Preparation technology of high-stability copper alloy for high-end electronic equipment
Through hot rolling, solid solution treatment, double-sided milling and other process flows, combined with the "1+2 milling method" and belt cleaning machine and other technologies, the mechanical properties and conductivity of copper alloys are optimized, and the existing solutions are solved The waste problems caused by intricate milling and edge cutting operations in the technology improve production efficiency and material performance.
Patent Information
- Application Number
- CN202411540846.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-stability copper alloys are not operated in milling surfaces, edge cutting and other processes, resulting in the production of waste materials, and the production efficiency and material performance need to be further improved.
Using hot rolling, opening, solid solution treatment, double-side milling, rough rolling, edge cutting, annealing, pickling, oil removal, finish rolling, bending and straightening, etc., combined with the "1+2 milling method" and horizontal shearing Cutting and resegmentation, belt cleaning machine and other technologies to optimize the mechanical properties and electrical conductivity of copper alloys.
It effectively solves the internal stress problems caused by temperature difference, improves the strength and conductivity of the material, reduces waste generation, and improves production efficiency and material performance.
Smart Images

Figure CN119035265A_ABST
Abstract
Description
Technical Field
[0001] The present invention mainly relates to the technical field of alloy processing, specifically a high-stability copper alloy preparation technology for high-end electronic equipment. Background Art
[0002] High-stability copper alloy is a commonly used material for high-end electronic equipment. Copper alloy has good electrical and thermal conductivity. Through the optimization of preparation technology, these properties can be further improved, making it more widely used in electrical, electronic, refrigeration and other fields. This material is made by copper alloy preparation technology through reasonable alloy design and preparation process, which can significantly improve the strength, hardness, toughness and other mechanical properties of copper alloy, and meet the requirements of various industrial applications for material performance. The existing high-stability copper alloy is made using a complete copper alloy preparation process.
[0003] According to the fatigue-resistant copper alloy material for electrical and electronic equipment and its preparation method provided by application number CN201310729114.5, it is composed of the following chemical components in mass percentage: Ni1.5-2.0, Co1.1-1.4, Cr0.8-1.2, Mg0.5-1, Zn0.4-0.8, Si0.3-0.6, Be0.2-0.4, V0.15-0.25, Ga0.1-0.2, Te0.04-0.08, Hf0.03-0.05, Pr0.02-0.03, Gd0.01-0.02, P≤0.03, S≤0.015, and the balance is copper. The copper alloy material of the invention has excellent comprehensive performance, high fatigue resistance, long service life, and excellent electrical conductivity, thermal conductivity, mechanical strength, stress relaxation resistance, corrosion resistance and other properties, and is widely used in electrical and electronic equipment.
[0004] The above patent document is suitable for industrial large-scale production and has huge economic benefits due to its simple process, convenient operation, high yield rate and low production cost. However, in the production process, especially in the processes such as milling, trimming and fine brushing, waste is often produced due to the lack of meticulous operation process.
[0005] Therefore, we proposed a high-stability copper alloy preparation technology for high-end electronic devices in order to solve the above-mentioned problems. Summary of the invention
[0006] Based on this, the purpose of the present invention is to provide a high-stability copper alloy preparation technology for high-end electronic devices to solve the technical problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions: A high-stability copper alloy preparation technology for high-end electronic equipment includes the following process flow: Hot rolling → solution treatment → double-sided milling → rough rolling → first trimming → bell furnace annealing → intermediate rolling → first pickling and degreasing → second trimming → first air cushion furnace annealing → brushing and grinding → finishing rolling → second pickling and degreasing → third trimming → finishing rolling to pre-finished product → second air cushion furnace annealing → brushing and grinding → pickling, rewinding and finishing rolling to finished product → third pickling and degreasing → bell furnace aging → bending and straightening → performance testing → finished product slitting.
[0008] Preferably, the hot rolling blanking process includes heating the titanium-copper alloy in a walking-beam heating furnace with a heating temperature of 900°C. The walking-beam heating furnace is provided with 16 zones, zones 1-2 are heated to 920°C, zones 3-10 are kept at 920°C, zones 11-16 are reduced and maintained at 900°C, and the furnace opening temperature drops sharply by 57°C. The hot rolling blanking process uses a reciprocating rolling mill, including 13 rolling passes with a rolling time of 10 minutes. The thickness of the titanium-copper alloy ingot is rolled from 130 mm to 11.2 mm, and the rolling force increases from 570 t in the first pass to 940 t in the final pass, and the rolling temperature decreases from the starting rolling temperature of 843°C to the final rolling temperature of 560°C.
[0009] Preferably, the solution treatment uses a box-type heating furnace to heat the hot-rolled raw material to 830-850°C and keep it warm for 2-4h, and the mechanical properties and corrosion resistance of the alloy are improved by solution treatment. The annealing temperature in the air cushion furnace is 830°C, and the heating zone of the air cushion furnace uses 4 groups of 8 1200kw heating fans arranged in parallel and obliquely, and the cooling zone uses 3 groups of 6 cooling fans arranged in parallel and obliquely. The air cushion furnace is provided with inlet and outlet loops to store materials, and there is a device for detecting surface defects at the winding position to detect white spots, white silk, black marks, holes, and cracked edges.
[0010] Preferably, the double-sided milling adopts the "1+2 milling method" of one straightening + two milling. When milling, the rotation direction of the milling cutter is opposite to the forward direction of the sheet. The milling time of a single coil is 40 minutes, the single-sided milling is 0.3mm, and the single-side milling is 1.5mm. The surface and edge oxide layers and segregation products are removed to reduce the transverse and longitudinal thickness differences of the sheet. The pits on the surface of the sheet that cannot be milled are polished smooth with an angle grinder. After the first and second milling, the coil is wound with liner paper to prevent the milled surface from contacting and affecting the surface quality. The liner paper is removed when the next rough rolling uncoil is unrolled.
[0011] Preferably, the rough rolling process uses a rough rolling mill to roll the material thickness from 9.5 mm to 2.5 mm. This process requires 11 rolling passes. If the incoming material is thicker, the rolling passes are increased accordingly, generally around 10-13 passes. The rolling speed is ≤25 m / min to prevent the speed from being too fast to adjust. The rolling force increases from 413 t in the first pass to 680 t in the final pass, and the front and rear tension is 43 KN.
[0012] Preferably, the first trimming process and the second trimming process are performed by a thick material trimming machine series, and the third trimming process is performed by a thin strip trimming machine series. The depth of the cracks on both sides of each coil is measured before trimming, and the cutters of the trimming machine series are replaced according to the depth. The cut edges are crushed into 10 cm pieces by a shredder, and then segmented by a cross-cutting shear during trimming. The remaining cracks are smoothed with an angle grinder to avoid the expansion of small cracks after rolling and causing strip breakage during subsequent rolling.
[0013] Preferably, the bell furnace annealing process is: heating to 680℃ for 6h, keeping warm for 8h, pure nitrogen atmosphere for oxidation protection, a tray is used to separate every two coils, the bell furnace is divided into an inner tank and an outer insulation cover, and a single furnace can hold six coils. The 2.5mm thick material that has been rough-rolled is annealed and softened after trimming to reduce its strength and hardness and improve its plasticity and toughness to facilitate further rolling.
[0014] Preferably, the pickling and degreasing process successively passes through an alkaline washing tank, a pickling tank, a cold water spray, a fine brushing room, a hot water spray, a passivation tank, a drying tank and a winding process. The main process adopts a sand belt cleaning machine with the function of cleaning + grinding in one go. The grinding roller in the fine brushing room is made of silicon carbide. The thick belt is first ground by a 180-mesh grinding brush and then by a 320-mesh grinding brush. When grinding thin belts, the mesh number of the grinding brush is 3200 mesh.
[0015] Preferably, the intermediate rolling, finishing rolling, pre-finished product rolling and finished product rolling processes are all carried out by a four-roll rolling mill. The intermediate rolling is rolled to 0.9mm, and the finishing rolling is rolled to 0.27mm. The rolling speed during intermediate rolling and finishing rolling is 80-260m / min, which increases as the thickness of the plate and strip decreases. The first pass of the intermediate rolling process of 2.5mm-0.9mm is minimized by tensioning to 29KN, and the front tension is increased to 31KN. The rolling speed is slowed down to ≤15m / min. There are thickness gauges before and after the rolling mill. The tolerance of finished product rolling is ±2.5μm, and the negative tolerance is +0 / -0.01mm.
[0016] Preferably, the aging treatment process adopts a bell furnace with a temperature of 400°C for 4.5 hours, a heat preservation for 8 hours, and a pure nitrogen atmosphere for oxidation protection. The stretching and straightening process uses a stretching and straightening machine to cause the thin plate to undergo longitudinal and transverse deformation at the same time, thereby fully improving the flatness and material properties of the thin plate. The stretching and straightening machine series uses a replaceable set roller box, and the diameter of the roller in the roller box that is in direct contact with the surface of the strip is d≈16 mm.
[0017] In summary, the present invention mainly has the following beneficial effects: 1. In this embodiment, by adopting the "1+2 milling method", compared with directly performing two milling operations, the problem of the temperature difference between the edge and the core during solution quenching, which generates internal stress and causes the core to bulge, that is, when straightened with the help of the inlet leveling roller system, the middle of the cross section of the rolled plate will be slightly arched after leveling, resulting in the two sides of the upper surface of some rolled plates not being milled is solved; when trimming, the cross-cutting and segmenting process is used to solve the problem of the side bending of the head and tail of the plate not controlling the reduction amount during cold rolling, resulting in excessive reduction on one side and the plate tilting to the other side. The angle grinder is used to grind it smooth to avoid the expansion of small cracks in the subsequent rolling process after rolling to cause strip breakage.
[0018] 2. By using the abrasive belt cleaning machine to replace the fine brushing chamber structure in cleaning, not only can the cleaning and grinding be integrated in the fine brushing process, but also when switching between fine brushing thick strips and thin strips, the cleaning + grinding can be completed in one go without changing the grinding roller, which saves the time of changing the grinding roller and improves production efficiency; in the first pass of the medium rolling 2.5mm-0.9mm process, the rear tension is reduced to 29KN, the front tension is increased to 31KN, and the rolling speed is slowed down to ≤15m / min, which eliminates the interlayer scratches of the coil. In the final stretching and straightening plus trimming and removal, the problem of tiny double-sided waves during rolling due to the very thin coil can be avoided.
[0019] 3. Annealing in a continuous online air cushion furnace makes the annealing temperature fluctuate less, the heating and cooling speeds are fast, and the production efficiency is greatly improved; it makes it easier to achieve the functions of reducing stress, improving crystal structure, improving mechanical properties, adjusting hardness, improving electrical properties and eliminating defects; by increasing the thickness of the head and tail during subsequent stitching, using manual spot welding instead of machine stitching, waiting for the stitched joint to pass through the air cushion furnace before increasing it to the given process tension, and marking the overheating section to observe the subsequent tape breakage, the problem of overheating of the strip in the heating furnace caused by the disconnection of the stitching interface can be effectively solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is the overall preparation process flow chart of the present invention; Figure 2 It is the hot rolling process parameter diagram of the present invention; Figure 3 It is a schematic diagram of the milling machine of the present invention; Figure 4 The rough rolling process parameter diagram of the present invention is Figure 5 The annealing process parameters of the air cushion furnace for strips of different sizes according to the present invention are shown; Figure 6 It is the process parameter diagram of the intermediate rolling of the present invention; Figure 7 This is a process parameter diagram for finishing rolling of a pre-finished product of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Please refer to the attached Figure 1-Figure 2 As shown, a high-stability copper alloy preparation technology for high-end electronic equipment includes the following process flow: Hot rolling → solution treatment → double-sided milling → rough rolling → first trimming → bell furnace annealing → intermediate rolling → first pickling and degreasing → second trimming → first air cushion furnace annealing → brushing and grinding → finishing rolling → second pickling and degreasing → third trimming → finishing rolling to pre-finished product → second air cushion furnace annealing → brushing and grinding → pickling, rewinding and finishing rolling to finished product → third pickling and degreasing → bell furnace aging → bending and straightening → performance testing → finished product slitting.
[0023] The hot rolling process includes heating the titanium-copper alloy in a walking-beam heating furnace with a heating temperature of 900°C. The walking-beam heating furnace is equipped with 16 zones, with zones 1-2 heated to 920°C, zones 3-10 kept at 920°C, and zones 11-16 reduced and maintained at 900°C. The furnace opening temperature drops by 57°C. The hot rolling process uses a reciprocating rolling mill, including 13 rolling passes with a rolling time of 10 minutes. The thickness of the titanium-copper alloy ingot is rolled from 130mm to 11.2mm, and the rolling force increases from 570t in the first pass to 940t in the final pass. The rolling temperature drops from the starting rolling temperature of 843°C to the final rolling temperature of 560°C.
[0024] It should be noted that hot rolling refers to a process in which the rectangular flat ingot billet after forging is heated in a heating furnace above the recrystallization temperature of the alloy and below the melting point, and then rolled through a rolling mill, from a billet thickness of 130mm to a rough rolling thickness of about 11mm. The billet is a drawn material after forging. The metal undergoes a large plastic deformation during the forging process, and the internal structure has been transformed from a cast structure to a forged structure, that is, the cast columnar grains have been broken into finer grains, and the plastic toughness and hardness have increased. The deformation amount during the hot rolling process is large, and most of the irregular fine grains of the billet are rolled and elongated into fibers consistent with the rolling direction. During hot rolling, the deformed metal has a hardening and softening process at the same time. Due to the fast deformation speed, the recovery and recrystallization processes are not carried out in time. The metal will produce a certain degree of work hardening as the degree of deformation increases. At the end of hot rolling, the recrystallization of the metal is often incomplete. The plate and strip after hot rolling presents a state of coexistence of recrystallization and deformation structure. After hot rolling is completed and coiled, the strength and hardness of the metal are increased to a certain extent.
[0025] Please refer to the attached Figure 3-Figure 4 As shown, the solution treatment uses a box-type heating furnace to heat the hot-rolled raw materials to 830-850℃ and keep them warm for 2-4h. The mechanical properties and corrosion resistance of the alloy are improved by solution treatment. The temperature of the air cushion furnace annealing is 830℃. The heating zone of the air cushion furnace uses 4 groups of 8 1200kw heating fans arranged in parallel and tilted. The cooling zone uses 3 groups of 6 cooling fans arranged in parallel and tilted. The air cushion furnace is equipped with inlet and outlet loopers to store materials. There is a device for detecting surface defects at the winding part to detect white spots and white silk. , black marks, holes, cracked edges; double-sided milling adopts the "1+2 milling method" of one straightening + two milling. When milling, the milling cutter rotates in the opposite direction of the sheet forward. The milling time for a single coil is 40 minutes, single-sided milling is 0.3mm, and single-side milling is 1.5mm. The surface and edge oxide layer and segregation products are removed to reduce the transverse and longitudinal thickness difference of the sheet. The pits on the sheet surface that cannot be milled are polished smooth with an angle grinder. After the first and second milling, the coil is rolled with liner paper. Coil up to prevent the surface after milling from contacting and affecting the surface quality. When the next rough rolling uncoil is unrolled, the lining paper is removed. The rough rolling process uses a rough rolling mill to roll the material thickness from 9.5mm to 2.5mm. This process requires 11 passes. If the incoming material is thicker, the rolling passes are increased accordingly, generally around 10-13 passes. The rolling speed is ≦25m / min to prevent the speed from being too fast and not being able to adjust in time. The rolling force increases from 413t in the first pass to the final pass. The material is 680t, with a front and rear tension of 43KN. The first and second trimming processes are performed by thick material trimming machine trains, and the third trimming process is performed by thin strip trimming machine trains. Before trimming, the crack depth on both sides of each coil is measured, and the cutter of the trimming machine train is replaced according to the depth. The cut edges are crushed into 10cm pieces by a shredder. When trimming, they are removed and segmented by a cross-cutting shear. The remaining cracks are smoothed with an angle grinder to avoid the expansion of small cracks after rolling and causing strip breakage during the subsequent rolling process.
[0026] It should be noted that if two milling operations are performed directly and straightening is performed only with the aid of the inlet leveling roller system, the middle of the cross section of the rolled plate will be slightly arched after leveling, resulting in the failure to mill both sides of the upper surface of some rolled plates. The reason is that the temperature of the edge and the core are inconsistent during solution quenching, and there is a temperature difference, which generates internal stress and causes the core to bulge. The "1+2 milling method", i.e. one straightening + two milling operations, has been adopted to improve the problem. The bending of the head and tail of the plate is because the reduction amount is not well controlled during cold rolling, resulting in excessive reduction on one side, and the metal hardness is extremely high, with almost no widening, so the metal basically flows longitudinally. Because the rolling speed is certain, once the reduction on one side is large, the plate will tilt toward the other side. This phenomenon generally occurs at the head or tail. When trimming, it can be removed by cross-cutting and then segmented. When the cracked edge is not cut cleanly, the reason for using an angle grinder to grind it smooth is to avoid the expansion of small cracked edges after rolling in the subsequent rolling process, causing broken strips.
[0027] Please refer to the attached Figure 5-Figure 7 As shown, the bell furnace annealing process is: 680℃ heating for 6h, insulation for 8h, pure nitrogen atmosphere for oxidation protection, a tray is used to separate every two coils, the bell furnace is divided into an inner tank and an outer insulation cover, and a single furnace can hold six coils. The 2.5mm thick material that has been rough-rolled is annealed and softened after trimming to reduce its strength and hardness, and improve its plasticity and toughness, so as to continue rolling; the pickling and oil removal process successively passes through the alkali washing tank, pickling tank, cold water spray, fine brushing room, hot water spray, passivation tank, drying tank and winding process. The main process uses a sand belt cleaning machine with the function of cleaning + grinding in one go. The grinding roller in the fine brushing room is made of silicon carbide. The thick strip is first ground by a 180-mesh grinding brush and then by a 320-mesh grinding brush. The mesh number of the grinding brush for thin strip grinding is 3200 mesh; the intermediate rolling, fine rolling, pre-finished product rolling and finished product rolling processes are all carried out by a four-roll mill. The intermediate rolling is rolled to 0.9mm, and the finishing rolling is rolled to 0.27mm. The rolling speed is 80-260m / min during the intermediate rolling and finishing rolling, and increases with the decreasing thickness of the plate and strip. The first pass of the intermediate rolling process of 2.5mm-0.9mm has a small tension of 29KN, and the front tension is increased to 31KN. The rolling speed is slowed down to ≤15m / min. There are thickness gauges before and after the rolling mill. The tolerance of the finished product rolling is ±2.5μm, and the negative tolerance is +0 / -0.01mm; the aging treatment process adopts a bell furnace with a temperature rise of 400℃ for 4.5h, insulation for 8h, and pure nitrogen atmosphere for oxidation prevention. The stretch bending straightening process uses a stretch bending straightening machine to make the thin plate produce longitudinal and transverse deformation at the same time, thereby fully improving the flatness and material properties of the thin plate. The stretch bending straightening machine adopts a replaceable set roller box, and the diameter of the roller in the roller box that directly contacts the strip surface is d≈16mm.
[0028] It should be noted that the main purpose of cleaning is to remove the lubricating oil remaining during rolling, mainly during intermediate rolling and finishing rolling. When the fine brush roller in the fine brush room is replaced with a grinding roller, the cleaning and grinding operation can be performed in one operation. The grinding roller material for thick strip and thin strip grinding is the same, both of which are made of silicon carbide, but the mesh count of the grinding roller is inconsistent. With the use of a sand belt cleaning machine, the cleaning and grinding can be completed in one go without replacing the grinding roller, which saves the time of replacing the grinding roller and improves production efficiency. In the first pass of the intermediate rolling process of 2.5mm-0.9mm, since the coil is annealed in a bell-type annealing furnace, The material is relatively loose after annealing. In order to solve the interlayer scratch phenomenon of the previous batch of coils, the tension after the first pass can be reduced to 29KN, the front tension can be increased to 31KN, and the rolling speed can be slowed down to ≤15m / min, which eliminates the interlayer scratch phenomenon of the coil. Subsequently, it is determined that the first pass of this rolling process is changed to the above process, which lays a good foundation for the surface quality of subsequent products. Since the coil is very thin at this time, it is almost always accompanied by tiny double-sided waves during rolling, which can be removed in the final stretch straightening and trimming.
[0029] Although an embodiment of the present invention has been shown and described, this specific embodiment is merely an explanation of the present invention and is not a limitation of the invention. The specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. After reading this specification, those skilled in the art may make modifications, substitutions and variations to the embodiments without creative contributions as needed without departing from the principles and purpose of the present invention. However, as long as they are within the scope of the claims of the present invention, they are protected by patent law.
Claims
1. A high-stability copper alloy preparation technology for high-end electronic equipment, characterized in that: The process includes the following: Hot rolling → solution treatment → double-sided milling → rough rolling → first trimming → bell furnace annealing → intermediate rolling → first pickling and degreasing → second trimming → first air cushion furnace annealing → first brushing → finishing rolling → second pickling and degreasing → third trimming → finishing rolling to pre-finished product → second air cushion furnace annealing → second brushing → pickling, rewinding and finishing rolling to finished product → third pickling and degreasing → bell furnace aging → bending and straightening → performance testing → finished product slitting.
2. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The hot rolling blanking process includes heating the titanium-copper alloy in a walking-beam heating furnace with a heating temperature of 900°C. The walking-beam heating furnace is provided with 16 zones, zones 1-2 are heated to 920°C, zones 3-10 are kept at 920°C, zones 11-16 are reduced and maintained at 900°C, and the furnace opening temperature drops by 57°C. The hot rolling blanking process uses a reciprocating rolling mill, including 13 rolling passes with a rolling time of 10 minutes. The thickness of the titanium-copper alloy ingot is rolled from 130 mm to 11.2 mm. The rolling force increases from 570 t in the first pass to 940 t in the final pass, and the rolling temperature decreases from the starting rolling temperature of 843°C to the final rolling temperature of 560°C.
3. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The solution treatment uses a box-type heating furnace to heat the hot-rolled raw materials to 830-850°C and keep them warm for 2-4 hours. The mechanical properties and corrosion resistance of the alloy are improved by solution treatment. The annealing temperature of the air cushion furnace is 830°C. The heating zone of the air cushion furnace uses 4 groups of 8 1200kw heating fans arranged in parallel and obliquely. The cooling zone uses 3 groups of 6 cooling fans arranged in parallel and obliquely. The air cushion furnace is equipped with inlet and outlet loops to store materials. There is a device for detecting surface defects at the winding position to detect white spots, white silk, black marks, holes, and cracked edges.
4. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The double-sided milling adopts the "1+2 milling method" of one straightening + two milling. When milling, the rotation direction of the milling cutter is opposite to the forward direction of the sheet. The milling time of a single coil is 40 minutes, the single-sided milling is 0.3mm, and the single-side milling is 1.5mm. The oxide layer and segregation products on the surface and edges are removed, and the transverse and longitudinal thickness differences of the sheet are reduced. The pits on the surface of the sheet that cannot be milled are polished smooth with an angle grinder. After the first and second milling, the coil is wound with liner paper to prevent the surface after milling from contacting and affecting the surface quality. The liner paper is removed when the next rough rolling uncoil is unrolled.
5. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The rough rolling process uses a rough rolling mill to roll the material thickness from 9.5mm to 2.5mm. This process requires 11 rolling passes. If the incoming material is thicker, the rolling passes are increased accordingly, generally around 10-13 passes. The rolling speed is ≤25m / min to prevent the speed from being too fast to adjust in time. The rolling force increases from 413t in the first pass to 680t in the final pass, and the front and rear tension is 43KN.
6. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The first trimming process and the second trimming process are performed by a thick material trimming machine series, and the third trimming process is performed by a thin strip trimming machine series. Before trimming, the crack depths on both sides of each coil are measured, and the cutters of the trimming machine series are replaced according to the depths. The cut edges are crushed into 10 cm pieces by a crushing machine, and are then cut and segmented using a cross-cutting shear during trimming. The remaining cracks are smoothed using an angle grinder to avoid the expansion of small cracks after rolling during subsequent rolling and causing strip breakage.
7. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The bell furnace annealing process is: heating to 680℃ for 6h, keeping warm for 8h, pure nitrogen atmosphere for oxidation protection, a tray is used to separate every two coils, the bell furnace is divided into an inner tank and an outer insulation cover, and a single furnace can hold six coils. The 2.5mm thick material that has been rough-rolled is annealed and softened after trimming to reduce its strength and hardness and improve its plasticity and toughness to facilitate further rolling.
8. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The pickling and degreasing process successively passes through an alkaline washing tank, a pickling tank, a cold water spray, a fine brushing room, a hot water spray, a passivation tank, a drying tank and a winding process. The main process adopts a sand belt cleaning machine with the function of cleaning and grinding in one go. The grinding roller in the fine brushing room is made of silicon carbide. The thick belt is first ground by a 180-mesh grinding brush and then by a 320-mesh grinding brush. When grinding thin belts, the mesh number of the grinding brush is 3200 mesh.
9. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The intermediate rolling, finishing rolling, pre-finished product rolling and finished product rolling processes are all carried out by a four-roll rolling mill. The intermediate rolling is rolled to 0.9mm, and the finishing rolling is rolled to 0.27mm. The rolling speed during the intermediate rolling and finishing rolling is 80-260m / min, which increases as the thickness of the plate and strip decreases. The first pass of the intermediate rolling 2.5mm-0.9mm process has a minimum rear tension of 29KN, and the front tension is increased to 31KN. The rolling speed is slowed down to ≤15m / min. There are thickness gauges before and after the rolling mill. The tolerance of the finished product rolling is ±2.5μm, and the negative tolerance is +0 / -0.01mm.
10. The high-stability copper alloy preparation technology for high-end electronic equipment according to claim 1 is characterized in that: The aging treatment process adopts a bell furnace with a temperature of 400°C for 4.5 hours, a heat preservation for 8 hours, and a pure nitrogen atmosphere for oxidation protection. The stretching and straightening process uses a stretching and straightening machine to make the thin plate produce longitudinal and transverse deformation at the same time, thereby fully improving the flatness and material properties of the thin plate. The stretching and straightening machine series adopts a replaceable set roller box, and the diameter of the roller in the roller box that directly contacts the surface of the strip is d≈16mm.
Citation Information
Patent Citations
Small-size LED copper strip production process
CN108155281A
Copper alloy strip with high intensity, high conductivity and high bending performance and preparation method thereof
CN108998695A
Tin brass band production process
CN109127762A
Lug copper material production technology
CN109304371A
Copper strip rolling production process flow
CN113083891A