg / mol.

[0040] Most preferred are graft copolymers having a combination of the following characteristics:

[0041] (i)M n (B) is at least 23 kg / mol,

[0042] (ii)n s is at least 6,

[0043] (iii)M n (A) is at least 4.5 kg / mol,

[0044] (iv)ns Multiply by M n (A) is at least 13 kg / mol,

[0045] (iv)M n (A)×n s / [M n (B)+M n (A)×n s ] is 0.40 to 0.70.

[0046] The graft copolymers of the invention may also differ in their structure, i.e. in the spatial distribution of the grafted branches on the graft copolymer main chain. The grafting of the grafted branches on the graft copolymer main chain may be randomly distributed ("random grafting"). It is also possible that (i) the grafted branches are arranged uniformly and equidistantly on the graft copolymer main chain ("uniform equidistant grafting"). It is also possible that (ii) the grafted branches are arranged completely at one end of the graft copolymer main chain ("single-end grafting"), (iii) the grafted branches are arranged at both ends of the graft copolymer main chain ("double-end grafting"), or (iv) the grafted branches are arranged in the center of the graft copolymer main chain of the graft copolymer ("central grafting"). Figure 1 Structures (i) to (iv) are schematically shown in FIG.

[0047] The graft copolymer of the present invention is preferably a center-graft or a double-end-graft, and more preferably a center-graft.

[0048] Structures (ii), (iii) and (iv) have a graft copolymer backbone, which includes a portion with grafted branches and a portion without grafted branches. Graft copolymers are preferred, wherein the portion of the graft copolymer backbone having grafted branches accounts for a total mass proportion of at most 50% by weight, more preferably at most 40% by weight, and more preferably at most 30% by weight of the graft copolymer backbone.

[0049] In the context of the present invention, polymers made from vinyl monomers are also referred to as vinyl (co)polymers.

[0050] In the context of the present invention, block B is also referred to as graft copolymer backbone, graft copolymer main chain or main chain. Block A is referred to as side chain or graft branch chain.

[0051] The at least one vinyl monomer is preferably selected from styrene, styrene derivatives, vinyl cyanide, acrylates, acrylate derivatives, olefins, maleimide and maleimide derivatives.

[0052] The blocks of polymers A and B preferably have similar polarities, and further preferably have chemical structures similar to the polymers that form the polymer blend or polymer melt mixture that seeks to reduce interfacial tension. That is, the polymer combination of blocks A and B preferably has Flory-Huggins parameters similar to the polymer combination that forms the polymer blend or polymer melt mixture that seeks to reduce interfacial tension.

[0053] It is further preferred that the blocks consist of the same polymers A and B also contained in the polymer blend or polymer melt mixture in which the interfacial tension is sought to be reduced, these polymers A and B. The expression "made of the same polymers A and B" refers to the chemical structure but not necessarily to the molecular weight.

[0054] Condensation polymer

[0055] One of the polymers forming the graft copolymer according to the invention, preferably polymer A, is a polycondensation polymer selected from the group consisting of polycarbonates, polyester carbonates, polyesters and polyamides. It is also possible to use mixtures of different polycondensation polymers of similar polarity and chemical structure, for example mixtures of structurally different, preferably aromatic polycarbonates, preferably aromatic polyester carbonates or preferably aromatic polyesters, preferably mixtures of structurally different, preferably aromatic polycarbonates, or mixtures of structurally different, preferably aromatic polyester carbonates, or mixtures of structurally different, preferably aromatic polyesters, more preferably mixtures of structurally different, preferably aromatic polycarbonates.

[0056] The polycarbonates and / or polyester carbonates according to component A which are suitable according to the invention are known from the literature or can be prepared by methods known from the literature (for the preparation of polycarbonates, see, for example, Schnell, "Chemistry and Physics of Polycarbonates", Interscience Publishers, 1964 and DE-AS 1495626, DE-A 2232877, DE-A 2703376, DE-A 2714544, DE-A 3000610, DE-A 3832396; for the preparation of polyester carbonates, see, for example, DE-A 3007934).

[0057] The polycarbonates are prepared, for example, by reacting at least one aliphatic and / or aromatic diol (diphenol) with a carbonyl halide (preferably phosgene) and / or with a preferably aromatic dicarboxylic acid dihalide (preferably phthalic acid dihalide) by the phase interface process, optionally with the use of chain terminators (for example monophenols) and optionally with trifunctional or more than trifunctional branching agents (for example trisphenols or tetraphenols). Mixtures of aliphatic and aromatic diols can also be used. They can likewise be prepared by reacting aliphatic and / or aromatic diols (diphenols) with, for example, diphenyl carbonate by the melt polymerization process.

[0058] The diphenols used for preparing the aromatic polycarbonates and / or aromatic polyester carbonates are preferably those having the formula (1)

[0059]

[0060] in

[0061] A is a single bond, C1 to C5 alkylene, C2 to C5 alkylidene, C5 to C6 cycloalkylidene, -O-, -SO-, -CO-, -S-, -SO2-, C6 to C6 alkylene which may be fused with other aromatic rings optionally containing heteroatoms, 12 Arylene,

[0062] or a group of formula (2) or (3)

[0063]

[0064] B represents C1 to C 12 alkyl, preferably methyl, halogen, preferably chlorine and / or bromine,

[0065] x is in each case independently of one another 0, 1 or 2,

[0066] p is 1 or 0, and

[0067] R 5 and R 6 For each X 1 are selected individually and independently of one another to be hydrogen or C1 to C6 alkyl, preferably hydrogen, methyl or ethyl,

[0068] X 1 is carbon, and

[0069] m is an integer from 4 to 7, preferably 4 or 5, provided that at least one X 1 R on the atom 5 and R 6 At the same time it is an alkyl group.

[0070] Preferred diphenols are hydroquinone, resorcinol, dihydroxybiphenols, bis(hydroxyphenyl)C1-C5 alkanes, bis(hydroxyphenyl)C5-C6 cycloalkanes, bis(hydroxyphenyl)ethers, bis(hydroxyphenyl)sulfoxides, bis(hydroxyphenyl)ketones, bis(hydroxyphenyl)sulfones and α,α-bis(hydroxyphenyl)diisopropylbenzene and their ring-brominated and / or ring-chlorinated derivatives.

[0071] Particularly preferred diphenols are 4,4'-dihydroxybiphenyl, bisphenol A, 2,4-bis(4-hydroxyphenyl)-2-methylbutane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl sulfone and dibrominated and tetrabrominated or chlorinated derivatives thereof, for example 2,2-bis(3-chloro-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane or 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane. Particularly preferred is 2,2-bis(4-hydroxyphenyl)propane (bisphenol A).

[0072] The diphenols can be used individually or in the form of any desired mixtures. The diphenols are known from the literature or can be obtained by literature processes.

[0073] Suitable aliphatic diols are selected from cyclohexane-1,2-diol, cyclohexane-1,3-diol, cyclohexane-1,4-diol, cyclohexane-1,2-dimethanol, cyclohexane-1,3-dimethanol, cyclohexane-1,4-dimethanol, 2,2-bis(4-hydroxycyclohexyl)propane, tetrahydrofuran-2,5-dimethanol, 2-butyl-2-ethylpropane-1,3-diol, 2-(2-hydroxyethoxy)ethanol, 2,2,4,4-tetramethylcyclobutane-1 ,3-diol, 2,2,4-trimethylpentane-1,3-diol, 2,2-dimethylpropane-1,3-diol, cyclobutane-1,1-diyldimethanol, 8-(hydroxymethyl)-3-tricyclo[5.2.1.02,6]decyl]methanol, propane-1,2-diol, propane-1,3-diol, butane-1,4-diol, pentane-1,5-diol, hexane-1,6-diol, octane-1,8-diol, isosorbide and any mixture thereof.

[0074] Examples of chain terminators suitable for producing thermoplastic aromatic polycarbonates include phenol, p-chlorophenol, p-tert-butylphenol or 2,4,6-tribromophenol, and long-chain alkylphenols, for example 4-[2-(2,4,4-trimethylpentyl)]phenol, 4-(1,3-tetramethylbutyl)phenol according to DE-A 2842005, or mono- or dialkylphenols having a total of 8 to 20 carbon atoms in the alkyl substituent, for example 3,5-di-tert-butylphenol, p-isooctylphenol, p-tert-octylphenol, p-dodecylphenol, 2-(3,5-dimethylheptyl)phenol and 4-(3,5-dimethylheptyl)phenol. The chain terminators are generally used in an amount of 0.5 to 10 mol %, based on the total number of moles of the diphenols used in each case.

[0075] Thermoplastic aromatic polycarbonates can be branched in a known manner by incorporation of trifunctional or more than trifunctional compounds, for example compounds having three or more phenolic groups. However, preference is given to using linear polycarbonates, which are more preferably based on bisphenol A.

[0076] Both homopolycarbonates and copolycarbonates are applicable. In order to prepare the copolycarbonates according to component A of the present invention, 1 to 25% by weight, preferably 2.5 to 25% by weight of polydiorganosiloxanes with hydroxyaryloxy end groups, based on the total amount of diols used, can also be used. These are known (US 3419634) and can be prepared by known literature methods. For example, the preparation of copolycarbonates containing polydiorganosiloxanes is described in DE-A 3334782 and WO 2015 / 052106 A2.

[0077] Also preferred are copolycarbonates made from diphenols of the following structure:

[0078]

[0079] wherein R1 is hydrogen, C1 to C4 alkyl, preferably hydrogen or methyl, particularly preferably hydrogen,

[0080] R2 is independently aryl or alkyl, preferably methyl,

[0081] X is a single bond, -SO2-, -CO-, -O-, -S-, C1 to C6 alkylene, C2 to C5 alkylidene, or C6 to C6 alkylene which may be optionally fused with other aromatic rings containing heteroatoms. 12 Arylene,

[0082] X is preferably a single bond, a C1 to C5 alkylene group, a C2 to C5 alkylidene group, a C5 to C 12 Cycloalkylidene, -O-, -SO-, -CO-, -S-, -SO2-, X is particularly preferably a single bond, isopropylidene, C5 to C 12 cycloalkylidene or oxo, very particularly preferably isopropylidene,

[0083] n is an average number of 10 to 400, preferably 10 to 100, particularly preferably 15 to 50, and

[0084] m is an average number of 1 to 10, preferably 1 to 6, particularly preferably 1.5 to 5.

[0085] Aromatic dicarboxylic acid dihalides for preparing aromatic polyester carbonates are preferably diacid dichlorides of isophthalic acid, terephthalic acid, diphenyl ether 4,4'-dicarboxylic acid and naphthalene-2,6-dicarboxylic acid. Particularly preferred are mixtures of diacid dichlorides of isophthalic acid and terephthalic acid in a ratio of 1:20 to 20:1.

[0086] In the preparation of the polyester carbonates, carbonyl halides, preferably phosgene, are additionally used as difunctional acid derivatives.

[0087] Useful chain terminators for the preparation of aromatic polyester carbonates include, in addition to the monophenols already mentioned, their chlorocarbonates and the acid chlorides of aromatic monocarboxylic acids, which may optionally be replaced by C1 to C 22 Alkyl or halogen atom substituted, and aliphatic C2 to C 22 Monocarboxylic acid chloride.

[0088] The amount of chain terminators is in each case from 0.1 to 10 mol %, based on the moles of diphenol for phenolic chain terminators and on the moles of dicarboxylic acid chloride for monocarboxylic acid chloride chain terminators.

[0089] For the preparation of the aromatic polyester carbonates, it is also possible to use one or more aromatic hydroxycarboxylic acids.

[0090] The aromatic polyester carbonates may be either linear or branched in a known manner (cf. DE-A 2940024 and DE-A 3007934), with preference being given to linear polyester carbonates.

[0091] The branching agents used may be, for example, trifunctional or polyfunctional carboxylic acid chlorides, for example trimesoyl chloride, cyanuric chloride, 3,3',4,4'-benzophenonetetracarboxylic acid chloride, 1,4,5,8-naphthalenetetracarboxylic acid chloride or pyromellitic acid chloride, or trifunctional or polyfunctional phenols, for example phloroglucinol, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)hept-2-ene, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptane, 1,3,5-tri(4-hydroxyphenyl)benzene, 1,1,1-tri(4-hydroxyphenyl)ethane, tri ... or tri(4-hydroxyphenyl)ethane. The branching agent may be 0.01 to 1.0 mol % (based on the diphenol used) of phenolic branching agents and acyl chloride branching agents.

[0092] The proportion of carbonate structural units in the thermoplastic aromatic polyester carbonate can be changed arbitrarily. Preferably, the proportion of carbonate groups is based on the sum of ester groups and carbonate groups, and is at most 99.9 mol%, especially at most 80 mol%, and particularly preferably at most 50 mol%. Both the ester part and the carbonate part of the aromatic polyester carbonate can be present in the polycondensate in the form of blocks or in a randomly distributed form.

[0093] In a preferred embodiment, the polyesters that come into consideration are aromatic, more preferably polyalkylene terephthalates. In a particularly preferred embodiment, they are reaction products of aromatic dicarboxylic acids or their reactive derivatives (e.g. dimethyl esters or anhydrides) with aliphatic, cycloaliphatic or araliphatic diols, and mixtures of these reaction products.

[0094] Particularly preferred aromatic polyalkylene terephthalates contain at least 80% by weight, preferably at least 90% by weight, of terephthalic acid groups, based on the dicarboxylic acid component, and at least 80% by weight, preferably at least 90% by weight, of ethylene glycol groups and / or butane-1,4-diol groups, based on the diol component.

[0095] In addition to terephthalic acid groups, the preferred aromatic polyalkylene terephthalates may contain up to 20 mol %, preferably up to 10 mol %, of groups of other aromatic or cycloaliphatic dicarboxylic acids having 8 to 14 carbon atoms or groups of aliphatic dicarboxylic acids having 4 to 12 carbon atoms, for example groups of phthalic acid, isophthalic acid, naphthalene-2,6-dicarboxylic acid, 4,4′-biphenyldicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid or cyclohexanediacetic acid.

[0096] In addition to ethylene glycol and / or butane-1,4-diol radicals, the preferred aromatic polyalkylene terephthalates may contain up to 20 mol %, preferably up to 10 mol %, radicals of other aliphatic diols having 3 to 12 carbon atoms or radicals of cycloaliphatic diols having 6 to 21 carbon atoms, for example propane-1,3-diol, 2-ethylpropane-1,3-diol, neopentyl glycol, pentane-1,5-diol, hexane-1,6-diol, cyclohexane-1,4-dimethanol, 3-ethylpentane-2,4-diol, radicals of 2-methylpentane-2,4-diol, 2,2,4-trimethylpentane-1,3-diol, 2-ethylhexane-1,3-diol, 2,2-diethylpropane-1,3-diol, hexane-2,5-diol, 1,4-di(β-hydroxyethoxy)benzene, 2,2-bis(4-hydroxycyclohexyl)propane, 2,4-dihydroxy-1,1,3,3-tetramethylcyclobutane, 2,2-bis(4-β-hydroxyethoxyphenyl)propane or 2,2-bis(4-hydroxypropoxyphenyl)propane (DE-A 2407674, 2407776, 2715932).

[0097] Particular preference is given to aromatic polyalkylene terephthalates which have been prepared exclusively from terephthalic acid and its reactive derivatives (for example dialkyl esters thereof) and ethylene glycol and / or butane-1,4-diol, and mixtures of these polyalkylene terephthalates.

[0098] Preferred mixtures of aromatic polyalkylene terephthalates comprise 1 to 50% by weight, preferably 1 to 30% by weight, of polyethylene terephthalate and 50 to 99% by weight, preferably 70 to 99% by weight, of polybutylene terephthalate.

[0099] The aromatic polyalkylene terephthalates can be prepared by known methods (see, for example, Kunststoff-Handbuch, Vol. VIII, p. 695 ff., Carl-Hanser-Verlag, München 1973).

[0100] In one embodiment of the invention, amorphous and / or semicrystalline polyamides are used as polycondensation polymers. Suitable polyamides are aliphatic polyamides, for example PA-6, PA-11, PA-12, PA-4,6, PA-4,8, PA-4,10, PA-4,12, PA-6,6, PA-6,9, PA-6,10, PA-6,12, PA-10,10, PA-12,12, PA-6 / 6,6 copolyamide, PA-6 / 12 copolyamide, PA-6 / 11 copolyamide, PA-6,6 / 11 copolyamide, PA-6,6 / 12 copolyamide, PA-6 / 12 copolyamide, PA-6 / 11 copolyamide, PA- ...0, PA-6 / 10, PA-6 / 12 copolyamide, PA-6 / 10, PA-6 / 10 A-6 / 6,10 copolyamide, PA-6,6 / 6,10 copolyamide, PA-4,6 / 6 copolyamide, PA-6 / 6,6 / 6,10 terpolymer and copolyamides of cyclohexane-1,4-dicarboxylic acid with 2,2,4- and 2,4,4-trimethylhexamethylenediamine, aromatic polyamides such as PA-6,1, PA-6,1 / 6,6 copolyamide, PA-6,T, PA-6,T / 6 copolyamide, PA-6,T / 6,6 copolyamide, PA-6,1 / 6,T copolyamide, PA-6,6 / 6,T / 6,1 copolyamide, PA-6,T / 2-MPMDT copolyamide (2-MPMDT = 2-methylpentamethylenediamine), PA-9,T, copolyamides formed from terephthalic acid, 2,2,4- and 2,4,4-trimethylhexamethylenediamine, copolyamides formed from isophthalic acid, laurolactam and 3,5-dimethyl-4,4-diaminodicyclohexylmethane, copolyamides formed from isophthalic acid, azelaic acid and / or sebacic acid and 4,4-diaminodicyclohexylmethane, Copolyamides formed from aminodicyclohexylmethane, copolyamides formed from caprolactam, isophthalic acid and / or terephthalic acid and 4,4-diaminodicyclohexylmethane, copolyamides formed from caprolactam, isophthalic acid and / or terephthalic acid and isophoronediamine, copolyamides formed from isophthalic acid and / or terephthalic acid and / or other aromatic or aliphatic dicarboxylic acids, optionally alkyl-substituted hexamethylenediamine and alkyl-substituted 4,4-diaminodicyclohexylamine, or copolyamides thereof, and mixtures of the above polyamides.

[0101] Preference is given to using exclusively linear polycarbonates based on bisphenol A as polycondensation polymers.

[0102] Vinyl (co)polymer

[0103] The vinyl (co)polymer of the present invention is a polymer made from one or more vinyl monomers, preferably selected from styrene, styrene derivatives, acrylonitrile, acrylate, acrylate derivatives, olefins, maleimide and maleimide derivatives.

[0104] In the context of the present invention, vinyl (co)polymers are also understood to mean polymers made from one or more vinyl monomers which also contain graft-active units incorporated as comonomers or end groups into the polymer chain and / or grafted onto the polymer chain. The amount of these graft-active units determines the characteristics of the present invention. s .

[0105] Examples of suitable styrene derivatives are α-methylstyrene and vinyl aromatics substituted on the ring, such as p-methylstyrene and p-chlorostyrene.

[0106] Examples of acrylates and acrylate derivatives are C1-C8 alkyl (meth)acrylates, such as methyl methacrylate, n-butyl acrylate and tert-butyl acrylate, and glycidyl methacrylate.

[0107] Examples of the vinyl cyanide include acrylonitrile and methacrylonitrile.

[0108] Depending on which method for preparing the graft copolymer of the present invention described below is used, it may be necessary to use at least partially vinyl monomers with reactive groups for the coupling reaction, such as hydroxyl, carboxyl, amino, groups containing double bonds, such as vinyl, allyl or acryloyl, carbonyl, nitrile, ester or epoxy groups. Preferably, epoxy groups are used, and more preferably glycidyl methacrylate is used as at least one of the vinyl monomers. Here, glycidyl methacrylate can be polymerized into the main chain of the vinyl (co)polymer or grafted as a side group onto the main chain of the vinyl (co)polymer. Preferably, glycidyl methacrylate is polymerized into the main chain of the vinyl (co)polymer.

[0109] Other suitable vinyl (co)polymers are (co)polymers made from the following components

[0110] B.1 50 to 99% by weight, preferably 65 to 85% by weight, more preferably 70 to 80% by weight, based on the (co)polymer B, of at least one monomer selected from vinyl aromatics, ring-substituted vinyl aromatics and C1-C8 alkyl (meth)acrylates, and

[0111] B.2 Based on the (co)polymer B, 1 to 50% by weight, preferably 15 to 35% by weight, more preferably 20 to 30% by weight, of at least one monomer selected from vinyl cyanide and C1-C8 alkyl (meth)acrylate.

[0112] Vinyl (co)polymers are known and can be produced, for example, by free-radical polymerization, in particular by emulsion, suspension, solution or bulk polymerization.

[0113] Polyolefins are also prepared by chain polymerization, for example by free radical or anionic polymerization. Here, olefins are used as monomers. Another name for olefins is olefins. The monomers can be polymerized individually or as a mixture of different monomers. Preferred monomers are ethylene, propylene, 1-butene, isobutylene, 1-pentene, 1-heptene, 1-octene and 4-methyl-1-pentene.

[0114] The polyolefin may contain up to 50% by weight, more preferably up to 30% by weight, of other vinyl comonomers, such as and preferably methyl acrylate, ethyl acrylate, butyl acrylate, glycidyl methacrylate and methyl methacrylate.

[0115] Polyolefins can be amorphous or semi-crystalline. They can be linear or branched. The production of polyolefins has long been known to those skilled in the art.

[0116] The polymerization can be carried out, for example, at a pressure of 1 to 3000 bar and a temperature of 20° C. to 300° C., optionally using a catalyst system. Examples of suitable catalysts include mixtures of titanium and aluminum compounds and metallocenes.

[0117] By changing the polymerization conditions and the catalyst system, the number of branches, crystallinity and density of the polyolefin can be varied within a wide range. These measures are also well known to those skilled in the art.

[0118] Preparation of the graft copolymer of the present invention

[0119] Graft copolymerization is a technique for producing polymers in which the main chain forms the starting point for other chains of different monomer types. Thus, this produces a copolymer B-(A) ns , whose main chain B is connected to multiple chains A formed by other monomer types in a comb-like manner, and n s In the context of the present invention, the main chain A is also referred to as the main chain and the chain B is referred to as a side chain or a grafted branch chain.

[0120] For the present invention, it is not important according to which method the graft copolymer structure of the present invention is produced, that is to say, all graft copolymerization methods known to those skilled in the art are suitable in principle for producing such graft copolymers of the present invention, as long as they achieve the claimed product characteristics.

[0121] The person skilled in the art is familiar with, for example, the following three graft copolymerization processes which are suitable in principle for producing the graft copolymers according to the invention:

[0122] "Graft to" method:

[0123] The polymer is exposed to high-energy electromagnetic radiation (e.g., gamma radiation), which generates free radicals along the main chain, which then form the starting point for further free radical polymerization of the second polymer. Alternatively, instead of high-energy electromagnetic radiation, a free radical former can also be used to generate free radicals along the main chain of the first polymer. At the high temperature of the grafting reaction or alternatively under the influence of higher-energy electromagnetic radiation (e.g., ultraviolet radiation), such free radical formers decompose and form free radicals, which themselves can generate free radicals by extracting, for example, hydrogen atoms from the main chain of the first polymer along its main chain or on the side groups of the polymer, which then form the starting point for further free radical polymerization of the second polymer. Preferred free radical formers are azo compounds, such as azoisobutyronitrile (AIBN) and organic or inorganic peroxides, such as dibenzoyl peroxide (DBPO) or alkali metal peroxydisulfate. Such grafting polymerization methods can in principle be carried out in a solution, emulsion or suspension of the first polymer, in a melt of the first polymer, or in a solid of the first polymer. In the latter case, the monomers of the second polymer for forming the graft branches are impregnated into the solid of the first polymer and then polymerized.

[0124] In another method, the existing polymer and the monomers to be added are dissolved in a nonpolar solvent (e.g. dichloromethane) and a Lewis acid (coinitiator) is added. The Lewis acid now removes electrons from various sites of the polymer. The positively charged sites thus generated now constitute starting points for cationic polymerization with the monomers, which form the graft.

[0125] "Graft from" method:

[0126] In this method, reactive functional groups such as hydroxyl, carboxyl, amino, double bond-containing groups such as vinyl, allyl or acryloyl, carbonyl, nitrile, ester or epoxy groups are incorporated into the main chain of the first polymer along its main chain or on its possible side groups. This can be achieved by copolymerization with monomers containing such functional groups or by subsequent chemical treatment of the main chain polymer. Then, attack points for graft copolymerization can be formed on these reactive functional groups in the main chain polymer, thereby forming grafted branches from monomer units. Depending on the functional group, different polymerization methods, such as polycondensation, polyaddition or free radical, anionic or cationic polymerization are all suitable for forming grafted branches.

[0127] Grafting method via macromonomer:

[0128] In this process, in a first step, polymer blocks carrying reactive groups in the graft backbone and side chains are prepared by those polymerization methods known in principle to the person skilled in the art, such as polycondensation, polyaddition or free radical, anionic or cationic polymerization, and in a second step, the two reactive polymers (macromers) are chemically coupled together to form a graft copolymer.

[0129] The chemical coupling reaction can be carried out either in a solution containing a solvent suitable for the two polymers to be coupled or in a molten mixture of the two polymers. A melt reaction is preferred in terms of environmental protection since it does not require a solvent. Such a melt reaction can be carried out, for example, in a stirred tank reactor, a continuous tubular reactor equipped with a mixing device or preferably in commercially available compounding devices such as twin-screw extruders, planetary roller extruders or internal kneaders, preferably also in a Filmtruder, where the temperature is above the melting temperature of the two polymers to be coupled.

[0130] In this case, examples of reactive groups suitable for coupling reactions are also hydroxyl, carboxyl, amino, groups containing double bonds, such as vinyl, allyl or acryloyl, carbonyl, nitrile, ester or epoxy groups, wherein the functional groups in the two polymer blocks that form the main chain and the grafted branches in the graft copolymer, respectively, must match each other in pairs so that they allow coupling reactions, preferably in the form of condensation or addition reactions, more preferably in the form of addition reactions. Preference is given to, for example, the combination of hydroxyl, amino or carboxyl as the functionalization of one of the polymers and epoxy as the functionalization of the second polymer, more preferably the combination of amino or carboxyl as the functionalization of one of the polymers and epoxy as the functionalization of the second polymer. When the polycondensation polymer is a polycarbonate, polyester or polyester carbonate, the combination of carboxyl as the functionalization of one of the polymers and epoxy as the functionalization of the second polymer is particularly preferred. It is further preferred that the polycarbonate, polyester or polyester carbonate is functionalized with carboxyl groups and the vinyl (co)polymer is functionalized with epoxy groups.

[0131] The functional groups in the polymer forming the grafted branches are preferably introduced from the terminal. The macromonomer used to form such grafted branches is preferably a polymer block containing only a low proportion of multifunctional polymer molecules (i.e., polymer molecules having more than one reactive functional group). The polymer used to form the grafted branches is particularly preferably a polymer containing an average of a maximum of 1.5, further preferably a maximum of 1.3, and most preferably a maximum of 1.1 reactive functional groups per polymer molecule. The polymer used to form the grafted branches is most preferably a polymer containing only terminal functional groups. This can minimize the number of branch structures in the graft copolymer and prevent the formation of such undesirable structures.

[0132] The production of grafted branches for forming particularly preferred carboxyl-terminated polycarbonates or polyester carbonates is carried out, for example, as described in US Pat. No. 4,959,411. In this case, for the formation of carboxyl-functionalized end groups, carboxyl-functionalized phenols or preferably derivatives, in particular esters of carboxyl-functionalized phenols, more preferably tert-butyl esters of carboxyl-functionalized phenols, most preferably tert-butyl 4-hydroxybenzoate are used as chain terminators in the polycondensation reaction to form the polycarbonate or polyester carbonate, which is preferably carried out in the phase interface phosgenation of bisphenols. In the preferred case of using tert-butyl esters of carboxyl-functionalized phenols as chain terminators for forming the end groups, the terminal carboxyl groups are released in a subsequent pyrolysis step, in which isobutylene is eliminated at temperatures above 200° C. and removed from the reaction mixture under reduced pressure to change the chemical equilibrium.

[0133] Although only carboxyl functionalized phenols or preferred derivatives, especially esters of carboxyl functionalized phenols are used as chain terminators in the polymers disclosed in US Pat. No. 4,959,411 and thus double-end functionalized polycarbonates are formed, in order to produce polymer blocks that are particularly suitable for forming graft branches in the present invention, it is recommended to use a mixture of such carboxyl functionalized phenols or preferred derivatives (especially esters of carboxyl functionalized phenols) and non-reactive functionalized phenols (e.g. tert-butylphenol or phenol) as chain terminators. In this way, the average carboxyl functionality of the resulting polycarbonate blocks can be reduced to the desired level described previously. In these chain terminator mixtures, the molar proportion of the non-reactive phenols used is preferably at least 50 mol%, further preferably at least 65 mol%, more preferably at least 70 mol%, more preferably at least 75 mol%.

[0134] The carboxyl or carboxyl derivative functionalized polycarbonates thus prepared can be coupled with epoxy functional groups of glycidyl methacrylate graft polymers or with epoxy functional groups of vinyl (co)polymers containing structural units derived from glycidyl methacrylate by the method described in the same way in US Pat. No. 4,959,411 to prepare the graft copolymers of the present invention. If such glycidyl methacrylate graft polymers or vinyl (co)polymers containing structural units derived from glycidyl methacrylate are used as graft backbones in the preparation of the graft copolymers, the number of grafted branches n in the resulting graft copolymers can be precisely controlled by correspondingly selecting the molar ratio of glycidyl methacrylate and non-reactive vinyl monomers. s The preparation of such glycidyl methacrylate-modified polymers is generally known to those skilled in the art. Corresponding commercial products are available, for example, as Fine-Blend TM SAG and Fine-Blend TM SOG (both from Fine-Blend Polymer Shanghai Co., Ltd.) or Lotader TMIt is available in the market under brand names such as AX (Arkema).

[0135] Particularly preferred double-end grafted and center-grafted graft copolymers can in principle be prepared by chemical coupling of macromolecular monomers according to the same method as described above; wherein in a specific embodiment of the present invention, block copolymers are used as grafting main chains, preferably block copolymers composed of blocks of vinyl (co)polymers.

[0136] When producing a double-end grafted graft copolymer, a block copolymer containing at least three blocks is used as the graft backbone, wherein only the two outer blocks of the block copolymer are equipped with reactive functional groups in accordance with the above-mentioned preferred range, and at the center of the block copolymer serving as the graft backbone, there is a part consisting of at least one block that does not contain a functional group suitable for coupling with the grafted branch block.

[0137] When producing a centrally grafted graft copolymer, a block copolymer comprising at least three blocks is used as the graft backbone, wherein the two outer portions of the block copolymer are each composed of at least one block not comprising a functional group suitable for coupling with the grafted branch block, while a block equipped with reactive functional groups in the preferred range described above is used in the central portion of the block copolymer.

[0138] The block equipped with reactive functional groups used herein is preferably a copolymer of glycidyl methacrylate and at least one other vinyl monomer, more preferably a random copolymer.

[0139] The production of such block copolymers which are suitable as grafting backbones for the production of centrally grafted and / or double-end grafted copolymers is known in principle to the skilled person. In order to produce such well-defined block copolymers from blocks of different chemical compositions, preferably controlled polymerization methods (often also referred to as "living" polymerizations) are used. Suitable in principle are living anionic polymerization, living cationic polymerization, living ring-opening metathesis polymerization, living radical polymerization and living polycondensation. Preferably, living radical polymerization methods are used, more preferably atom transfer radical polymerization ("atom transfer radical polymerization" = ATRP) or reversible addition-fragmentation chain transfer polymerization ("reversible addition-fragmentation chain transfer" = RAFT).

[0140] Controlled ("living") polymerization is understood to mean a polymerization in which no chain termination reactions and chain transfers occur and the rate of the chain initiation reaction is much greater than the rate of the chain extension reaction. This makes it possible to control the molar mass with a narrow distribution and to produce chemically well-defined polymer structures, such as specific block copolymers with a well-defined sequence length and block composition. In this case, the block copolymers are formed in a plurality of steps by using different monomers or monomer mixtures in each step.

[0141] Thus, for example, block copolymers composed of structural units derived, for example, from styrene, which are suitable as graft backbones for producing center-grafted graft copolymers, can be produced by one of the above-described living polymerization processes, for example by ATRP, wherein in a first step first only styrene is polymerized to the desired chain length, then in a second step a mixture of styrene and glycidyl methacrylate is polymerized onto the polymer from step 1, and finally in a third step pure styrene is polymerized again onto the polymer from step 2, wherein the distance between two graft branches in the center-grafted graft copolymer can be defined by the molar ratio of styrene to glycidyl methacrylate in step 2.

[0142] Thus, block copolymers made of structural units derived, for example, from styrene, which are suitable as graft backbones for producing double-end-grafted graft copolymers, can be produced in a similar manner and type, for example by one of the above-described living polymerization processes (for example by ATRP), wherein in a first step a mixture of styrene and glycidyl methacrylate is first polymerized to the desired chain length, then in a second step pure styrene blocks are polymerized onto the polymer from step 1, and finally in a third step a mixture of styrene and glycidyl methacrylate is polymerized again onto the polymer from step 2, wherein the distance between the two graft branches in the two end blocks can be defined by the molar ratio of styrene to glycidyl methacrylate in steps 1 and 3. The ratios of styrene to glycidyl methacrylate in the two end blocks can be chosen to be equal or different, and the block lengths of the three blocks can likewise be configured independently of one another.

[0143] Experimental determination of the structural characteristics of the graft copolymers of the present invention

[0144] The structural characteristics of the graft copolymers of the present invention can be determined analytically by a multi-step process.

[0145] The structural characteristics of the graft copolymers of the present invention, in which the grafted main chain is a vinyl (co)polymer and the side chains are condensation polymers, can be determined, for example, by an analytical method consisting of the following steps:

[0146] 1.) By nuclear magnetic resonance spectroscopy (NMR), especially 1H NMR and / or 13 C NMR determines the chemical composition of the graft copolymer, i.e. the nature of the blocks A and B and the monomer composition. The solvent here is selected accordingly for the graft copolymer. In particular in the case of graft copolymers with blocks A and B of greatly different polarities, for example B=polyolefin and A=aromatic polycarbonate, it is generally necessary to carry out the NMR spectroscopy at elevated temperatures >60° C. in order to completely dissolve the graft copolymer. Polychlorinated solvents such as deuterated dichloroethane, deuterated tetrachloroethane, tetrachloromethane or deuterated dichlorobenzene, trichlorobenzene or tetrachlorobenzene are preferably suitable for this purpose.

[0147] 2.) Determine the weight proportion x of the polymer A block in the graft copolymer based on the NMR spectroscopy data determined in step 1 A .

[0148] 3.) By NMR spectroscopy, in particular 1 H NMR and / or 13 C NMR determines the number of grafted branches based on the intensity of the NMR signal assigned to the carbon atom directly involved in the covalent graft bond or to the carbon atom adjacent to the graft bond or to the proton adjacent to the covalent graft bond. s .

[0149] 4.) Determine the molecular weight distribution of the graft copolymer by gel permeation chromatography (GPC) and thereby determine the number average molecular weight M n , where the GPC data determined for the graft copolymer were evaluated by calibration against two polymers A and B as standards, where M was determined n (A) and M n (B) value, where M n,A and M n,B is the molecular weight calibrated against polymer A and B standards, and thus according to the formula M n =x A ·M n,A +(1–x A )·M n,B Calculate the value M of the graft copolymer n In GPC, in particular in the case of graft copolymers with blocks A and B of greatly different polarities, e.g. B=polyolefin and A=aromatic polycarbonate, it is generally necessary to carry out the studies at high temperatures >60° C. in order to completely dissolve the graft copolymer. Suitable solvents for this purpose are, for example and preferably, the same as for NMR spectroscopy in step 1, wherein GPC does not require the use of deuterated solvents.

[0150] 5.) Alkaline saponification or acid- or base-catalyzed complete hydrolysis of the polycondensation blocks (i.e., complete back cleavage of the polycondensation polymer components into the monomer units used to form them) and separation of the remaining intact vinyl (co)polymer blocks (grafted backbones) by precipitation with subsequent washing and drying. The back cleavage of the polycondensation polymer components into monomer units is preferably carried out by alkaline saponification, for example in an ethanolic solution of potassium hydroxide at elevated temperature, preferably under reflux.

[0151] 6.) Determine the molecular weight distribution of the vinyl (co)polymer blocks (grafted backbone) separated in step 5 by gel permeation chromatography (GPC), and thereby determine the number average molecular weight M n (B), wherein the GPC measurement is calibrated for the respective vinyl (co)polymer in the graft copolymer as a standard. The solvent here is selected for the respective vinyl (co)polymer. For example, for polystyrene, polymethyl methacrylate or styrene-acrylonitrile copolymer (SAN), which in each case contains glycidyl methacrylate as grafting active sites for comonomer or trimer units, dichloromethane or chloroform is preferably used as solvent. In these cases, it is generally feasible and preferred to carry out GPC at room temperature. On the other hand, for polyolefins, especially semi-crystalline polyolefins and polyolefins with higher molecular weights, it is generally necessary to carry out GPC at high temperatures>60°C to completely dissolve the graft copolymer. Preferred polychlorinated solvents suitable for this purpose are, for example, ethylene dichloride, tetrachloroethane, tetrachloromethane or dichlorobenzene, trichlorobenzene or tetrachlorobenzene, especially o-dichlorobenzene.

[0152] 7.) Through the formula n s ·M n (A)=M n -M n (B) M determined in step 4 n value and the M determined in step 6 n (B) Value calculation n s ·M n (A) value, and n determined in step 3 s The value is obtained by dividing the variable n s ·M n (A) Calculation of M n (A) value.

[0153] In order to determine the structural characteristics of the graft copolymers of the present invention, wherein the grafted main chain is a polycondensation polymer and the side chains are vinyl (co)polymers, a similar analytical method can be used, which does not differ from the above method in the above steps 1.) to 4.), but step 4.) is followed by the following steps:

[0154] 5.) Alkaline saponification or acid or base catalyzed complete hydrolysis of the polycondensation blocks (i.e. complete reversion of the polycondensation polymer into its monomer units, similar to the above case) and subsequent separation of the remaining intact vinyl (co)polymer blocks (grafted branches) by precipitation with subsequent washing and drying.

[0155] 6.) Determine the molecular weight distribution of the vinyl (co)polymer blocks (grafted branches) separated in step 5 by gel permeation chromatography (GPC) and thereby determine the number average molecular weight M n (A), wherein the GPC measurement is calibrated against the respective vinyl (co)polymer in the graft copolymer as standard. The solvent is selected as described above.

[0156] 7.) Through formula M n (B)=M n -n s ·M n (A) M determined in step 4 n value, M determined in step 6 n (A) value and n determined in step 3 s Value calculation M n (B) value.

[0157] In the case of graft copolymers composed of aromatic polycarbonate blocks and polyolefin blocks, NMR and GPC measurements of the graft polymer and polyolefin blocks (optionally containing graft-active units) are preferably carried out at a temperature of 80° C. in (deuterated) o-dichlorobenzene.

[0158] In the case of graft copolymers consisting of aromatic polycarbonate blocks and polymer blocks selected from polystyrene, polymethyl methacrylate and styrene-acrylonitrile copolymers, optionally containing graft-active units, the NMR measurements are preferably carried out in deuterated dichloromethane at room temperature.

[0159] GPC measurements of graft copolymers are preferably carried out in dichloromethane at room temperature, while GPC measurements of vinyl (co)polymer blocks are preferably carried out in tetrahydrofuran at room temperature.

[0160] Production of molding compounds

[0161] The molding compound can be produced from the graft copolymer of the invention and other components, such as homopolymers A and B or polymers having a polarity or chemical structure similar to homopolymers A and B, and optionally other components.

[0162] The thermoplastic molding materials of the invention can be produced, for example, by mixing the individual components of the composition in a known manner and melt compounding and melt extruding at temperatures preferably from 180° C. to 320° C., particularly preferably from 200° C. to 300° C., very particularly preferably from 240° C. to 290° C. in conventional apparatuses such as internal kneaders, extruders and twin-screw extruders.

[0163] This process is generally referred to as compounding in the context of this application.

[0164] Therefore, "molding material" is understood to mean the product obtained after melt compounding and melt extrusion of the components of the composition.

[0165] The individual components of the composition can be mixed in a known manner sequentially or simultaneously and can be mixed at temperatures of about 20° C. (room temperature) or higher. This means, for example, that some components can be metered in via the main feed opening of the extruder and the remaining components are supplied later in the compounding process via a side extruder.

[0166] A further subject matter of the invention is the resulting moulding materials.

[0167] The molding compound of the present invention can be used to produce moldings. These can be produced, for example, by injection molding, extrusion and blow molding methods. Another form of processing is to produce moldings from previously produced plates or films by deep drawing. The molding compound of the present invention is particularly suitable for processing by extrusion, blow molding and deep drawing methods.

[0168] It is also possible to meter the components of the composition directly into the conveying extruder of an injection molding machine, produce the molding compound according to the invention in the conveying extruder, and process the molding compound directly to a molding by correspondingly discharging it into an injection molding mold (compound injection molding).

[0169] The present invention therefore further provides a molding obtainable from a composition according to the invention or a molding material according to the invention or comprising such a molding material.

[0170] Further embodiments of the present invention are described as follows:

[0171] 1. With general structure B-(A) ns A graft copolymer consisting of blocks of two polymers A and B having different chemical compositions, one of which is a polycondensation polymer selected from polycarbonate, polyester carbonate, polyester and polyamide, and the other polymer is a polymer made from at least one vinyl monomer,

[0172] Features

[0173] (i) The number average molecular weight M of the block of polymer B n (B) is at least 13 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy,

[0174] (ii) The number of side chains in the graft copolymer n s is at least 3 and at most 15, as determined by NMR spectroscopy,

[0175] (iii) The number average molecular weight M of the block of polymer A n (A) is at least 1.5 kg / mol and at most 15 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy, and

[0176] (iv)n s Multiply by M n (A) is at least 13 kg / mol.

[0177] 2. The graft copolymer according to embodiment 1, wherein polymer A is selected from aromatic polycarbonates, aromatic polyester carbonates and aromatic polyesters.

[0178] 3. The graft copolymer according to embodiment 1 or 2, wherein polymer A is an aromatic polycarbonate.

[0179] 4. The graft copolymer according to any one of the preceding embodiments, wherein polymer B is a polymer made from one or more different vinyl monomers selected from styrene, styrene derivatives, acrylonitrile, acrylate, acrylate derivatives, olefins, maleimide and maleimide derivatives.

[0180] 5. The graft copolymer according to embodiment 4, wherein the vinyl monomer is selected from styrene, acrylonitrile, methyl methacrylate, glycidyl methacrylate and olefins.

[0181] 6. The graft copolymer according to any one of the preceding embodiments, wherein n s is at least 4.

[0182] 7. The graft copolymer according to any one of the preceding embodiments, wherein n s is at least 5.

[0183] 8. The graft copolymer according to any one of the preceding embodiments, wherein M n (A) is at least 3.0 kg / mol.

[0184] 9. The graft copolymer according to any one of the preceding embodiments, wherein M n (B) is at least 20 kg / mol.

[0185] 10. The graft copolymer according to any one of the preceding embodiments, wherein M n (B) is at least 23 kg / mol.

[0186] 11. The graft copolymer according to any one of the preceding embodiments, wherein the following features are present:

[0187] (i)M n (B) is at least 23 kg / mol,

[0188] (ii)n s is at least 5,

[0189] (iii)M n (A) is at least 3.0 kg / mol,

[0190] (iv)n s Multiply by M n (A) is at least 13 kg / mol.

[0191] 12. The graft copolymer according to any one of the preceding embodiments, wherein n s At least 6.

[0192] 13. The graft copolymer according to any one of the preceding embodiments, wherein M n (A) is at least 4.5 kg / mol.

[0193] 14. A graft copolymer according to any one of the preceding claims, wherein the following features are present:

[0194] (i)M n (B) is at least 23 kg / mol,

[0195] (ii)n s is at least 6,

[0196] (iii)M n (A) is at least 4.5 kg / mol,

[0197] (iv)n s Multiply by M n (A) is at least 13 kg / mol.

[0198] 15. The graft copolymer according to any one of the preceding embodiments, wherein M n (A)·n s / [M n (B)+M n (A)·n s ] is 0.25 to 0.75.

[0199] 16. The graft copolymer according to any one of the preceding embodiments, wherein M n (A)·n s / [M n (B)+M n (A)·ns ] is 0.40 to 0.70.

[0200] 17. The graft copolymer according to any one of the preceding embodiments, wherein the following features are present:

[0201] (i)M n (B) is at least 23 kg / mol,

[0202] (ii)n s is at least 6,

[0203] (iii)M n (A) is at least 4.5 kg / mol,

[0204] (iv)n s Multiply by M n (A) is at least 13 kg / mol.

[0205] (v)M n (A)·n s / [M n (B)+M n (A)·n s ] is 0.40 to 0.70.

[0206] 18. The graft copolymer according to any one of the preceding embodiments, wherein M n (A) is at least 5.3 kg / mol.

[0207] 19. The graft copolymer according to any one of the preceding embodiments, wherein M n (B) is at least 30 kg / mol.

[0208] 20. The graft copolymer according to any one of the preceding embodiments, wherein M n (A)·n s / [M n (B)+M n (A)·n s ] is 0.40 to 0.60.

[0209] 21. The graft copolymer according to any one of the preceding embodiments, wherein n s Multiply by M n (A) is at least 20 kg / mol.

[0210] 22. The graft copolymer according to any one of the preceding embodiments, wherein n s Multiply by M n (A) is at least 30 kg / mol.

[0211] 23. The graft copolymer according to any one of the preceding embodiments, wherein ns Multiply by M n (A) is at least 35 kg / mol.

[0212] 24. The graft copolymer according to any one of the preceding embodiments, wherein n s The maximum is 12.

[0213] 25. The graft copolymer according to any one of the preceding embodiments, wherein n s The maximum value is 10.

[0214] 26. The graft copolymer according to any one of the preceding embodiments, wherein n s The maximum is 8.

[0215] 27. The graft copolymer according to any one of the preceding embodiments, wherein M n (A) is a maximum of 12 kg / mol.

[0216] 28. The graft copolymer according to any one of the preceding embodiments, wherein M n (A) is a maximum of 9 kg / mol.

[0217] 29. The graft copolymer according to any one of the preceding embodiments, wherein M n (A) is a maximum of 8 kg / mol.

[0218] 30. The graft copolymer according to any one of the preceding embodiments, wherein M n (B) is a maximum of 200 kg / mol.

[0219] 31. The graft copolymer according to any one of the preceding embodiments, wherein M n (B) is a maximum of 100 kg / mol.

[0220] 32. The graft copolymer according to any one of the preceding embodiments, wherein M n (B) is a maximum of 50 kg / mol.

[0221] 33. The graft copolymer according to any one of the preceding embodiments, wherein n s Multiply by M n (A) is a maximum of 120 kg / mol.

[0222] 34. The graft copolymer according to any one of the preceding embodiments, wherein n s Multiply by M n (A) is a maximum of 80 kg / mol.

[0223] 35. The graft copolymer according to any one of the preceding embodiments, wherein n s Multiply by Mn (A) is a maximum of 50 kg / mol.

[0224] 36. The graft copolymer according to any one of the preceding embodiments, wherein the structure of the graft copolymer is selected from dual-end grafting and central grafting.

[0225] 37. The graft copolymer according to any one of the preceding embodiments, wherein the structure of the graft copolymer is center-grafted.

[0226] 38. Use of the graft copolymer according to any one of the preceding embodiments for reducing the interphase tension in a mixture comprising polymers A and B or a mixture of polymers with similar polarity.

[0227] 39. A polymer composition comprising polymers A and B and a graft copolymer according to any one of the preceding embodiments 1 to 37 as component C, wherein polymers A and B have the same chemical structure as the blocks of polymers A and B in the graft copolymer according to component C.

[0228] 40. A polymer composition according to embodiment 39, wherein the ratio of the mass proportion of polymer A in the polymer composition based on the sum of polymers A and B in the composition to the mass proportion of grafted branches in the graft copolymer according to component C is 0.6 to 1.4.

[0229] 41. The polymer composition of embodiment 40, wherein the ratio is from 0.7 to 1.3.

[0230] 42. The polymer composition of embodiment 40, wherein the ratio is from 0.8 to 1.2.

[0231] 43. The polymer composition according to any one of embodiments 39 to 42, wherein the graft copolymer is used in a concentration of 0.1 to 20% by weight.

[0232] 44. The polymer composition according to any one of embodiments 39 to 42, wherein the graft copolymer is used in a concentration of 1.0 to 10 wt%.

[0233] 45. The polymer composition according to any one of embodiments 39 to 42, wherein the graft copolymer is used in a concentration of 2 to 5 weight percent.

[0234] 46. ​​Moulding material obtained from the composition according to any one of embodiments 39 to 45.

[0235] 47. A molded article comprising the composition according to any one of embodiments 39 to 45.

[0236] 48. A molded article made of the molding compound according to embodiment 46. Example

[0237] Simulation of interfacial tension

[0238] The effect of the structure of graft copolymers formed by blocks of two different polymers A and B on the interfacial tension at the phase interface in polymer blends composed of homopolymers A and B was studied by computer-aided simulations. Dissipative particle dynamics simulations were used. The simulations were performed using the open source program LAMMPS (“LAMMPS - a flexible simulation tool for particle-based material modeling at the atomic, mesoscopic and continuum scales”, AP Thompson, HM Aktulga, R. Berger, DSBolintineanu, WM Brown, P S Crozier, P Jin't Veld, A. Kohlmeyer, SG Moore, T D N Guyen, R. Shan, MJ Stevens, J. Tranchida, C. Trott, SJ Primpton, Comp Phys Comm, 271 (2022) 10817).

[0239] The operations in the simulation are performed as follows. To simplify the language, some explanations are written in the present tense, but refer to the actual operations performed.

[0240] In a dissipative particle dynamics (“dissipative particle dynamics” = DPD) simulation, relatively large molecules (in this case polymers) are modeled by beads (“beads”), which interact via pairwise interaction potentials. A bead in a DPD simulation represents a cluster consisting of multiple polymer monomer units. The beads behave according to Newton’s formulas of motion under the influence of their interaction forces. The total force acting on each bead is represented by the sum of conservative forces, dissipative forces, and random forces. The simulation uses the following characteristic variables: r c Unit of length ("cutoff distance"), m Unit of mass, k B T energy unit (k b is the Boltzmann constant, T is the temperature) and Unit of time.

[0241] In the following, the beads forming the homopolymers A and B are referred to as a and b, respectively. The same is true for the beads forming the corresponding blocks of the graft copolymer. This is explained by the three characteristic variables (l b , l s and n s ) simplifies the characterization of grafted copolymers. bis the number of beads that form the main chain ("backbone") of the graft copolymer and is therefore a measure of its molecular weight. s is the number of beads forming grafted branches and is therefore a measure of its molecular weight. s is the number of side chains (grafted branches) grafted onto the main chain of the graft copolymer, wherein in the simulation, these side chains are always grafted in an equidistant distribution over the entire graft copolymer main chain except for the three specific molecular structures (ii) to (iv) defined below. The terms "grafted branches" and "side chains" are used synonymously herein.

[0242] Therefore, a particular embodiment of such graft copolymers studied in the simulation is a graft copolymer with uniform equidistant grafting. In such graft copolymers, the grafted branches are uniformly and equidistantly distributed throughout the graft copolymer backbone. Therefore, this results in a distance I between the side chains. sp (in units of the number of beads), the distance is given by the formula I sp =1+[(l b –n s ) / (n s +1)] calculation.

[0243] In the examples of the present application, specific nomenclature has been defined for such uniformly equidistantly grafted graft copolymers: for example, nomenclature b 31 (a4)3 represents a graft copolymer formed by a graft copolymer backbone consisting of 31 b-type beads, wherein 3 blocks (each formed by 4 a-type beads) are grafted onto the copolymer backbone in an equidistant distribution. Figure 2 Using graft copolymer b 31 (a4) 3 is used as an example to schematically illustrate the structure of such a graft copolymer with uniform equidistant grafting on which the simulation is based. Figure 2 The graft copolymer molecule b shown in the example 31 (a4)3 consists of a total of 31 b-type beads and 3·4=12 a-type beads.

[0244] In the DPD simulations performed in the present invention, the size of the beads was chosen so that the masses of the beads of type a and type b were as similar as possible within the range allowed by the molecular masses of the monomer units, i.e. the molecular masses of the beads of type a and type b were substantially identical. This therefore resulted in a mass ratio of polymer blocks A and B in the graft copolymer which substantially corresponded to the ratio of beads of type a and type b in the graft copolymer. The ratio of beads of type b in a graft copolymer molecule consisting of a graft copolymer backbone of polymer A and grafted side chains of polymer blocks B is calculated according to the formula x=n s ·l s / (l b +n s ·l s )calculate.

[0245] In the present invention, according to Figure 2 The DPD simulations were performed on different graft copolymers with uniform and equidistant grafting, where n s , l s and l b The value of varies systematically.

[0246] In addition, the graft copolymer structures were simulated and compared with each other, in which the molecular weight of the copolymer main chain, the number of grafted branches, and the molecular weight of the grafted branches were kept constant, which were l b =47, l s =8 and n s = 11, but the arrangement (i.e. grafting) of the grafted branches on the main chain of the copolymer is different. Figure 1 In addition to the graft copolymer (i) of the structure shown in FIG. 1 (wherein the grafted branches are arranged uniformly and equidistantly on the main chain of the copolymer (“uniform equidistant grafting”)), the copolymers having a side chain spacing of I sp =1, (ii) wherein all 11 grafted branches are completely arranged at one end of the graft copolymer main chain ("single-end grafting"), (iii) wherein 5 and 6 of the total 11 grafted branches are arranged at both ends of the graft copolymer main chain, respectively ("double-end grafting"), and (iv) wherein all 11 grafted branches are arranged at the center of the graft copolymer main chain of the graft copolymer ("center grafting"). Figure 1 The molecular structures of these three specific graft copolymers (ii) to (iv) are schematically depicted in Figure 1 and compared with the structure of the homogeneous equidistant graft copolymer (i). According to the above nomenclature definition, the four graft copolymers (i) to (iv) can be described as follows, wherein the square brackets in each case enclose a continuous part of a homopolymer block or a graft copolymer block:

[0247] (i)b 47 (a8) 11

[0248] (ii)[b 11 (a8) 11 ]–[b 36 ]

[0249] (iii)[b5(a8)5]–[b 36 ]–[b6(a8)6]

[0250] (iv)[b 18 ]–[b 11 (a8) 11 ]–[b 18 ]

[0251] The simulation of the phase compatibilization efficiency of the graft copolymer formed by the blocks of polymers A and B in the two-phase blend of homopolymers A and B includes the following steps:

[0252] 1. Form the starting configuration of molecules in the simulation box

[0253] Method step 1 includes the following two sub-steps:

[0254] 1.1 First, the Cartesian coordinates of the A-type and B-type homopolymer molecules and the graft copolymer molecules formed by the polymer A and B blocks are specified by the coordinates of the beads forming these polymers. The initial bond length between the two beads is set to the value 0.2·r c During the simulation, the bond lengths change due to the interaction forces, i.e. the final bond lengths in the equilibrium state of the simulation usually do not correspond to the values ​​at the start of the simulation.

[0255] 1.2 A total of 162,000 DPD beads are placed in a periodic box (the size of the box is ) in a substantially uniform random manner, wherein molecular overlap is avoided. This results in a bead density of According to general expert experience, this accurately reflects the thermodynamics of the fluid. The starting configuration depicted here has a 0.5r c The distance tolerance of . In this method step 1.2, the number of homopolymer molecules A and B is selected so that the mass concentration of the two homopolymers is equal, i.e. the simulation is carried out in a blend of homopolymers A and B in which the mass proportion of the homopolymers is 50 wt. % in each case. The polymer molecules of type A and type B from method step 1.1 are duplicated and placed in different halves of the simulation box. For the two homopolymers A and B, molecules consisting of 60 beads in each case are used in the simulation. Then n c = 200 graft copolymer molecules with the respective structure were placed near the interface between homopolymers A and B. With this starting configuration, the formation of the thermodynamic equilibrium state in the interface during the DPD simulation was accelerated. In each simulation, all 200 graft copolymer molecules were placed in each case with n selected. s , l s and l b The values ​​of and the spatial distribution of the grafted branches on the grafted main chain have the same structure.

[0256] 2. Simulation of polymer molecular dynamics up to thermodynamic equilibrium

[0257] The position and pulse of the DPD bead are calculated in discrete time interval steps in the continuous phase space. The motion is simulated here by an algorithm that digitally solves the classical Newtonian motion formula (4)

[0258]

[0259] In formula (4), f i is the sum of the other beads acting on mass m i The force on bead i, P i is the impulse of the bead. The Verlet algorithm is used to perform step-by-step numerical integration of formula (1).

[0260] The force f exerted on bead i by all other beads is i Here, it is described by formula (5), which simulates the pairwise interaction force F between bead i and its respective other beads j in the box: ij The sum of these pairwise interaction forces includes the conservative force component Dissipative force component and random force components

[0261] Dissipative force component and random force components Together they act as a thermostat, where η and σ represent the friction parameter and the noise amplitude, where η = σ 2 / 2k B T;r ij =r i -r j 、v ij =v i -v j As the relative velocity of beads i and j, e ij =r ij / r ij ω D (r ij ) and ω R (r ij ) are the position-dependent weighting functions of the dissipative force component and the random force component, respectively. ξ ij is a Gaussian distributed random number with a mean of zero for each interaction between beads i and j in each time interval Δt. In the simulations performed in this application, ω is chosen D (r ij )=[ω R (r ij )] 2 and σ = 3. Conservative force component is exclusive, through the exclusion parameter α ij definition.

[0262] The repulsion parameter α between polymers A and B AB According to formula (6) and Flory-Huggins parameter χ AB association.

[0263] α AB =α AA +3.27χ AB (6)

[0264] α AA and α BB is the repulsion parameter for chemically identical molecules (i.e., A with A or B with B), where The value of α represents the compressibility of the fluid as best as possible based on experience. AB The higher the value, the higher the incompatibility of polymer species A and B, ie the greater the repulsion.

[0265] In the simulation on which this application is based, the oscillator spring force The binding interaction between two directly adjacent beads of the same polymer molecule is modeled, where is the spring constant of the oscillator.

[0266] The simulation is continued until the mean square radius of gyration of the simulated system remains constant over time, where this constancy is chosen as the criterion for reaching equilibrium. After reaching equilibrium, 2×10 6 A further simulation step (Δt = 0.06t dpd ). The equilibrium configuration generated in this way is used to determine the interfacial tension γ in step 4 (described below).

[0267] 3. Assignment to real polymer systems ("mapping")

[0268] "Mapping" refers to the step of the simulation method in which beads of type A and type B and the repulsion parameter α are mapped to AB Assigned to a real polymer species or oligomeric units of a real polymer species.

[0269] In the simulation, each bead constituting the polymer used for the simulation represents an oligomeric unit of the respective polymer, i.e. a structural unit formed from a number n of monomer units. When a concrete real polymer is assigned to the abstract polymer system, a specific value of n can be given for the individual polymers, wherein this value varies for chemically different polymers with repeating units of different molar masses. The determination of n is carried out under the framework condition that the beads of type a and type b constituting the homopolymers and graft copolymers used for the simulation have approximately the same volume and therefore approximately the same mass.

[0270] In the second step of the “mapping”, the Flory-Huggins parameter χ AB Determine the rejection parameter value α of the specific AB polymer system according to formula (6): ABAfter assigning specific oligomeric units of the respective polymers A and B formed from n monomer units to each a-type and b-type bead in a first step of “mapping”, χ AB The value of is determined using the COSMO-RS model. For this purpose, the activity coefficient γ of A in the mixture is calculated by the COSMO-RS model and quantum chemically with the aid of the Biova COSMOtherm 2019 (Dassault Systèmes) software for an equimolar mixture of oligomer units formed by n monomer units of polymers A and B. A Then the activity coefficient γ A Calculate the Flory-Huggins parameter according to formula (7)

[0271]

[0272] In formula (7), x A represents the molar proportion of A in the mixture (in our case therefore x A =0.5), V A and V B are the volumes of species A and B, respectively, and V tot =V A +V B .

[0273] COSMO-RS ("Conductor-like Screening Model for Real Solvents") is a quantum chemical-based equilibrium thermodynamic simulation method well known to those skilled in the art for predicting chemical potentials in fluids. The details of the COSMO-RS model and its application to the problems in this application are known to those skilled in the art, for example from the review article "The COSMO and COSMO-RS solvationmodels" by A. Klamt, WIREs ComputMol Sci 2018, 8:e1338.doi:10.1002 / wcms.1338 and the work cited therein.

[0274] From this, two different polymer systems were assigned (mapped) and then DPD simulations were performed:

[0275] System 1: Polymer B (grafted backbone) = polystyrene, polymer A (grafted branches) = polycarbonate based on bisphenol A

[0276] System 2: Polymer B (grafted backbone) = polypropylene, polymer A (grafted branches) = polycarbonate based on bisphenol A

[0277] For both systems, the “mapping” procedure gives α for a temperature of 100 °C according to Table 1 AB Value and type a (Ma ) and type b (M b ) The molar mass of the beads, which served as the basis for the simulation.

[0278] Table 1

[0279] Grafted main chain Grafted branched chain <![CDATA[α AB ]]> <![CDATA[M b [gmol -1 ]]]> <![CDATA[M a [gmol -1 ]]]> Polystyrene Polycarbonate 28 668 792 Polypropylene Polycarbonate 35 717 792

[0280] Using the molar masses of beads of type A and type B according to Table 1, the number of beads in the grafted backbone l can be calculated by multiplication b and the number of beads in the grafted branch l s Converted to the molar mass of the grafted main chain M n (B) and the molar mass M of the grafted branch n (A).

[0281] 4. Determination of interfacial tension and efficiency of graft copolymers as phase compatibilizers from equilibrium configurations simulated by DPD

[0282] The interfacial tension γ is determined from the equilibrium configuration obtained in step 3 according to formula (8):

[0283]

[0284] P xx , P yy and P zz is the diagonal component of the pressure tensor, which is calculated according to formula (9)

[0285]

[0286] Where N is the total number of beads and V = L x ×L y ×L z is the volume of the simulation box.

[0287] In an analogous manner the interfacial tension γ0 determined for similar blends of homopolymers A and B in the absence of graft copolymer molecules, ie for incompatible blends, serves as a reference in determining the phase compatibilizer efficiency E=(1-γ / γ0) of the respective graft copolymer.

[0288] Tables 2 and 3 show the phase compatibilizer efficiency E obtained with different graft copolymer structures. Here the number of side chains (n s ), the molecular weight of the main chain M n (B) and the molecular weight M of a single side chain n (A). From this, the molecular weight of the graft copolymer can also be calculated (by M n (B)+n s Multiply by M n (A))、M n (A) Multiply by n sand the molar mass proportion of the side chains in the graft copolymer (expressed in wt%) (mass proportion of grafted branches). Graft copolymers with a main chain consisting of polystyrene (PS, Table 2) or polypropylene (PP, Table 3) were simulated. In both cases, the side chains were formed by polycarbonate based on bisphenol A.

[0289] Table 4 shows the molecular weights M of the main chain and side chains for each graft copolymer system. n The effects of the graft structures according to the designations (i) to (iv) used above were investigated in the case of 1.1% to 1.1% of the total number of graft copolymers. All graft copolymers according to the structures (i) to (iv) have 11 side chains. The investigations were carried out with both polystyrene and polypropylene as graft copolymer backbones and in each case with polycarbonate based on bisphenol A as side chains.

[0290] Table 2: Graft copolymers with uniform and equidistant grafting based on polystyrene (PS) as the main chain and simulated E values

[0291]

[0292]

[0293] Table 2 continued

[0294]

[0295]

[0296] Table 2 continued

[0297]

[0298]

[0299] Table 2 continued

[0300]

[0301] Table 2 continued

[0302]

[0303] Table 3: Graft copolymers with uniform and equidistant grafting based on polypropylene (PP) as the main chain and simulated E values

[0304]

[0305] Table 3 continued

[0306]

[0307]

[0308] Table 3 continued

[0309]

[0310] Table 4: Effect of grafting structure on E

[0311]

[0312]

[0313] The data in Tables 2 and 3 show that only the graft copolymer embodiments of the present invention exhibit increased phase compatibilizer efficiency, ie, a value of E=(1-γ / γ0) of at least 30.

[0314] In addition, the data evaluation in Tables 2 and 3 shows that when M n (A) Beyond a certain value, further increase in the value of this variable no longer leads to a significant further improvement in the phase compatibilizer efficiency, i.e. higher values ​​of E = (1-γ / γ0). This can be seen, for example, from the relationship between E and M for all values ​​in Table 2. n (A) It can be seen that the constant M n (B) is, for example, 20.7 kg / mol, constant n s For example, M is 4. However, as mentioned above, the goal is to achieve effective effects of the graft copolymer at a molecular weight as low as possible. n (A) should not be allowed to be greater than 15 kg / mol in order to achieve the necessary balance between good compatibilizer efficiency E and good runnability in the polymer melt, so that the phase interface is reached quickly.

[0315] Similarly, the evaluation of the data in Tables 2 and 3 shows that when n s Beyond a certain value, a further increase in the value of this variable no longer leads to a significant further improvement in the phase compatibilizer efficiency, i.e. higher values ​​of E=(1-γ / γ0). This can be seen, for example, from the relationship between E and n for all values ​​in Table 2. s The relationship diagram shows that the constant M n (B) is, for example, 20.7 kg / mol, constant M n (A) is, for example, 5.5 kg / mol. The same applies to all values ​​of E and n in Table 3. s The relationship diagram, where the constant M n (B) is, for example, 22.2 kg / mol, with a constant M n (A) is, for example, 5.5 kg / mol. n (A) Similar reasons as described above, ns The upper limit of E is 15 in order to obtain a graft copolymer having a good phase compatibilizer efficiency E and good runnability in the polymer melt.

[0316] The data evaluation in Tables 2 and 3 also shows that when the product M n (A)xn s When the value of exceeds about 50 kg / mol, further increase of the value of this variable no longer brings about significant further improvement of the phase compatibilizer efficiency, i.e. higher values ​​of E=(1-γ / γ0). This can be seen from the E and M of all values ​​in Table 2. n (A)xn s The relationship diagram shows that the constant M n (B) is, for example, 20.7 kg / mol, or as can be seen from all the values ​​in Table 3, where the constant M n (B) is, for example, 22.2 kg / mol, or even other constant M within the scope of the present invention. n (B) This is also clearly seen in the corresponding relationship diagram of the values.

[0317] Finally, the evaluation of the data in Tables 2 and 3 shows that when M n Above a value of about 50 kg / mol, a further increase in the value of this variable no longer leads to a significant further improvement in the phase compatibilizer efficiency, i.e., higher values ​​of E=(1-γ / γ0). This can be seen, for example, from the relationship between E and M for all values ​​in Table 2. n (B) shows that the constant M n (A) is, for example, 6.3 kg / mol, constant n s For example, 11.

[0318] When M n (B), M n (A), n s and M n (A)xn s Above the stated values, the phase compatibilizer efficiency of the graft copolymer in the equilibrium state is only slightly improved, if at all, and, on the contrary, a further increase of these variables characterizing the graft copolymer would hinder the goal pursued; by minimizing the molecular weight of the graft copolymer, its mobility in the polymer melt mixture is maximized, thereby accelerating the achievement of equilibrium.

[0319] The data in Table 4 show that the graft copolymers with double-end grafting and especially central grafting structures exhibit improved phase compatibilizer efficiency, i.e., higher values ​​of E=(1-γ / γ0), compared with graft copolymers with uniform equidistant grafting and especially single-end grafting structures that are similar in chemical composition, number of grafted branches, and molar mass of grafted backbone and grafted branches.

[0320] The number of simulation steps required to reach the equilibrium state was evaluated for some of the simulation experiments selected in Table 2. The results of this analysis are shown in Table 5.

[0321] Table 5 : The number of experimental and simulation steps selected

[0322]

[0323] The data in Table 5 confirm that when M n (A), M n (B) and n s When the value of is high, the molar mass M of the graft copolymer n Higher and M n (A)xn s At higher values ​​of , more simulation steps are required to reach the steady-state equilibrium state. Transferred to real polymer mixtures, this means that longer times are required until a stable distribution of the graft copolymer in the mixture is achieved and thus a stable morphology of the components (i.e. polymers A and B and graft copolymer) is achieved. For this purpose, it is therefore necessary to set an increased residence time in the mixing device (e.g. extruder), which in many cases can only be achieved due to equipment difficulties or is accompanied by other disadvantages (e.g. thermal damage to the polymer components). The number of grafted branches n has a major influence on the number of simulation steps required to reach the steady-state equilibrium state. s (Experiments 4 and 6); secondly, M n The value of (A), i.e. the molecular weight of the grafted side chains (experiments 4 and 9), and thus the results, in particular, the product M n (A)×n s values ​​(all data in Table 5).

[0324] Therefore, it can be inferred from the data in Table 5 that in order to minimize the number of simulation steps required to reach equilibrium or, moving to the industrial level, to minimize the residence time required to reach this desired equilibrium state, it is recommended not to set n s and M n The value of (A) and in particular the product M n (A)×n s The values ​​of are chosen to be higher than those absolutely necessary to achieve the desired phase compatibilizer efficiency E. This consideration leads to upper limits for these three characteristic values, above which the improvement in the phase compatibilizer efficiency E shows only a small or no longer significant improvement, but the residence time required to reach the equilibrium state that must be established to achieve this phase compatibilizer efficiency E increases dramatically.

[0325] For preferred graft copolymers with specific graft structures ("dual-end grafting" and "central grafting"), corresponding studies were also conducted on the number of simulation steps required to reach equilibrium. It was found that, compared with the graft copolymers with the same ns 、M n (A) and M n Compared to the “uniformly equidistantly grafted” graft copolymers with (B) values, this architecture has no effect, i.e., within the determined accuracy of this variable, the number of simulation steps required to reach equilibrium is the same for all three different graft copolymer architectures.

Claims

1. With general structure B-(A) ns A graft copolymer consisting of blocks of two polymers A and B having different chemical compositions, one of which is a polycondensation polymer selected from polycarbonate, polyester carbonate, polyester and polyamide, and the other polymer is a polymer made from at least one vinyl monomer, Features (i) The number average molecular weight M of the block of polymer B n (B) is at least 13 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy, (ii) The number of side chains in the graft copolymer n s is at least 3 and at most 15, as determined by NMR spectroscopy, (iii) The number average molecular weight M of the block of polymer A n (A) is at least 1.5 kg / mol and at most 15 kg / mol, as determined by a combination of gel permeation chromatography and NMR spectroscopy, and (iv)n s Multiply by M n (A) is at least 13 kg / mol.

2. The graft copolymer according to claim 1, wherein polymer A is selected from the group consisting of aromatic polycarbonates, aromatic polyester carbonates and aromatic polyesters.

3. The graft copolymer according to claim 1 or 2, wherein polymer A is an aromatic polycarbonate.

4. The graft copolymer according to any one of the preceding claims, wherein polymer B is a polymer made from one or more different vinyl monomers selected from styrene, styrene derivatives, acrylonitrile, acrylates, acrylate derivatives, olefins, maleimide and maleimide derivatives.

5. The graft copolymer according to claim 4, wherein the vinyl monomer is selected from styrene, acrylonitrile, methyl methacrylate, glycidyl methacrylate and olefins.

6. The graft copolymer according to any one of the preceding claims, characterized in that The following characteristics exist: (i)M n (B) is at least 23 kg / mol, (ii)n s is at least 6, (iii)M n (A) is at least 4.5 kg / mol, (iv)n s Multiply by M n (A) is at least 13 kg / mol, and (v)M n (A)·n s / [M n (B)+M n (A)·n s ] is 0.40 to 0.

70.

7. A graft copolymer according to any one of the preceding claims, wherein n s The maximum is 12.

8. The graft copolymer according to any one of the preceding claims, wherein M n (B) is a maximum of 200 kg / mol.

9. The graft copolymer according to any one of the preceding claims, wherein M n (A) is a maximum of 12 kg / mol.

10. The graft copolymer according to any one of the preceding claims, wherein n s Multiply by M n (A) is a maximum of 80 kg / mol.

11. The graft copolymer according to any one of the preceding claims, wherein the structure of the graft copolymer is selected from dual-end grafted and center grafted.

12. Use of a graft copolymer according to any one of the preceding claims for reducing the interphase tension in a mixture comprising polymers A and B.

13. A polymer composition comprising polymers A and B and as component C the graft copolymer according to any one of claims 1 to 11, wherein polymers A and B have the same chemical structure as the blocks of polymers A and B in the graft copolymer according to component C.

14. The polymer composition according to claim 13, wherein the ratio of the mass proportion of polymer A in the polymer composition based on the sum of polymers A and B in the composition to the mass proportion of grafted branches in the graft copolymer according to component C is 0.6 to 1.

4.