Manufacturing method and system of high-elasticity metal sealing ring

By using nickel-beryllium alloy materials and liquid forming technology, combined with solution treatment and aging heat treatment, the manufacturing challenges of highly elastic metal sealing rings have been solved, ensuring that the sealing rings do not leak at different temperatures, thus improving the product's performance and lifespan.

CN119035294APending Publication Date: 2024-11-29JINCHENG NANJING ELECTROMECHANICAL HYDRAULIC PRESSURE ENG RES CENT AVIATION IND OF CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411112243.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing technologies make it difficult to effectively manufacture highly elastic metal sealing rings, especially thin-walled metal sealing rings with a C-shaped cross-section, which makes them prone to leakage in high and low temperature environments.

Method used

By using nickel-beryllium alloy as raw material, and combining solution treatment and liquid forming with appropriate aging heat treatment and metallographic structure testing, the problem of the difficult removal of the punch of the C-shaped ring is solved, ensuring that the sealing ring has good elastic properties.

Benefits of technology

The fabrication of a highly elastic metal sealing ring has been achieved, ensuring no leakage under different ambient temperatures and improving product quality and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035294A_ABST
    Figure CN119035294A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method and system of a high-elasticity metal sealing ring. The method comprises the steps that 1, solution treatment is conducted on a nickel beryllium alloy strip; 2, a circular-tube-shaped blank piece is machined; 3, the circular-tube-shaped blank piece is cut into a cylindrical blank piece; 4, the cylindrical blank is subjected to solution treatment; 5, the cylindrical blank is placed in a hydraulic forming die; 6, the hydraulic forming equipment is started, high-pressure hydraulic oil is introduced into the hydraulic forming die, and pressure maintaining is conducted; 7, the hydraulic forming equipment is closed, high-pressure hydraulic oil is discharged, the hydraulic forming die is detached, and the formed metal sealing ring blank is taken out; 8, aging treatment is conducted on the metal sealing ring blank; step 9, performing metallographic structure inspection and evaluation on the metal sealing ring blank; 10, double-sided grinding is conducted on the metal sealing ring blank; and 11, silver plating surface treatment is conducted on the metal sealing ring obtained after double-face grinding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of complex forming and manufacturing of metal materials, and in particular to a manufacturing method and system for a high-elasticity metal sealing ring. Background Art

[0002] The metal sealing ring is a sealing element on the electro-hydraulic servo valve. It is required to have high elasticity, high strength limit, high fatigue limit, and be able to maintain good elasticity in both high and low temperature environments to prevent the high-pressure hydraulic oil inside the servo valve from leaking. Therefore, it is necessary to invent a highly elastic metal sealing ring to meet this requirement. See the assembly diagram of the metal sealing ring in the product. Figure 1 This metal sealing ring has a thin wall, about 0.2mm thick, and a C-shaped cross section. Figure 2 As shown. Since the metal sealing ring has the characteristics of thin wall, C-shaped cross section, and high material elasticity. And the metal sealing ring is a circular thin-walled part with a C-shaped cross section, it is difficult to realize it using traditional concave and convex dies. This is mainly because this structure cannot realize the extrusion of the punch and the removal of the punch from the C-shaped structure (the C-shaped outlet size is smaller than its internal maximum size). Therefore, the manufacturing method of the metal sealing ring has certain difficulties in terms of material selection, forming method, mold design, heat treatment process, metallographic structure detection, etc. It is urgent to invent a manufacturing method and system for highly elastic metal sealing rings to solve it. Summary of the invention

[0003] The purpose of the present invention is to solve the problems of thin wall, C-shaped cross section and high elasticity requirements of metal sealing rings, and use nickel-beryllium alloy as its raw material. Taking advantage of its good plasticity after solution treatment, it is plastically formed, and a unique liquid forming scheme is used to solve the problem that the punch of the C-shaped ring is not easy to remove. In addition, with appropriate aging heat treatment and metallographic structure detection and control scheme, it has good elastic properties. The present invention provides a manufacturing method and system for a highly elastic metal sealing ring to achieve the preparation of a highly elastic metal sealing ring. The principle is that the elongation of the nickel-beryllium alloy material after solution treatment is greater than 30%, and it has good plastic forming ability. The problem of difficult C-shaped ring forming can be solved through a reasonable forming scheme; after a suitable aging treatment process, the yield strength is greater than 1400MPa, so that the metal sealing ring has good elastic properties, ensuring its sealing during operation and solving the problem of easy oil leakage.

[0004] The technical solution is as follows:

[0005] A method for manufacturing a high-elasticity metal sealing ring, the method comprising the following steps:

[0006] Step 1: performing solid solution treatment on the nickel-beryllium alloy strip;

[0007] Step 2: Processing the nickel-beryllium alloy strip after solid solution treatment into a round tube blank by deep drawing;

[0008] Step 3: Cut the round tube blank into cylindrical blanks of a certain size;

[0009] Step 4: The cut cylindrical blank is subjected to solution treatment again;

[0010] Step 5: Place the cylindrical blank after solution treatment in step 4 in a hydroforming die;

[0011] Step 6: Turn on the hydraulic forming equipment, introduce high-pressure hydraulic oil into the hydraulic forming die, and maintain the pressure;

[0012] Step 7: Turn off the hydraulic forming equipment, release the high-pressure hydraulic oil, disassemble the hydraulic forming die, and take out the formed metal sealing ring blank;

[0013] Step 8: Perform aging treatment on the formed metal sealing ring blank;

[0014] Step 9: Conduct metallographic inspection and evaluation on the metal sealing ring blank after aging treatment to ensure that it has a good microstructure and good elastic properties;

[0015] Step 10: Double-sided grinding is performed on the metal sealing ring blank that has passed the metallographic structure inspection to ensure that the parallelism of the two end surfaces meets the requirements;

[0016] Step 11: Perform silver plating on the double-sided ground metal sealing ring to complete the manufacture of the metal sealing ring.

[0017] Furthermore, in step 1, a nickel-beryllium alloy strip is used as the material of the high-elasticity metal sealing ring.

[0018] Furthermore, in step 1, the solution treatment process is a solution temperature of 1050° C., heat preservation for 0.5 hours, and water cooling.

[0019] Furthermore, in step 4, the solution temperature is 1050° C., the temperature is maintained for 0.5 hours, and the solution is water-cooled.

[0020] Furthermore, in step 6, the pressure holding time is 3 to 5 minutes.

[0021] Furthermore, in step 8, the aging treatment process is an aging temperature of 490° C., keeping warm for 1.5 hours, and air cooling.

[0022] Furthermore, in step 10, the parallelism of the two end surfaces reaches 15 μm.

[0023] Furthermore, in step 11, the thickness of the silver plating layer is 20 μm.

[0024] A manufacturing system for a high-elasticity metal sealing ring, used in the method described, the system comprising: a hydraulic forming die, a hydraulic forming device,

[0025] The hydraulic forming die is used for forming highly elastic metal sealing rings;

[0026] The hydraulic forming die comprises two symmetrical forming units, the two forming units are connected, a cavity for placing a cylindrical blank is formed inside the two forming units, forming cavities with the same outer dimensions as the metal sealing ring are arranged on the opposite surfaces of the two forming units, an upper pressing plate and a lower pressing plate are arranged at the upper and lower ends of the two forming units respectively, and an oil delivery pipe nozzle is arranged on the upper pressing plate;

[0027] The hydraulic forming equipment is used to connect the hydraulic forming mold during the forming process of the high-elastic metal sealing ring, and then continuously input high-pressure hydraulic oil into the hydraulic forming mold, and then continuously maintain the pressure, so that the cylindrical blank after solid solution treatment undergoes plastic deformation in the mold to complete the forming of the high-elastic metal sealing ring.

[0028] Furthermore, the hydraulic forming mold is provided with mounting pins, mounting holes and positioning keyways, and the two forming units are connected by the mounting pins and mounting holes, and the positioning keyways are used to realize the positioning, assembly and disassembly between the two forming units and the upper pressing plate and the lower pressing plate.

[0029] Beneficial effects of the present invention:

[0030] Through the present invention, a nickel-beryllium alloy material with good cold processing plasticity and excellent elastic performance is adopted; the designed oil pressure forming scheme is applied to solve the problem that the punch of the C-shaped circular ring is difficult to remove; the metallographic structure detection method is used to control the beryllium-rich phase dissolution effect in the heat treatment aging treatment process of the metal sealing ring, so that it has better elastic performance; the manufacturing method and system of the whole set of high-elasticity metal sealing rings can ensure the successful preparation and processing of such thin-walled C-shaped circular metal sealing rings, and have higher elastic mechanical properties, solve the problem that sometimes the high-pressure hydraulic oil inside the servo valve will leak at different ambient temperatures, and improve the quality and service life of the entire product. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the metal sealing ring assembly.

[0032] Figure 2 It is a schematic diagram of the shape of the metal sealing ring.

[0033] Figure 3 It is a schematic diagram of a cylindrical blank.

[0034] Figure 4 It is a schematic diagram of the hydraulic forming die.

[0035] Figure 5 It is a schematic diagram of the hydroforming assembly.

[0036] Figure 6 This is the metallographic structure of the metal sealing ring after aging treatment at 100 times.

[0037] Figure 7 This is the metallographic structure of the metal sealing ring after aging treatment at 500 times. DETAILED DESCRIPTION

[0038] The metal sealing ring is a sealing element on the electro-hydraulic servo valve. It is required to have high elasticity, high strength limit, high fatigue limit, and be able to maintain good elastic properties in both high and low temperature environments, so as to achieve the purpose of preventing the high-pressure hydraulic oil inside the servo valve from leaking. Therefore, it is necessary to invent a highly elastic metal sealing ring to meet its requirements. This metal sealing ring has a thin wall, a wall thickness of about 0.2mm, and a C-shaped cross section. Because the metal sealing ring has the characteristics of thin wall, C-shaped cross section, and high material elasticity. Therefore, the manufacturing method of the metal sealing ring has certain difficulties in terms of material selection, forming method, mold design, heat treatment process, metallographic structure detection, etc. The nickel-beryllium alloy material selected by the present invention is used as the high-elasticity metal sealing ring material, and its elongation after solution treatment is greater than 30%, and its yield strength after aging treatment is greater than 1400MPa. It has good cold processing plasticity and excellent elastic properties. The designed oil pressure forming scheme can solve the problem that the punch of the C-shaped circular ring is not easy to remove. The metallographic structure detection method can control the beryllium-rich phase dissolution effect of the metal sealing ring during the aging treatment process, so that it has better elastic properties. The whole set of high-elasticity metal sealing ring manufacturing method and system can ensure the successful preparation and processing of this thin-walled C-shaped circular metal sealing ring, and has high elastic mechanical properties, solving the problem of high-pressure hydraulic oil leakage inside the servo valve at different ambient temperatures.

[0039] By using nickel-beryllium alloy material with good cold processing plasticity and excellent elastic properties, and taking advantage of its excellent plastic deformation characteristics after solution treatment, it is deep drawn from a thin strip with a thickness of about 30um into a cylindrical blank with a wall thickness of about 20um, such as Figure 3 The cylindrical blank is subjected to solution treatment again to restore its plastic deformation ability. Then it is formed using hydraulic forming dies and equipment to solve the problem that the punch of the C-shaped ring is difficult to remove. Figure 4-5 . The formed metal sealing ring blank is then subjected to aging heat treatment and metallographic structure inspection. Figure 6-7, ensuring that it has high elastic mechanical properties. Finally, the two end faces of the metal sealing ring are double-sided ground and silver-plated. In the specific operation process, it is necessary to apply appropriate solution treatment process, aging treatment process, control of metallographic structure morphology, control of the parallelism of the two end faces and the thickness of the silver plating layer to assist in completing the entire manufacturing process of the high elastic metal sealing ring.

[0040] One embodiment of the present invention is a method for manufacturing a high-elasticity metal sealing ring, the method comprising the following steps:

[0041] Step 1: Solution treatment of the nickel-beryllium alloy strip; using the nickel-beryllium alloy strip as the material of the high elastic metal sealing ring, the solution treatment process is solution temperature 1050° C., heat preservation for 0.5 hours, and water cooling.

[0042] Step 2: Processing the nickel-beryllium alloy strip after solid solution treatment into a round tube blank by deep drawing;

[0043] Step 3: Cut the round tube blank into cylindrical blanks of a certain size;

[0044] Step 4: subject the cut cylindrical blank to solution treatment again; the solution temperature is 1050°C, kept warm for 0.5 hours, and water cooled.

[0045] Step 5: Place the cylindrical blank after solution treatment in step 4 in a hydroforming die;

[0046] Step 6: Turn on the hydraulic forming equipment, introduce high-pressure hydraulic oil into the hydraulic forming mold, and maintain the pressure for 3 to 5 minutes;

[0047] Step 7: Turn off the hydraulic forming equipment, release the high-pressure hydraulic oil, disassemble the hydraulic forming die, and take out the formed metal sealing ring blank;

[0048] Step 8: Perform aging treatment on the formed metal sealing ring blank; the aging treatment process is aging temperature 490°C, heat preservation for 1.5 hours, and air cooling;

[0049] Step 9: Conduct metallographic inspection and evaluation on the metal sealing ring blank after aging treatment to ensure that it has a good microstructure and good elastic properties;

[0050] Step 10: Double-sided grinding is performed on the metal sealing ring blank that has passed the metallographic structure inspection to ensure that the parallelism of the two end surfaces reaches 15 μm;

[0051] Step 11: The double-sided ground metal sealing ring is subjected to a silver-plated surface treatment, the thickness of the silver-plated layer is 20 μm, and the manufacture of the metal sealing ring is completed.

[0052] The second embodiment of the present invention is a manufacturing system for a high elastic metal sealing ring, which is used in the method described above. The system includes: a hydraulic forming die, a hydraulic forming device,

[0053] The hydraulic forming die is used for forming highly elastic metal sealing rings;

[0054] The hydraulic forming die comprises two symmetrical forming units, the two forming units are connected, a cavity for placing a cylindrical blank is formed inside the two forming units, forming cavities with the same outer dimensions as the metal sealing ring are arranged on the opposite surfaces of the two forming units, an upper pressing plate and a lower pressing plate are arranged at the upper and lower ends of the two forming units respectively, and an oil delivery pipe nozzle is arranged on the upper pressing plate;

[0055] The hydraulic forming equipment is used to connect the hydraulic forming mold during the forming process of the high-elastic metal sealing ring, and then continuously input high-pressure hydraulic oil into the hydraulic forming mold, and then continuously maintain the pressure, so that the cylindrical blank after solid solution treatment undergoes plastic deformation in the mold to complete the forming of the high-elastic metal sealing ring.

[0056] Furthermore, the hydraulic forming mold is provided with mounting pins, mounting holes and positioning keyways, and the two forming units are connected by the mounting pins and mounting holes, and the positioning keyways are used to realize the positioning, assembly and disassembly between the two forming units and the upper pressing plate and the lower pressing plate.

[0057] The third embodiment of the present invention provides a method for manufacturing a highly elastic metal sealing ring, and the specific operation process is as follows:

[0058] Step 1: Solution treatment of the nickel-beryllium alloy strip at a solution temperature of 1050°C, heat preservation for 0.5 hours, and water cooling;

[0059] Step 2: Processing the nickel-beryllium alloy strip after solid solution treatment into a round tube shape by deep drawing;

[0060] Step 3: Cut the processed circular tubular blank into cylindrical blanks of a certain size;

[0061] Step 4: The cut cylindrical blank is subjected to solution treatment again, with the solution temperature at 1050°C, kept at this temperature for 0.5 hours, and then water-cooled;

[0062] Step 5: Place the cylindrical blank after solution treatment in the designed hydroforming die;

[0063] Step 6: Turn on the hydraulic forming equipment switch, introduce high-pressure hydraulic oil into the forming mold, and maintain the pressure;

[0064] Step 7: Turn off the hydraulic forming equipment switch, release the hydraulic oil, disassemble the forming die, and take out the formed metal sealing ring blank;

[0065] Step 8: Perform aging treatment on the formed metal sealing ring blank, aging temperature: 490°C, keep warm for 1.5 hours, and air cool;

[0066] Step 9: Conduct metallographic inspection and evaluation on the metal sealing ring blank after aging treatment to ensure that it has a good microstructure and good elastic properties.

[0067] Step 10: Double-sided grinding is performed on the metal sealing ring blank that has passed the metallographic structure inspection to ensure that the parallelism of the two end surfaces meets the requirements;

[0068] Step 11: The double-sided ground metal sealing ring is subjected to silver plating surface treatment, and the thickness of the silver plating layer reaches about 20um, completing the entire manufacturing process of the metal sealing ring.

[0069] The manufacturing method and system of the high-elasticity metal sealing ring of the present invention have been successfully applied in products and have also been promoted in some new products. The nickel-beryllium alloy material selected for the high-elasticity metal sealing ring has an elongation of more than 30% after solution treatment and a yield strength of more than 1400MPa after aging treatment. It has good cold processing plasticity and excellent elastic properties. The designed hydraulic forming scheme can solve the problem that the punch of the C-shaped circular ring is not easy to remove. The metallographic structure detection method can control the beryllium-rich phase dissolution effect of the metal sealing ring during the heat treatment and aging treatment process, so that it has better elastic properties. The whole set of high-elasticity metal sealing ring manufacturing method and system can ensure the successful preparation and processing of this thin-walled C-shaped circular metal sealing ring, and has high elastic mechanical properties, so as to achieve the purpose that it will not leak even if there is high-pressure hydraulic oil inside the servo valve at different ambient temperatures.

[0070] Application scenario 1: A certain electro-hydraulic servo valve uses a high-elasticity metal sealing ring processed by the manufacturing method of the present invention, which solves the problem that the high-pressure hydraulic oil inside the servo valve is prone to leakage under different ambient temperatures, leading to its early failure.

[0071] Application scenario two: A certain inclined plate control attachment uses a high-elasticity metal sealing ring processed by the manufacturing method of the present invention, which solves the problem that the high-pressure hydraulic oil inside it is prone to leakage, leading to its early failure.

[0072] The embodiment of the present invention further provides a system for manufacturing a high elastic metal sealing ring, which is used in the method described in the method embodiment of the present invention. The system comprises: a hydraulic forming die, a hydraulic forming device,

[0073] The hydroforming die is used for forming highly elastic metal sealing rings.

[0074] The hydraulic forming equipment is used to connect the hydraulic forming die during the forming process of the high elastic metal sealing ring, and then input high-pressure hydraulic oil into the hydraulic forming die, and then continuously maintain the pressure to make the cylindrical blank after the solid solution treatment undergo plastic deformation in the die to complete the forming of the high elastic metal sealing ring.

Claims

1. A method for manufacturing a highly elastic metal sealing ring, characterized in that: The method comprises the following steps: Step 1: performing solid solution treatment on the nickel-beryllium alloy strip; Step 2: Processing the nickel-beryllium alloy strip after solid solution treatment into a round tube blank by deep drawing; Step 3: Cut the round tube blank into cylindrical blanks of a certain size; Step 4: The cut cylindrical blank is subjected to solution treatment again; Step 5: Place the cylindrical blank after solution treatment in step 4 in a hydroforming die; Step 6: Turn on the hydraulic forming equipment, introduce high-pressure hydraulic oil into the hydraulic forming die, and maintain the pressure; Step 7: Turn off the hydraulic forming equipment, release the high-pressure hydraulic oil, disassemble the hydraulic forming die, and take out the formed metal sealing ring blank; Step 8: Perform aging treatment on the formed metal sealing ring blank; Step 9: Conduct metallographic inspection and evaluation on the metal sealing ring blank after aging treatment; Step 10: Double-sided grinding of the metal sealing ring blank that has passed the metallographic structure inspection; Step 11: Perform silver plating on the double-sided ground metal sealing ring to complete the manufacture of the metal sealing ring.

2. The method according to claim 1, characterized in that: In step 1, a nickel-beryllium alloy strip is used as the material of the high-elasticity metal sealing ring.

3. The method according to claim 1, characterized in that: In step 1, the solution treatment process is a solution temperature of 1050° C., holding for 0.5 hours, and water cooling.

4. The method according to claim 1, characterized in that: In step 4, the solution temperature is 1050°C, the temperature is kept for 0.5 hours, and the mixture is water-cooled.

5. The method according to claim 1, characterized in that: In step 6, the pressure holding time is 3 to 5 minutes.

6. The method according to claim 1, characterized in that: In step 8, the aging treatment process is aging temperature 490° C., heat preservation for 1.5 hours, and air cooling.

7. The method according to claim 1, characterized in that: In step 10, the parallelism of the two end surfaces reaches 15 μm.

8. The method according to claim 1, characterized in that: In step 11, the thickness of the silver plating layer is 20 μm.

9. A manufacturing system for a highly elastic metal sealing ring, characterized in that: The method used in any one of claims 1 to 8, wherein the system comprises: a hydraulic forming die, a hydraulic forming device, The hydraulic forming die is used for forming highly elastic metal sealing rings; The hydraulic forming die comprises two symmetrical forming units, the two forming units are connected, a cavity for placing a cylindrical blank is formed inside the two forming units, forming cavities with the same outer dimensions as the metal sealing ring are arranged on the opposite surfaces of the two forming units, an upper pressing plate and a lower pressing plate are arranged at the upper and lower ends of the two forming units respectively, and an oil delivery pipe nozzle is arranged on the upper pressing plate; The hydraulic forming equipment is used to connect the hydraulic forming mold during the forming process of the high-elastic metal sealing ring, and then continuously input high-pressure hydraulic oil into the hydraulic forming mold, and then continuously maintain the pressure, so that the cylindrical blank after solid solution treatment undergoes plastic deformation in the mold to complete the forming of the high-elastic metal sealing ring.

10. The system according to claim 9, characterized in that: The hydraulic forming mold is provided with mounting pins, mounting holes and positioning keyways, the two forming units are connected by the mounting pins and mounting holes, and the positioning keyways are used to realize the positioning, assembly and disassembly between the two forming units and the upper pressing plate and the lower pressing plate.

Citation Information

Patent Citations

  • Hydroforming method for manufacturing multilayer metal sealing gasket

    CN110587233A

  • Method for preparing high-elasticity high-temperature alloy sealing ring and sealing ring

    CN115870706A

  • Sealing ring material and preparation method thereof

    CN117488135A