Mixed platinum ruthenium oxides and electrodes for oxygen evolution reactions
Through the mixed oxide catalyst of platinum, palladium and transition metal, the problems of lack of iridium resources and poor stability in the oxygen evolution reaction are solved, and efficient and economical catalytic effect is achieved, which is suitable for corrosive conditions of PEM water electrolytic cells.
Patent Information
- Application Number
- CN202380028425.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-21
- Filing Date
- 2023-01-17
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the oxygen evolution reaction catalyst often uses the precious metal iridium (Ir), but its resources are limited and expensive, making it difficult to achieve economical and efficient catalytic effects in PEM water electrolytic cells, especially poor stability under corrosive conditions.
A mixed oxide catalyst composed of platinum (Pt) and palladium (Pd) oxides and transition metals (such as Cr, Ir, Mn, Si, V, Re, Nb, Ti, Sn, Pb, Ru) is used to react through solid phase Form a multiphase structure, including MO2 and Mex(Pt/d)yO4, combined with X-ray photoelectron spectroscopy (XPS) and transmission electron microscopy (TEM) analysis, optimized particle size and composition to improve activity and stability.
High catalytic activity and stability under acidic corrosive conditions are achieved, the service life of the catalyst is significantly improved, the problem of lack of iridium resources is solved, and a more economical and sustainable catalyst alternative is provided.
Smart Images

Figure BDA0005047971240000061 
Figure BDA0005047971240000101 
Figure BDA0005047971240000111
Abstract
Description
[0001] manual
[0002] The present invention relates to mixed metal oxide catalysts, particularly oxide-based catalysts containing Pt and Ru, for use in polymer electrolyte membrane (PEM) fuel cells, water electrolysis, regenerative fuel cells (RFC) or oxygen generation electrodes in various electrolysis applications.
[0003] Hydrogen is a promising clean energy carrier that can be produced by various technologies. High-quality hydrogen can be produced by water electrolysis. As known to those skilled in the art, a water electrolyzer contains at least one half-cell containing an anode in which an oxygen evolution reaction (OER) occurs, and at least one half-cell containing a cathode in which a hydrogen evolution reaction (HER) occurs. If two or more cells are connected together, a stacked configuration is obtained. Therefore, a water electrolyzer having a stacked configuration contains at least two half-cells containing an anode and / or at least two half-cells containing a cathode.
[0004] Different types of water electrolysers are known.
[0005] In a PEM water electrolyser, a solid polymer electrolyte is used which is responsible for the proton transport from the anode to the cathode while electrically insulating the electrodes from each other and for the separation of the product gases.
[0006] Due to its complexity, the oxygen evolution reaction has slow kinetics, which is why significant overpotentials are required on the anode side for oxygen to be produced at a reasonable rate. Typically, PEM water electrolyzers operate at voltages of about 1.5 V to 2 V. Since the pH is quite acidic (PEM: pH less than 2) and an overpotential must be applied, the materials present on the anode side of a PEM water electrolyzer need to be very corrosion resistant.
[0007] Typically, the anode of the water electrolyzer includes a catalyst for the oxygen evolution reaction (OER electrocatalyst). Suitable OER electrocatalysts are known to those skilled in the art and have been described by, for example, M. Carmo et al., "A comprehensive review on PEM water electrolysis", International Journal of Hydrogen Energy, Vol. 38, 2013, pp. 4901-4934; and H. Dau et al., "The Mechanism of Water Oxidation: From Electrolysis via Homogeneous to Biological Catalysis", ChemCatChem, 2010, 2, pp. 724-761.
[0008] It is known that iridium oxide or ruthenium oxide is an effective catalyst for the oxygen evolution reaction (EP 2 608 297 A1, Reier et al. Electrocatalytic Oxygen Evolution Reaction in Acidic Environments-Reaction Mechanisms and Catalysts. Adv. Energy Mater. 2017, 7, 1601275).
[0009] However, iridium resources are scarce and expensive, and ruthenium oxide alone or in the form of Pt-Ru alloys has little stability. Limited iridium resources will be a major obstacle to the development of PEM electrolysis technology. In order to expand the use of electrolyzers, anodes made of cheaper and more abundant materials are needed.
[0010] As an alternative form of iridium catalyst, some research has been conducted on platinum metal oxides using +1 / +2 / +3 ions such as Li, Na, Mg, Ca, Zn, Cd, Co, Ni, Mn, Cu, Ag, Bi, In and Ce, where the +1 / +2 ions fit perfectly into the bronze structure.
[0011] EP 3 581 682 discloses an anode for electrolysis, the anode comprising a homogeneous platinum bronze M containing a metal element M. x Pt3O4, where the metal element M is selected from the group of Mn, Co, Cu, Ag, Bi and Ce. These anodes are cheap and have excellent duration, and are therefore good alternatives to Ir anodes. However, the activity is still lower than that of Ir anodes.
[0012] RD Shannon et al., Inorg. Chem., 21, 3372 (1982) disclosed a method for synthesizing MxPt304 (M = Li, Na, Mg, Ca, Zn, Cd, Co and Ni).
[0013] WO03 / 005474 discloses an oxidation catalyst comprising metal oxide particles having a composition of PdCoO2 or PtCoO2. US 2008 / 050640 discloses a catalyst comprising PtRuOx. US 2002 / 183200 discloses a platinum titanium carbon (PtTiOJC) catalyst, the mass percentage of Pt is 40 weight %, and the atomic ratio is Pt:Ti=5:1.
[0014] WO 2018 / 110423 describes the synthesis of platinum bronze MxPt304 by mixing platinum oxide (PtO2) with metal nitrates in a molar ratio of 3:1 to obtain MxPt304 and Pt. As metal nitrates, Co, Ce, Ca, Li, Na, Bi, Ag, Cu, Mn and In are used. All metal nitrates are solid and mixed with platinum oxide using a mortar. In both cases, the metal nitrates are brought into solution and impregnated on platinum oxide. In addition to the MxPt304 (M=Co) phase, XRD analysis did not detect any other Pt phase.
[0015] Yim et al., International Journal of Hydrogen Energy 30 (2005) 1345 describe a method for preparing a hybrid PtRuOx material by physically mixing Pt and RuOx to obtain an electrocatalyst with an appropriate composition. The inorganic Ru precursor is dissolved in deionized water, and the aqueous solution is then dried at 110°C for 12 hours and subsequently calcined in air at 400°C for 5 hours to form an oxidized phase.
[0016] Kamitaka et al. Catalysts 2018, 8, 258 discloses Co-Pt bronze for electrocatalysis in acidic media.
[0017] Yi et al., in “Effect of Pt introduced on Ru-based electrocatalyst for oxygen evolution activity and stability” (Electrochemistry Communications 104 (2019) 106469), disclosed a catalyst composed of Ru9Pt1 deposited on a carbon support. The results showed that by including Pt in the Ru structure, the stability of ruthenium can be improved. However, the presence of the carbon support makes the material unsuitable for electrolytic applications due to the corrosive environment.
[0018] The OER activity of other compounds containing ruthenium or iridium, such as isochlores and perovskites, has been studied (L. C. Seitz, C. F. Dickens, K. Nishio, Y. Hikita, J. Montoya, A. Doyle, C. Kirk, A. Vojvodic, H. Y. H. Wang, J. K. Norskov, and T. F. Jaramill0, “A highly active and stable IrOx / SrIrO3 catalyst for the oxygen evolution reaction,” Science, Bd. 353, p. 1011, 92016).
[0019] The object of the present invention is to provide a composition which is not based on iridium and is reduced iridium or does not contain iridium at all and which is an effective electrocatalyst, in particular for the oxygen evolution reaction, shows a high stability under very corrosive conditions (for example in PEM water electrolysis or PEM fuel cells) and is viable from an economic point of view.
[0020] invention
[0021] The catalyst composition comprises a platinum and / or palladium (Pt / d) oxide and a transition metal (M) oxide that forms a +4 ion, preferably, wherein M=Cr, Ir, Mn, Si, V, Re, Nb, Ti, Sn, Pb and / or Ru, and the composition comprises at least two separate oxide phases: (i) MO2 phase and (ii) Me x (Pt / d) y O4 phase, wherein Me = M, Pt, Ca, Sr, Ba, Bi, Pd, Mn, Co, Cu, Ag, Ce, Mg, Zn, Cd, Co, Ni, Li, Na and / or K, and x = 0.1 to 0.9 and y = 2.7 to 3, wherein the particle size of the MO2 phase particles is in the range of 5 nm (d10) and 70 nm (d90), and the Me x (Pt / d) y The particle size of the particles of the O4 phase is in the range of 5 nm (d10) and 80 nm (d90) both measured by TEM particle size analysis.
[0022] Preferably, Me represents M, Pt, Pd, Sr, Bi, Na and / or K, more preferably, represents M, Pt, Na and / or K.
[0023] Preferably, the MO2 phase is a tetragonal phase. Preferably, Me x (Pt / d) y The O4 phase is a cubic phase.
[0024] Preferably, the particle size of the particles of the MO2 phase measured by TEM particle size analysis is in the range of 2nm (d10) and 60nm (d90), more preferably, in the range of 7nm (d10) and 50nm (d90), even more preferably, in the range of 10nm (d10) and 40nm (d90). Preferably, all particles of the MO2 phase have a particle size below 100nm measured by TEM particle size analysis.
[0025] Preferably, Me x (Pt / d) y The particle size of the particles of the O4 phase measured by TEM particle size analysis is in the range of 2nm (d10) and 70nm (d90), more preferably, in the range of 7nm (d10) and 60nm (d90), even more preferably, in the range of 10nm (d10) and 50nm (d90), even more preferably, in the range of 15nm (d10) and 50nm (d90).
[0026] Preferably, Me x (Pt / d) y All particles of the O4 phase had a particle size below 100 nm as measured by TEM particle size analysis.
[0027] Preferably, the catalytic composition comprises platinum oxide and ruthenium oxide, which comprises at least two separate oxidation phases (i) RuO2 phase and (ii) MexPt3yO4 phase. Preferably, the ratio of Ru to Pt is between 0.04 and 5, more preferably between 0.1 and 2, in particular between 0.4 and 0.7.
[0028] Preferably, the catalyst composition shows a platinum peak having a binding energy of Pt 4f between 71 eV and 75 eV and a ruthenium peak having a binding energy of Ru 3d between 279 eV and 282 eV in an X-ray photoelectron spectroscopy (XPS) spectrum.
[0029] Preferably, the binding energy gap between O1s and Ru3d is between 248.40 eV and 248.60 eV. Preferably, the binding energy gap between O1s and Ru3d is lower than 248.60 eV.
[0030] The present invention also includes a method comprising the steps of: (a) mixing a predetermined amount of a platinum or palladium raw material with a transition metal (M) that forms +4 ions; (b) subjecting the raw material mixture to a solid phase reaction; and (c) removing by-products from the resulting reactant, wherein the transition metal raw material that forms +4 ions is provided in the form of a liquid solution.
[0031] The present invention demonstrates that the synthesis of platinum or palladium metal oxides using a second element that forms a +4 ion does not result in a homogeneous bronze structure.
[0032] The present invention demonstrates that materials based on platinum and ruthenium show surprisingly high catalytic activity for the oxygen evolution reaction and are very stable under highly corrosive conditions. Ruthenium is available 20 times more than iridium. This will solve the iridium supply problem and allow large-scale PEM electrolysis installations.
[0033] Catalyst characterization
[0034] The term "composite catalyst" means a catalyst containing a platinum or palladium oxide and a transition metal oxide forming a +4 ion and optionally elementary particles.
[0035] The catalyst composition contains a transition metal (M) forming +4 ions, preferably those transition metals (M) forming a tetragonal rutile network, such as CrO2, IrO2, MnO2, SiO2, VO2, ReO2, NbO2, TiO2, SnO2, PbO2, RuO2, more preferably, Ir, Sn, Re, Nb and / or Ru, especially ruthenium.
[0036] The catalyst composition preferably contains platinum.The catalyst composition preferably contains both platinum and ruthenium.
[0037] In the following description, the term "platinum" is used for and includes both options of platinum or palladium, and the term "ruthenium" is used for and includes all transition metal oxides that form +4 ions.
[0038] The atomic ratio of platinum to ruthenium can vary within a wide range. Typically, the atomic ratio of ruthenium to platinum is between 0.04 and 5, more preferably between 0.1 and 2, and in particular between 0.4 and 0.7.
[0039] Preferably, the total amount of platinum in the catalyst composition is in the range of 30 wt. % to 99 wt. %, more preferably, 40 wt. % to 98 wt. %, more preferably, 50 wt. % to 97 wt. %, more preferably, 60 wt. % to 96 wt. %, more preferably, 65 wt. % to 95 wt. %, more preferably, 70 wt. % to 95 wt. %, in particular 80 wt. % to 90 wt. %, relative to the total mass of the catalyst.
[0040] Preferably, the total amount of ruthenium in the composition is in the range of 1 wt. % to 70 wt. %, more preferably, 2 wt. % to 60 wt. %, more preferably, 3 wt. % to 50 wt. %, more preferably, 4 wt. % to 40 wt. %, more preferably, 5 wt. % to 35 wt. %, more preferably, 7 wt. % to 30 wt. %, in particular 10 wt. % to 20 wt. %, relative to the total mass of the catalyst.
[0041] Preferably, the catalyst composition contains 0.01 to 15 wt.-% Ca, Sr, Ba, Bi, Mn, Co, Cu, Ag, Ce, Mg, Zn, Cd, Co, Ni, Li, Na and / or K, preferably alkali metals, even more preferably Li, Na and / or K, especially sodium, relative to the total mass of the platinum precursor, e.g. PtO2.
[0042] Preferably, the remainder up to 100% by weight is oxygen.
[0043] Preferably, the catalyst composition contains 65 to 75 wt% of platinum, 10 to 20 wt% of ruthenium, 0.5 to 2 wt% of alkali metal (preferably sodium) and the remainder up to 100 wt% of oxygen, relative to the total mass of the catalyst.
[0044] The oxidation states of platinum and ruthenium can be verified by XPS.
[0045] Preferably, the ruthenium is present in oxidation state +IV as indicated by the Ru 3d signal in XPS.
[0046] Preferably, the platinum is present in a mixed valence state containing Pt atoms in oxidation state +IV and Pt atoms in oxidation state +II.
[0047] In addition, Pt in oxidation state 0 and polarized Pt species ("Pt(+δ)"), where the binding energy of the Pt 4f electrons is between that expected from Pt atoms in oxidation states 0 and +II, as detected in XPS measurements.
[0048] The exact binding energies of the Pt 4f7 / 2 and 5 / 2 signals can be obtained from Table 1. The positions of all species except Pt(0) are given relative to the Pt(0) signal.
[0049] Table 1: Table of binding energies with different Pt signals
[0050]
[0051] Preferably, 2 to 30 atom %, more preferably, 3 to 20 atom %, even more preferably, 5 to 10 atom % of the platinum is present in the oxidation state +IV.
[0052] Preferably, 10 to 50 atom %, more preferably 15 to 45 atom %, even more preferably 30 to 40 atom % of the platinum is present in oxidation state +II. Preferably, 5 to 30 atom %, more preferably 10 to 25 atom %, even more preferably 10 to 20 atom % of the platinum is present in oxidation state +II, type I. Preferably, 5 to 30 atom %, more preferably 10 to 25 atom %, even more preferably 10 to 20 atom % of the platinum is present in oxidation state +II, type II.
[0053] Preferably, 30 to 80 atomic %, more preferably, 45 to 65 atomic %, even more preferably, 55 to 60 atomic % of the platinum is present in the oxidation state (Pt(+δ)). Preferably, 0 to 15 atomic %, more preferably, 0 to 10 atomic %, even more preferably, 0 to 6 atomic % of the platinum is present in the oxidation state 0.
[0054] Preferably, platinum is present in an oxidation state of +IV at 5 to 10 atomic %, an oxidation state of +II (Type I) at 10 to 20 atomic %, an oxidation state of +II (Type II) at 10 to 20 atomic %, an oxidation state of (Pt(+δ)) at 55 to 60 atomic %, and an oxidation state of 0 at 0 to 8 atomic %.
[0055] Preferably, 80 to 100 atomic %, more preferably 90 to 100 atomic %, even more preferably 95 to 100 atomic % of the ruthenium is present in oxidation state +IV, as indicated by the Ru 3d signal in XPS. In particular, all of the ruthenium is present in oxidation state +IV.
[0056] The gap between the binding energies of O1s and Ru3d is preferably below 248.60 eV and is therefore approximately 0.2 eV narrower than that of non-inventive materials having similar compositions.
[0057] The Pt phase (Me x (Pt / d) y The particle size of the O4 phase) is preferably 10nm to 60nm on average, more preferably 20nm to 50nm, more preferably 20nm to 40nm, more preferably 10nm to 40nm, especially 15nm to 35nm.
[0058] The particle size of the Ru phase characterized by TEM measurement is preferably 5 nm to 60 nm on average, more preferably 10 nm to 35 nm, further preferably 15 nm to 30 nm.
[0059] The MexPtyO4 unit cell volume undergoes some shrinkage and is preferably below As measured by XRD, the unit cell volume of MexPtyO4 is preferably and More preferably, between and More preferably, between and The XRD grain size of the Pt phase is below 20 nm. Preferably, it is between 5 nm and 17 nm, more preferably, it is between 10 nm and 15 nm, and most preferably, it is between 11 nm and 14 nm.
[0060] The shape of the particles is preferably spherical. Preferably, the shape of the Pt particles is not cubic.
[0061] At the nanoscale, the platinum and ruthenium phases are preferably distributed inhomogeneously. Preferably, there are different Pt- and Ru-rich regions that do not mix significantly. Platinum and ruthenium preferably reside in segregated form, but traces of up to 10 wt.% platinum / ruthenium can be detected (incorporated) in the structure of the Ru / Pt phase, and vice versa.
[0062] On a macroscopic scale, these Ru- and Pt-rich regions / phases are uniformly distributed.
[0063] Preferably, sodium is predominantly present in / associated with the Pt-rich phase, preferably greater than 80% of the total sodium content, as characterized by TEM EDX.
[0064] Preferably, the catalyst composition comprises two phases.
[0065] (i) RuO2 phase, preferably, tetragonal RuO2 phase.
[0066] (ii)Me x PtyO4 phase, preferably cubic Me x Pt y O4 phase, where Me = Ru, Pt and / or Na and x = 0.1-0.9 and y = 2.7-3.
[0067] Preferably, the phase (i) RuO2 and (ii) Me x Pt y The ratio of O4 is between 0.02 and 5, preferably between 0.1 and 2, most preferably between 0.2 and 0.7.
[0068] The BET surface area of the catalyst composition of the present invention is 5 m 2 / g to 200m 2 / g, preferably 20m 2 / g to 150m 2 / g, more preferably, 30m2 / g to 100m 2 / g.
[0069] Carrier
[0070] The bulk catalyst may have a limited electrochemically active surface area. In order to increase the catalytically active surface area, the catalyst composition may also be loaded on a suitable carrier material. The carrier material is preferably an inorganic oxide, carbide or nitride material, such as antimony-doped tin oxide (ATO), low-valent titanium oxide (TiO, Ti2O3, Ti3O5 and Ti4O7), TiC, ZrC, HfC, TaC, TiN, ZrN, HfN, TaN, boron carbide, boron-oxygen-carbide or boron carbide containing other elements such as boron silicon carbide, more preferably, TiO2, doped or undoped SnO2.
[0071] The catalyst composition of the present invention may also be used as a support material itself and coated with further catalytic materials, for example with iridium.
[0072] Method for producing catalyst
[0073] Ruthenium platinum oxide is obtained by the following steps:
[0074] (a) mixing a predetermined amount of a raw material of platinum or palladium and a transition metal that forms a +4 ion, preferably a predetermined amount of a raw material of ruthenium and platinum;
[0075] (b) subjecting the raw material mixture to a solid phase reaction under predetermined conditions; and
[0076] (c) removing by-products from the obtained reaction product as necessary.
[0077] The starting material of the transition metal which forms the +4 ion is provided in the form of a liquid solution.
[0078] mix :
[0079] First, mix the raw materials of ruthenium and platinum. There is no particular limitation on the platinum source, and examples of platinum sources include: platinum oxide (PtO2); and / or nitrates, chloro complexes, ammine salts and hydroxy complexes of platinum, preferably PtO2. Platinum oxide may also contain sodium in the range of 0.1 wt% to 5 wt%, most preferably in the range of 1 wt% to 2 wt%, relative to the total mass of the platinum oxide compound used. There is no particular limitation on the ruthenium source, and examples of metal sources include: salts of inorganic anions, such as nitrates, fluoride salts, chloride salts, bromide salts, iodide salts, carbonates, perchlorates, preferably nitrates.
[0080] The optimum mixing ratio of ruthenium and platinum is selected according to the purpose and is as described above.
[0081] Preferably, a Pt precursor is used whose sodium content is 0.1 wt% to 5 wt%.Preferably, the sodium changes the crystal structure of the Pt precursor so that a stable Pt Ru oxide material is formed during the heat treatment step.
[0082] Preferably, mixing is performed to enable intimate contact between the precursors, leading to critical interaction of the participating elements during the subsequent thermal treatment step. Intimate contact can be achieved by optimizing wetting.
[0083] Different mixing techniques may result in different material properties. Mixing the Pt and Ru precursors after temperature treatment of the materials individually does not result in the catalyst of the present invention.
[0084] Intimate mixing of the precursors will result in:
[0085] - Less Pt leaching during the aqua regia (AR) treatment step
[0086] - Small amounts of elemental Pt (characterized by XRD) and cubic Pt particles
[0087] Composition (characterized by TEM)
[0088] - Smaller Pt and Ru oxide particles (characterized by TEM)
[0089] -Me x Pt y The grain size of O4 is less than 20nm and the shrinkage rate of unit cell volume is lower than
[0090] -The change of ionization energy of Na1s, O1s and Ru3d, among which the ion between O1s and Ru3d
[0091] Energy gap less than 248.6 eV (measured by XPS)
[0092] -High electrochemical activity / stability
[0093] Heat Treatment :
[0094] Then, the raw material mixture is subjected to solid phase reaction. The reaction temperature depends on the composition of the platinum ruthenium oxide, usually 500°C to 800°C, preferably 550°C to 750°C, more preferably 600°C to 700°C. The reaction time is usually several minutes to several hours, preferably between 30 minutes and 12 hours, particularly between 4 hours and 8 hours. When a liquid Ru precursor is used, preferably, a drying step is performed before the solid phase reaction. The drying temperature is preferably between 60°C and 100°C, particularly between 70°C and 90°C. The drying time is usually about several minutes to several hours, preferably between 15 minutes and 2 hours, particularly between 20 minutes and 40 minutes. Typically, the heat treatment is carried out in an oxidizing atmosphere such as air. In principle, an inert atmosphere can also be used.
[0095] Optionally, the heat treatment may be repeated, for example 1 to 4 times.
[0096] purification
[0097] The solid phase product is already an electrocatalytically active and stable material. Byproducts, such as oxidizable Pt species, can then be optionally removed from the resulting reactants. Preferably, the byproducts are removed by aqua regia treatment. Preferably, the aqua regia treatment is carried out at room temperature to the boiling point of aqua regia (108° C.) for 10 to 120 minutes, preferably at 70 to 90° C. for 20 to 40 minutes.
[0098] The obtained platinum ruthenium oxide is preferably filtered to remove soluble components.
[0099] The leaching of platinum upon aqua regia treatment is preferably in the range between 30% and 60% (see Table 5).
[0100] Finally, the platinum ruthenium oxide is optionally dried. The drying step is preferably carried out at a temperature of 70° C. to 90° C. and a pressure of 50 mbar to 1000 mbar for 12 to 24 hours.
[0101] The final platinum ruthenium oxide may be subjected to a second, repeated heat treatment.
[0102] Manufacturing of anodes / applications
[0103] To make electrodes or catalyst-coated membranes, the catalyst composition can be processed into inks or pastes by adding a suitable solvent.The catalyst ink can be deposited on a gas diffusion layer (GDL), current collector, membrane or separator by known deposition methods.
[0104] The present invention also relates to an electrochemical device containing the catalyst composition.
[0105] The electrochemical device may be an electrolyser, in particular a water electrolyser, such as a PEM water electrolyser, or a fuel cell, such as a PEM fuel cell. The PEM fuel cell may also be a regenerative PEM fuel cell.
[0106] As in any water electrolyzer, in the PEM water electrolyzer of the present invention there is at least one half-cell containing an anode in which the oxygen evolution reaction occurs and at least one half-cell containing a cathode in which the hydrogen evolution reaction occurs. The catalyst composition is present in the half-cell containing the anode.
[0107] According to another aspect, the invention relates to the use of a catalyst composition as described above as a catalyst for an oxygen evolution reaction, for example in an electrolyser or a regenerative fuel cell or other electrochemical device.
[0108] advantage
[0109] In contrast to the prior art, the described invention demonstrates that mixed platinum ruthenium oxide catalytic materials have surprisingly high activity and stability (much greater than the individual binary oxides) in the electrochemical oxygen evolution reaction under acidic conditions. Surprisingly, the beneficial mixing effect is confirmed in a wide ratio of Pt / Ru. The present invention solves the problem of limited Ir supply by providing an alternative mixed oxide of Pt and Ru, which are elements with significantly higher availability. In contrast to other reported materials containing Ru, higher stability is achieved. The mixed oxide is also significantly more active than the recently reported platinum bronze, and shows that the material has significantly different properties. The catalyst is shown to have commercially relevant activity under actual operating conditions in a single PEM electrolyzer.
[0110] Table 2 summarizes the characteristics of the catalysts of the present invention and compares these characteristics with those of materials of similar composition but lacking the advantages of the invention described herein.
[0111] Table 2: Summary of inventive features and comparison with non-inventive materials.
[0112]
[0113] Example
[0114] Experimental procedures
[0115] 1. X-ray diffraction pattern of powder
[0116] The samples were homogenized in a mortar and flattened into a sample holder and data were collected on a Bruker AXSD8 Advanced Diffractometer using a copper anode operating at 40 kV and 40 mA. Scans were performed from 2° to 80° (2θ) using a step size of 0.02° (2θ). TOPAS 6 (1) Analytical data. Using cubic Pt3O4 (2) , Tetragonal RuO2 (3) Platinum (4) The simulated powder diffraction pattern was modeled based on the crystal structure of . Quantitative data are reported from the refined model. Crystallite sizes are reported using the integrated width method (LVol-IB) as reported by TOPAS.
[0117] For sample BRZ4-AR, a basic structural model was created ( 2 ) in an attempt to improve the fit of the calculated diffraction patterns to the experimental data. The table below shows the quality of fit for the models of Na, Ru and Pt with unit cell origin. They show no discernible differences in the calculated diffraction patterns. The quality is reported using the RBrag statistic, which gives an understanding of the residual (R) of the experiment to the calculated data relative to a single structure in a model containing multiple structures. This is done in TOPAS6 ( 1 ) software. RBragg is defined as the residual, cumulative misfit of the model compared to the experiment. RBragg values are given in %. The lower the RBragg value, the better the experimental results are described by the model. Clearly, the model containing electron density at the origin of the unit cell (see the first three entries in Table 1) does show a better correspondence with the experimental data than the last entry in Table 1 where this position is unoccupied. RBragg values below 3% indicate a statistically significant improvement. Therefore, MexPtyO4, where Me = Na, Ru, Pt and x = 0.1-0.9 and y = 2.7-3, gives a better structural description than assuming only the Pt3O4 phase.
[0118] Table 3: Comparison of RBrag values for different crystal structures fitted to the BRZ-4-AR diffraction pattern. The crystal structure with occupied positions at coordinates (0,0,0) shows a lower cumulative misfit (residual) of about 3% compared to the Pt304 structure with unoccupied (0,0,0) positions.
[0119] structure RBragg, % <![CDATA[Na 0.9 Pt 2.7 O4]]> 5.2 <![CDATA[Ru 0.1 Pt 2.8 O4]]> 5.4 <h2 style=";text-align:left;direction:ltr"><![CDATA[Pt <h2 style=";text-align:left;direction:ltr"> 0.1 <h2 style=";text-align:left;direction:ltr"> Pt3O4<h2 style=";text-align:left;direction:ltr"> 5.3 <![CDATA[Pt3O4 (5) ]]> 8.5
[0120] literature
[0121] (1)TOPAS 6 User Manual, 201 7, Bruker AXS GmbH.Karlsruhe, Germany
[0122] (2)B.Grande,Hk.Müller-Buschbaum,Ein Beitrag zu Verbindungen vomTyp Mex Pt 3 O 4,Journal of Inorganic and Nuclear Chemistry,Vol:39,Issue:6.1084-1085(1977).
[0123] https: / / doi.org / 10.1016 / 0022-1902(77)80270-4
[0124] (3)F.A.Cotton and J.T.Mague,The Crystal and Molecular StructureofTetragonal Ruthenium Dioxide Inorganic Chemistry 19665(2),317-318DOI:10.1021 / ic50036a037
[0125] (4)Albert W.Hull,X-Ray Crystal Analysis of Thirteen Common Metals,Phys.Rev.17,571-588,1921
[0126] (5)Hector,A.L.,Parkin,I.P.Solid state metathesis preparations ofgroup VIII metal oxide powders.J Mater Sci Lett 13,219-221(1994).
[0127] https: / / doi.org / 10.1007 / BF00278 1 68
[0128] 2.TEM images and EDS distribution
[0129] The powder sample is dispersed in ethanol and applied to an ultrathin carbon-coated grid by a drop-on-grid-method. The Themis Z 3.1 machine (Thermo-Fisher, Waltham, USA) using probe correction is imaged by transmission electron microscopy (TEM) in different acquisition modes including high-angle annular dark field (HAADF) scanning transmission electron microscopy (STEM), integrated differential phase contrast (iDPC)-STEM, bright field TEM and electron diffraction. Chemical composition is analyzed with an integrated SuperX G2 energy dispersive x-ray spectroscopy (EDXS) detector (Thermo-Fisher, Waltham, USA). Data are analyzed using Velox 2.1x software (Thermo-Fisher, Waltham, USA). Particle size analysis was performed using the FIJI software tool (Schindelin, J., Ar-ganda-Carreras, I., Frise, E., Kaynig, V., Longair, M., Pietzsch, T., Cardona, A. (2012)). Fiji: an open source platform for biological image analysis. Nature Methods, 9(7), 676-682. doi: 10.1038 / nmeth.2019). Diffraction patterns were evaluated using Prodas software (Proscope, Gangelt, Germany, version: 1.4).
[0130] 3.XPS .
[0131] XPS analysis was performed with a Phi Versa Probe 5000 spectrometer using monochromatic Al Ka radiation. The XPS system was calibrated according to ISO 15472.2001. The BE (binding energy) of Au4f7 / 2 is 84.00 eV and the BE (binding energy) of Cu2p3 / 2 is 932.62 eV.
[0132] All samples were mounted insulated relative to ground and neutralized with a built-in charge neutralizer during the measurement and were measured at three non-overlapping sample locations using a spot size of 0.1 x 1.4 mm (large area mode).
[0133] Survey scan analysis was performed at a pass energy of 117.4 eV and an energy step size of 0.5 eV. High-resolution analysis was performed over the same analysis area at a pass energy of 23.5 eV and an energy step size of 0.1 eV.
[0134] The spectrum has been charge corrected to the maximum of only the Ru 3d line of RuO2, thus set at 280.6 eV.
[0135] All spectra were analyzed using standard XPS analysis software such as CasaXPS (Fairley N, (2021). CASA-XPS, 2.3.50 Rev1-0D, Casa Software Ltd) using Shirley background subtraction of the main peaks of the elements of interest. Quantification was performed using the relative sensitivity factors and transmission functions provided by the instrument manufacturer.
[0136] The Pt4f-signal was fitted with five doublets with an energy separation of 3.3 eV using the following constraints and line shapes. For all doublets, the area of the Pt 4f 5 / 2 peak was fixed at 0.75 times the area of the Pt 4f 7 / 2 peak. The metallic part of the Pt-signal was fitted based on the natural line shape (Pt-NULL-Lineshape) derived from the measurement of a pure metal reference.
[0137] The exact positions and FWHM are given in Table 4 together with the line shapes used.
[0138] Table 4: Exact line positions and FHWM of all Pt4f signals
[0139]
[0140]
[0141] XPS measurements were performed on all Pt Ru oxide samples. The Ru 3d signal indicated the presence of only RuO2 (see Figure 6 ).
[0142] 4. Electrochemical Measurements
[0143] The experiments were carried out in 0.5M H2SO4 electrolyte at room temperature and under argon atmosphere. The catalyst was dispersed in H2O / IPA 10 / 1 at 1 wt % to obtain an ink by ultrasonic treatment, which was drop-cast onto a gold electrode. All catalysts were deposited to achieve the same total mass loading on the electrode as the film. The electrode was immersed in the electrolyte and the activity was measured by linear sweep voltammetry in a potential range of 1.2 V to 1.7 V relative to the reversible hydrogen electrode (RHE).
[0144] Preparation of Examples
[0145] Sample of the present invention
[0146] According to Figure 1The method described in a was used to prepare binary platinum ruthenium oxide with a platinum to ruthenium ratio of 3: 1. Ru(NO)NO3 solution with a Ru content of 18.8 wt% from BASF Italia (batch number: 9002401825) was added dropwise to the PtO2 precursor and mixed by completely covering / wetting the solid precursor. PtO2 (model 206032) with a Na content of 1.6 wt% from Sigma Aldrich was used.
[0147] The PtO2 impregnated with the Ru-containing solution was then ground into a fine powder. The powder was then dried and heat treated using the following protocol.
[0148] 1. Dry at 80℃ for 12 hours
[0149] 2. Heating at 5K / min to 650°C
[0150] 3. Maintain at 650℃ for 6 hours
[0151] 4. Cooling (10k / min)
[0152] After the heat treatment, a portion of the sample was treated with aqua regia at 80°C for 30 minutes. The aqua regia treated sample was then dried again at 80°C for 12 hours. The composition of the resulting material was examined by atomic emission spectroscopy. Two samples, BRZ-4-AR and H2-PEM-185, were prepared according to this procedure. The preparation method of the inventive sample I is described in Figure 1 .a.
[0153] For one sample, the ratio of Ru / Pt was measured before and after the aqua regia treatment.
[0154] Comparison of the calculated and measured Ru / Pt ratios of Table 5 as well as comparison of the Ru / Pt ratios of the non-aqua regia and aqua regia treated samples clearly shows that Pt is removed, resulting in systematically higher Ru / Pt ratios.
[0155] Table 5: Effect of aqua regia treatment on the Ru / Pt ratio of the samples of the present invention
[0156]
[0157] Comparative Example 1
[0158] For the first comparative example, samples containing PtO2 and RuO2 were prepared according to the general preparation process outlined by Yim et al. PtO2 (model 206032) with a Na content of 1.6 wt% from Sigma Aldrich was used as the Pt-containing material. Ru(NO)NO3 solution (Ru content of 18.8 wt%) from BASF Italia (lot number: 9002401825) (as used in the present embodiment) was used as an inorganic Ru precursor. The Ru aqueous solution was dried and heat treated separately in the absence of other metal precursors. The following protocol was used:
[0159] 1. Dry at 80°C (dry in a vacuum drying oven and continue drying until the solution becomes dry powder)
[0160] 2. Heating at 5K / min to 650°C
[0161] 3. Maintain at 650℃ for 6 hours
[0162] 4. Cooling (10k / min)
[0163] The individually heat treated samples were then physically mixed and ground into a fine powder. A portion of this material was subjected to the same aqua regia treatment as described in the examples of the present invention. Two samples were prepared following this procedure. The preparation method of this comparative sample I is described in Figure 1 .b.
[0164] For one sample, the ratio of Ru / Pt was measured before and after the aqua regia treatment.
[0165] The resulting Ru / Pt ratios are given in Table 6. The Pt loss upon aqua regia treatment appears to be significantly higher than that of the corresponding inventive samples with comparable Ru / Pt ratios (see Table 5).
[0166] Table 6: Ru / Pt ratio of Comparative Example I with and without aqua regia treatment
[0167] Ru / Pt; calculated Ru / Pt, measured Loss of Pt Activity (I@1.6V vs RHE, in mA) H2-PEM-192-1 0.33 0.33 0% 0.101 H2-PEM-192-2 0.33 0.93 64.5% 0.307
[0168] Comparative Example II
[0169] For the second comparative example, samples containing PtO2 and RuO2 were prepared according to the general preparation process outlined in WO 2018 / 110423. PtO2 (model 206032) with a Na content of 1.6 wt% from Sigma Aldrich was used as a Pt-containing material. Ru(NO)NO3 solution (Ru content of 18.8 wt%) from BASF Italia (batch number: 9002401825) (as used in the embodiments of the present invention) was used as an inorganic Ru precursor. The Ru aqueous solution was dried at 120°C for 12 hours to a solid and mixed with platinum oxide using a mortar.
[0170] Use the following scheme:
[0171] 1. Dry at 80°C (dry in a vacuum drying oven and continue drying until the solution becomes dry powder)
[0172] 2. Heating at 5K / min to 650°C
[0173] 3. Maintain at 650℃ for 6 hours
[0174] 4. Cooling (10k / min)
[0175] The material was subjected to the same aqua regia treatment as described in the examples of the present invention. The preparation method of comparative sample II is described in Figure 1 .c. in.
[0176] The resulting Ru / Pt ratios are given in Table 7. The Pt loss upon aqua regia treatment appears to be significantly higher than that of the corresponding inventive samples with comparable Ru / Pt ratios (see Table 5).
[0177] Table 7: Ru / Pt ratio of Comparative Example II with and without aqua regia treatment
[0178] Ru / Pt; calculated Ru / Pt, measured Loss of Pt <![CDATA[Activity( I@1.6V for RHE, in mA)]]> BRZ-33 0.33 2.86 88% 0.312
[0179] Comparison of Inventive Examples and Comparative Examples
[0180] TEM
[0181] Figure 2 Depicted are TEM images and elemental distribution EDXS of a sample of the invention with a nominal Ru / Pt ratio of 0.33. At the nanoscale, there are distinct Pt-rich and Ru-rich regions that are not significantly mixed, while generally these Ru-rich and Pt-rich regions are evenly distributed and have an apparent particle size well below 90 nm. Na is associated with the Pt-rich particles.
[0182] The Pt and Ru rich particles are not well mixed in Comparative Sample I (H2-PEM-192) compared to the inventive sample, and the average size of the Pt and Ru rich particles is twice as large. As with the inventive sample, Na is associated with the Pt rich sample. SAED identifies not only NaPt3O4 and Pt3O4, but also PtO2 which is not detected in the inventive sample. When comparing the Pt and Ru particles, the different morphologies are evident. While the Ru particles are generally spherical in structure, the Pt particles show more rectangular structures for the comparative sample.
[0183] Comparative Example II does not have any similarity to the inventive sample. The platinum ruthenium is unevenly distributed and poorly mixed. The Ru oxide particles show a broad distribution in the range of 10nm to 150nm. The platinum oxide particles are in the range of 10nm to 5000nm.
[0184] Figure 3 a) shows a TEM image of comparative sample I after AR treatment. In contrast to the inventive sample, the Pt particles of comparative sample I have a distinct cubic shape. Figure 3 b) shows a TEM image of comparative sample II. The Pt and Ru particles are not mixed at all, and very large PtO2 up to 5000 nm can often be found.
[0185] Figure 4 and Figure 5 Box plot representations and bar graphs of Pt-rich and Ru-rich particles from TEM particle size analysis of the present invention sample 1 and comparative sample 1 are shown. In addition, Table 7 summarizes the quantiles, averages, and standard deviations of these samples. The present invention sample shows much smaller Pt-rich and Ru-rich particles, with an average size of about 22 nm for Ru and about 32 nm for Pt-rich particles. The particles of the comparative sample have much larger particles, with an average size of about 60 nm for Pt and about 66 for Ru.
[0186] No attempt was made to generate box plot representations and histograms of the Pt and Ru rich particles due to statistical irrelevance caused by the extremely poor mixing and inhomogeneous nature of Comparative Sample II.
[0187] Table 8: Quantile, average and Standard deviation.
[0188]
[0189] XPS
[0190] XPS measurements were performed on the inventive samples and the comparative samples.
[0191] Pt(+δ) appears to be somewhat less populated in the inventive samples (Table 8) compared to Comparative Sample I (Table 9).
[0192] Table 9: Atomic percentages of five Pt species found in the Pt 4f signal of the present samples
[0193] Pt(0) Pt(+d) Pt(II), Type I Pt(II), Type II Pt(IV) BRZ-4-AR 6.2 56.7 13.7 17.7 5.7 H2-PEM-185 3.0 41.8 15.6 32.1 7.5
[0194] Table 10: Atomic percentages of the five Pt species found in the Pt 4f signal of Comparative Sample I
[0195] Pt(0) Pt(+d) Pt(II), Type I Pt(II), Type II Pt(IV) H2-PEM-1 92-2 1.8 60.5 14.0 17.3 6.4 H2-PEM-1 94-2(w / AR) 5.5 63.7 12.2 14.7 3.8
[0196] Compare the peak positions of the detailed spectra of Na1s, O1s and Ru3d of sample I of the present invention and comparative sample II. For accurate analysis, the XPS spectra of all samples are moved in such a way that the maximum peak in the range between 73eV and 70eV in the Pt4f signal is superimposed at 72.00eV. The O1s spectrum is fitted in the following manner: the maximum peak of oxygen on Pt is 529.8eV, the maximum peak of RuO2 is 529.2eV, and it is allowed to shift within the limit of 0.2eV near this value. In CasaXPS, the peak shape and width of the two substances are the same (0.9+-0.05eV, symmetrical voigt line shape LA (1,1,900)). There are other peaks of organic oxygen and adsorbed water, but they are not related. Figure 6 The results of this comparison are shown for the inventive sample and comparative sample I. Although the peak position of the Na1s signal is shifted toward lower binding energy by 0.10 eV (Na1s), the oxygen contribution of RuO2 of the inventive sample is shifted toward higher binding energy by 0.15 eV to 0.20 eV (O1s) compared to the comparative sample. The Ru3d position of the inventive sample is shifted toward higher binding energy by about the same degree (0.15+-0.05 eV) compared to the comparative sample.
[0197] Figure 7 A comparison of the inventive sample and comparative sample II is provided. As with comparative sample I, the peak position of Na1s is shifted by 0.1 eV to lower binding energy, and the Ru 3d5 / 2 maximum peak is shifted by 0.15 eV to higher binding energy.
[0198] By far, Comparative II shows a much higher relative amount of RuO2 than the other samples (comparative samples and inventive samples alike), so the RuO2 signal occupies the maximum of the O1s spectrum, while the Pt-O signal is only slightly visible as a shoulder at about 529.8 eV binding energy. Therefore, although the Pt-O signal is only offset by about 0.1 eV, Figure 7 The overlay in shows a large difference in the position of the maximum peak.
[0199] The energy difference between O1s and Ru3d for the inventive samples and the comparative samples is provided in Table 11. The inventive samples show a consistent shift of the O1s and Ru3d binding energies to higher values.
[0200] Table 11: Absolute binding energy of sample I of the present invention and comparative sample II and the binding difference between O1s (RuO2) and Ru3d
[0201] RuO2(Ru3d) RuO2(O1s) Pt-O(O1s) 1s δ((RuO2)O1s-Ru3d) eV eV eV eV eV Comparison I 192-2 280.53 529.08 529.92 1069.70 248.55 Comparison I 194-2 280.51 529.08 529.92 1069.66 248.57 BRZ-4-AR of the present invention 280.70 529.31 529.88 1069.59 248.61 The present invention 185 280.64 529.25 529.86 248.61 Comparison II Reference BRZ-33 280.55 529.10 529.76 1069.75 248.55
[0202] XRD
[0203] The diffraction pattern of the sample mainly consists of two phases.
[0204] (i) Tetragonal RuO2 phase
[0205] (ii) Cubic Me x For PtyO4, the best fit was obtained for Me = Ru, Pt, Na with x = 0.1-0.9 and y = 2.7-3.
[0206] (iii) Some residual element Pt, especially for the comparative samples
[0207] Table 12 summarizes the phase composition data and grain size of this analysis for the examples of the present invention and the comparative examples. For consistency, the cubic Pt3O4 structure is used to describe the platinum oxide phase, because this allows the unit cell volume of the samples to be compared in a reliable manner. On the other hand, the measurement and comparison of grain size and unit cell volume are not affected by it in a measurable way. Obviously, the grain size Pt3O4 of the samples of the present invention is much smaller than that of the comparative samples.
[0208] The unit cell volume calculated for the inventive samples is always about 1.3 times lower than that of the comparative samples. But still higher than Pt304 grain unit cell (Russ. J. Inorg. Chem. (1971) 16, 1690-1693; Zh. Neorg. Khim. (1971) 16, 3190-3194) Only the comparative sample contained a significant amount of elemental Pt.
[0209] Table 12: Comparison of phase composition and grain size of the samples of the present invention and the comparative samples
[0210]
[0211]
[0212] The embodiments of the present invention with varying Ru / Pt ratios are as follows Figure 1 Table 12 summarizes the calculated and measured Ru / Pt ratios for these samples.
[0213] As the Ru content increases, it becomes increasingly difficult to dry the inventive examples, and the dried material begins to become very hygroscopic. In addition, for the two samples with the highest Ru content (BRZ-6, BRZ-11), the Pt loss attributed to the aqua regia treatment increases to more than 50%. No other samples with a Ru / Pt ratio higher than 5 were produced, as these samples would no longer be desirable for the reasons given.
[0214] Table 13: Calculated and measured Ru / Pt ratios and electrochemical activities of Pt Ru oxides
[0215]
[0216] XPS
[0217] For the Pt 4f signal, five species can be detected and the atomic concentrations of these species are given in Table 13. Consistent with the aforementioned inventive samples, the surface concentration of the Pt(+δ) species is mostly below 60 atomic %.
[0218] Table 14: Atomic percentage of 5Pt species found in the Pt 4f signal for the ratio of Ru / Pt Ratios of PtRu oxides varied during synthesis
[0219]
[0220]
[0221] The measured binding energy gaps between O1s and Ru3d for these samples are summarized in Table 14. In all cases, the gap is approximately 0.2 eV narrower than that of the comparative samples.
[0222] Table 15: Absolute binding energy and structure between O1s (RuO2) and Ru3d of samples of the present invention with varying Ru to P Difference
[0223] RuO2(Ru 3d) RuO2(O1s) Pt-O(O1s) 1s δ((RuO2)O1s-Ru3d) BRZ-9 280.56 529.51 529.89 1069.62 248.95 BRZ-8 280.56 529.38 529.84 1069.57 248.82 BRZ-3 280.52 529.3 529.7 248.8 BRZ-2 280.51 529.2 529.7 248.6 BRZ-1 280.63 529.21 529.85 1069.56 248.58 BRZ-5 280.51 529.1 529.7 248.6 BRZ-6 280.47 529.1 529.7 248.6 BRZ-11 280.60 529.16 529.77 1069.58 248.55
[0224] XRD
[0225] To illustrate the structural changes due to the variation in the ratio of Ru:Pt, Figure 7 Diffraction patterns showing varying ratios, starting with the first (bottommost) pattern with a Ru:Pt ratio of 0.037, the next higher pattern showing results for a Ru:Pt ratio of 0.117, the next 0.512, 2.192 and finally 4.998. The reflections of the first pattern show that Me x Strong reflections of the PtyO4 phase with some small contribution from the RuO2 phase. As the ratio of Ru / Pt increases, those reflections become weaker and those of tetragonal RuO2 become more dominant.
[0226] Table 15 summarizes the grain sizes Me of these samples. x PtyO4 (calculated based on cubic Pt3O4 structure). The obtained grain size and unit cell volume of all samples are consistent with the above results of the samples of the present invention ( Pt3O4 size <20nm) and is different from the results obtained from the comparative samples ( Pt3O4 size > 20nm). Table 144 also states the calculated relative concentrations of RuO2, Pt3O4 and Pt derived from the fit. In both cases no elemental Pt was found above 0.4 wt%.
[0227] Table 16: Grain size and Pt3O4 unit cell of inventive samples with varying Ru / Pt ratios volume
[0228]
[0229] Electrochemical activities of the examples of the present invention and the comparative examples
[0230] a.) Electrochemical activity
[0231] Comparison of the sample of the present invention (BRZ4-AR) with the Pt bronze catalyst described by Kamitaka et al. and commercially available IrO2 (Alfa Aesar) (see Fig. 9 ) show that the samples of the present invention have higher activity than various Pt bronze materials and comparable activity to IrO2. The experiments were carried out in 0.5M H2SO4 electrolyte at room temperature and under argon atmosphere. The catalyst was dispersed in H2O / IPA 10 / 1 at 1 wt % to obtain an ink by ultrasonic treatment, which was drop-cast onto a gold electrode. All catalysts were deposited to achieve the same total mass loading on the electrode as the film. The electrode was immersed in the electrolyte and the activity was measured by linear sweep voltammetry in a potential range of 1.2 V to 1.7 V relative to the reversible hydrogen electrode (RHE).
[0232] b) Effect of electrochemical cycling on cycling stability
[0233] Using the method described in a) (see Fig.10 ) Comparison of the inventive sample (BRZ4-AR) with RuO2 (Alfa Aesar) shows that although conventional RuO2 has a very high initial activity, when the material is cycled multiple times between 1.2 V and 1.7 V vs. RHE, the activity is rapidly lost and completely disappears after 30 cycles (see Fig.10 a), while the activity of the sample of the present invention is completely retained (see Fig.10 b).
[0234] c) Electrochemical activity
[0235] The method described in 5.1 was used to compare the inventive sample (BRZ4-AR) with the non-inventive comparative example I (H2-PEM-192-1) and comparative example II (BRZ 33) (see Fig.11 ), indicating that significantly higher activity was obtained by the embodiments of the present invention.
[0236] d) Activity of Examples of the Invention with Varying Ru / Pt Ratios
[0237] Relationship between activity and Ru content (see Fig.12 and Table 11) show that in a wide range of Ru / Pt contents (such as Fig.12 The activity is maintained within the measured ratio shown in Figure 1), while generally higher Ru contents lead to higher activities, albeit in a logarithmic relationship with the potential. This therefore allows the material to be prepared flexibly according to the desired application by adjusting the Ru / Pt content as required. At very low Ru loadings and completely without Ru (treated with HNO3), the activity reaches the limit activity compatible with NaPtBronze.
[0238] e) Stability test
[0239] Fig.13 shows that at 0.5A cm -2 Comparison of the samples of the present invention with commercially available Ir black in a PEM electrolysis single cell according to the following process and conditions at a constant current of .
[0240] f) Single battery (25cm 2 ) in a catalyst coated membrane (CCM), such as the sample of the present invention described in WO 2018 / 110423 (about 3.8 mg / cm -2 ) and commercial Ir black CCM (2 mg cm -2 , Quintech) and PtBi bronze (about 3.9 mg / cm 2 )(See Fig.14 ) at 60°C. The inks of PtBi bronze or the samples of the present invention (5 g water, 0.1 g Nafion 5% lower alcohol solution, 40 mg catalyst) were sprayed onto a commercial Nafion 117 membrane and 1 mg / cm Pt The membrane was coated with Pt / C (Quintech GmbH) of 1,000 μm while the substrate on which the CCM was located was kept at 60° C., thereby preparing a catalyst-coated membrane. The uniformly dried catalyst-coated membrane was then processed by a calendar roll at 130° C.
[0241] g) After the activation process and after about 1 week of constant operation (see Figure 15), the polarization curve of the same CCM with the inventive sample anode shows that no discernible degradation has occurred in the inventive sample.
[0242] Attached photos
[0243] Figure 1 : Illustration of the preparation process of the present invention (a), comparative sample I (b) and comparative sample II (c).
[0244] Figure 2 : TEM image and elemental distribution of the inventive sample with a nominal Ru / Pt ratio of 0.33.
[0245] Figure 3 : TEM images and elemental distribution of a) Comparative Sample I and b) Comparative Sample II, both having a nominal Ru / Pt ratio of 0.33.
[0246] Figure 4 : Box plot representation and histogram of Ru-rich particles from TEM particle size analysis of the inventive sample and comparative sample I.
[0247] Figure 5 : Box plot representation and histogram of Pt-rich particles from TEM particle size analysis of the inventive sample and comparative sample I.
[0248] Figure 6 : Na1s( Figure 6 a) O1s( Figure 6 b) Pt4f( Figure 6 c) and Ru3d( Figure 6 d) XPS spectrum.
[0249] Figure 7 : Na1s( Figure 7 a) O1s( Figure 7 b) Pt4f( Figure 7 c) and Ru3d( Figure 7 d) XPS spectrum.
[0250] Figure 8 : Diffraction patterns of samples of the invention with varying ratios of Ru to Pt.
[0251] Fig. 9 : Comparison of the electrochemical activity of samples of the present invention against Pt bronze (as described by Kamitaka et al.) and IrO2.
[0252] Fig.10 : a) Electrochemical cycling of the samples of the present invention against b) Cyclic stability of RuO2.
[0253] Fig.11 : Electrochemical activity of the sample of the present invention compared with comparative sample I (H2-PEM-192-2) and comparative sample II (BRZ-33).
[0254] Fig.12 : Electrochemical activities of the samples of the present invention with varying Ru / Pt ratios.
[0255] Fig.13 : Comparative stability of sample I of the present invention and Ir black in a PEM electrolysis cell.
[0256] Fig.14 : Polarization curves of the samples of the present invention, PtBi bronze and Ir black.
[0257] Fig.15 : Polarization curves of the sample of the present invention shortly after starting operation and one week later.
Claims
1. A catalyst composition comprising a platinum and / or palladium (Pt / d) oxide and a transition metal (M) oxide, wherein M = Cr, Ir, Mn, Si, V, Re, Nb, Ti, Sn, Pb and / or Ru, the composition comprising at least two separate oxide phases: (i) a MO2 phase and (ii) a Mex(Pt / d)yO4 phase, wherein Me = M, Pt, Ca, Sr, Ba, Bi, Pd, Mn, Co, Cu, Ag, Ce, Mg, Zn, Cd, Co, Ni, Li, Na and / or K, and x = 0.1 to 0.9 and y = 2.7 to 3, wherein the particle size of the MO2 phase particles is in the range of 5 nm (d10) and 70 nm (d90), and the Mex(Pt / d)yO4 phase is in the range of 0.1 to 0.9 and 0.7 to 0.
8. x (Pt / d) y The particle size of the particles of the O4 phase is in the range of 5 nm (d10) and 80 nm (d90) both measured by TEM particle size analysis.
2. The catalyst composition according to claim 1, wherein the MO2 phase is a tetragonal phase and the Me x (Pt / d) y The O4 phase is a cubic phase.
3. The catalyst composition according to claim 1 or 2, wherein at the nanoscale, the (i) MO2 phase and (ii) Me x (Pt / d) y The O4 phase is unevenly distributed, and on a macroscopic scale, the (i) MO2 phase and (ii) Me x (Pt / d) y The O4 phase is evenly distributed.
4. The catalyst composition according to at least one of claims 1 to 3, wherein the ratio of M to (Pt / d) is between 0.04 and 5.
5. The catalyst composition according to at least one of claims 1 to 4, wherein the catalyst composition contains Ca, Sr, Ba, Bi, Mn, Co, Cu, Ag, Ce, Mg, Zn, Cd, Co, Ni, Li, Na and / or K in an amount in the range of 0.01 wt.% to 5 wt.% relative to the total mass of the Pt or Pd precursor.
6. The catalyst composition according to at least one of claims 1 to 4, wherein the catalyst composition contains Li, Na and / or K in the range of 0.01 wt.-% to 5 wt.-% relative to the total mass of the Pt or Pd precursor.
7. The catalyst composition according to claim 1, wherein Li, Na and / or K are x (Pt / d) y O4 is associated.
8. The catalyst composition according to at least one of claims 1 to 7, wherein Pt oxide and Ru oxide are present in the catalyst composition.
9. The catalyst composition according to at least one of claims 1 to 8, wherein the Mex-PtyO4 unit cell volume is and between.
10. The catalyst composition according to at least one of claims 1 to 9, wherein the catalyst composition contains 65 to 75 wt. % of platinum, 10 to 20 wt. % of ruthenium, 1 to 2 wt. % of sodium and the remainder up to 100 wt. % of oxygen, relative to the total mass of the catalyst.
11. The catalyst composition according to at least one of claims 1 to 10, wherein the catalyst composition shows a platinum peak having a binding energy of Pt 4f between 71 eV and 75 eV and a ruthenium peak having a binding energy of Ru 3d between 279 eV and 282 eV in an X-ray photoelectron spectroscopy (XPS) spectrum.
12. The catalyst composition according to at least one of claims 1 to 11, wherein the binding energy gap between O1s and Ru3d is between 248.40 eV and 248.60 eV.
13. The catalyst composition according to at least one of claims 1 to 12, wherein the particle size of the Pt phase characterized by TEM measurements is on average 10 nm to 60 nm, and the particle size of the Ru phase is on average 5 nm to 60 nm.
14. The catalyst composition according to claim 1 , wherein the platinum is present in an oxidation state +IV of 5 to 10 atom %, in an oxidation state +II (type I) of 10 to 20 atom %, in an oxidation state +II (type II) of 10 to 20 atom %, in an oxidation state (Pt(+δ)) of 55 to 60 atom %, and in an oxidation state 0 of 0 to 8 atom %, and the ruthenium is present in an oxidation state +IV of 80 to 100 atom %.
15. A method for producing a catalyst, the method comprising the steps of: (a) mixing a predetermined amount of platinum or palladium raw material with a transition metal (M), wherein M = Cr, Ir, Mn, Si, V, Re, Nb, Ti, Sn, Pb and / or Ru; (b) subjecting the raw material mixture to a solid phase reaction; and (c) removing by-products from the resulting reactant, wherein the transition metal (M) raw material is provided in the form of a liquid solution.
16. An electrochemical device comprising the catalyst composition according to one of claims 1 to 14.
17. Use of the catalyst composition according to one of claims 1 to 14 as catalyst for the oxygen evolution reaction.