Preparation method of heat dissipation plate

By adding copper metal particles and performing ultrasonic stirring and laser blistering during the preparation process of copper-aluminum composite heat dissipation plate, the problem of unevenness of interface combination intensity and heat conduction performance in the prior art is solved, and a higher interface is achieved Combining strength and thermal conductivity reduces the generation of air holes and shrinkage holes, and improves the overall performance of the heat dissipation plate.

CN119035510AActive Publication Date: 2024-11-29GUANGZHOU ZHONGSHAN FASTENER CO LTD

Patent Information

Application Number
CN202411551883.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-11-29
Estimated Expiration
2044-11-01

AI Technical Summary

Technical Problem

There is unevenness in the interface bonding strength and heat conduction performance of existing copper-aluminum composite heat dissipation plates, resulting in low thermal conductivity and interface bonding strength. The adjustment of solid phase fraction cannot reduce the generation of pores and shrinkage pores at the same time, resulting in large batch differences.

Method used

By roughening the surface of the copper plate, 0.3-0.5% of copper metal particles with an average particle size of 5-10 μm were added to the semi-solid aluminum alloy paste, and prepared by ultrasonic stirring to form 15-35% solid The phase fraction semi-solid aluminum alloy paste is cast on the surface of the copper plate for die-casting, and combined with laser blistering and appropriate die-casting parameters to form a tight interface bonding layer.

Benefits of technology

The interface bonding strength and thermal conductivity of the copper-aluminum composite heat dissipation plate are improved, the generation of pores and shrinkage holes is reduced, the interface bonding force is enhanced, batch differences are reduced, and the overall performance of the heat dissipation plate is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035510A_ABST
    Figure CN119035510A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a heat dissipation plate, which comprises the following steps: roughening at least one surface of a copper plate to obtain a roughened surface, preheating the copper plate in a mold, heating an aluminum alloy to obtain an aluminum alloy melt of which the temperature is 10-20 DEG C above a liquidus, and metal particles with the mass fraction being 0.3-0.5% and the average particle size being 5-10 microns are added into the aluminum alloy melt, the aluminum alloy melt is prepared into semi-solid aluminum alloy slurry with the solid phase fraction being 15-35%, the metal particles comprise copper, the semi-solid aluminum alloy slurry is poured on the roughened face to form an aluminum layer, and the heat dissipation plate is obtained through die casting. The metal particles are deposited at the bottom of the slurry in the casting process, the average particle size of the metal particles is smaller than the grain average particle size of the solid aluminum metal particles, the metal particles can replace a part of a liquid phase to be filled in gaps between the rough surface and the solid aluminum metal particles, gaps generated by contraction after the liquid phase is cooled are reduced, a tighter interface bonding layer is formed, and the service life of the interface bonding layer is prolonged. The interface bonding strength and the heat conductivity coefficient are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal composite material manufacturing, and in particular to a method for preparing a heat dissipation plate. Background Art

[0002] The copper-aluminum composite heat sink combines the advantages of copper and aluminum, such as the electrical conductivity and heat transfer performance of copper and the light weight and corrosion resistance of aluminum, and helps to further reduce the cost of the heat sink. However, due to the large differences between copper and aluminum, the low mutual solubility, the poor interface bonding consistency of the copper-aluminum composite heat sink formed by welding and other methods, the uneven distribution of heat conduction and resistance, and the large differences in physical properties between copper and aluminum will affect the performance of the copper-aluminum composite heat sink.

[0003] The applicant disclosed a copper-aluminum composite metal plate and a casting method and its application in a radiator in CN118180357A. A composite metal plate with high interface bonding force and thermal conductivity is obtained by pouring semi-solid aluminum on the surface of copper after surface roughening treatment and then ultrasonically obtaining a composite metal plate. However, the solid phase fraction during semi-solid aluminum pouring has an important influence on the interface bonding strength, interface thermal resistance and interface microstructure of the copper-aluminum composite metal plate. The influence of the solid phase fraction on the interface bonding strength is manifested as follows: when the solid phase fraction in the semi-solid aluminum paste is low, the liquid phase in the aluminum paste accounts for a large proportion and has good fluidity, but it may cause the mechanical locking effect at the copper-aluminum interface to weaken, thereby reducing the interface bonding strength; as the solid phase fraction increases, the solid phase particles in the aluminum paste increase, and these particles form a tighter physical connection at the copper-aluminum interface, enhancing the interface bonding strength; but too high a solid phase fraction may cause the aluminum paste to have a decreased fluidity, which is not conducive to the uniform distribution of aluminum liquid in the copper plate, thereby affecting the interface bonding quality. The effect of solid phase fraction on interfacial thermal resistance is as follows: the change of solid phase fraction will affect the thermal conductivity of the copper-aluminum interface. A lower solid phase fraction may lead to more pores and defects at the interface, increasing thermal resistance. As the solid phase fraction increases, the pores and defects at the interface decrease, and the heat conduction path becomes smoother, thereby reducing the interfacial thermal resistance. The effect of solid phase fraction on the interface microstructure is as follows: at low solid phase fractions, a thinner reaction layer or intermetallic compound layer may form at the interface. As the solid phase fraction increases, the interface reaction is more complete, and the type and amount of intermetallic compounds will change, affecting the microstructure and performance of the interface. Therefore, the interface bonding strength and interfacial thermal resistance cannot be further improved by simply adjusting the solid phase content.

[0004] Therefore, it is necessary to provide a method for preparing a heat dissipation plate. Summary of the invention

[0005] In order to further improve the interface bonding strength and interface of the copper-aluminum composite heat sink, it is necessary to provide a method for preparing the heat sink.

[0006] The present invention provides a method for preparing a heat dissipation plate, comprising the following steps: At least one surface of a copper plate is roughened to obtain a roughened surface, the copper plate is placed in a mold for preheating, an aluminum alloy is heated to obtain an aluminum alloy melt having a temperature of 10-20°C above the liquidus, 0.3-0.5% by mass of metal particles having an average particle size of 5-10 μm are added to the aluminum alloy melt, the aluminum alloy melt is prepared into a semi-solid aluminum alloy slurry having a solid phase fraction of 15-35%, the metal particles containing copper, the semi-solid aluminum alloy slurry is poured on the roughened surface to form an aluminum layer, and the heat sink is obtained by die casting.

[0007] Beneficial effects of the present invention: When an aluminum composite layer is formed on the surface of a copper layer by semi-solid die-casting according to existing technology, if a semi-solid aluminum alloy slurry with a high solid phase fraction is used, the slurry may not be able to fully fill the mold due to poor fluidity, and pores may easily be generated in some areas. If a semi-solid aluminum alloy slurry with a low solid phase fraction is used, shrinkage cavities may be generated near the interface bonding layer due to volume shrinkage during cooling. Both pores and shrinkage cavities will lead to a decrease in the thermal conductivity and interface bonding strength of the heat sink. Conventional adjustment of the solid phase fraction cannot reduce the generation of pores and shrinkage cavities at the same time, and various parameters need to be strictly controlled, resulting in large batch differences. The present application adds metal particles with an average particle size of 5-10 μm at a mass fraction of 0.3-0.5% during the preparation of semi-solid aluminum alloy slurry. The metal particles contain copper. The metal particles are fully dispersed in the slurry during the slurry making process. During the casting process, the density of the metal particles is much greater than the density of the aluminum alloy, so the metal particles are deposited at the bottom of the slurry. The average particle size of the metal particles is smaller than the average particle size of the crystal grains of the solid aluminum metal particles. The metal particles can replace part of the liquid phase to fill the gap between the rough surface and the solid aluminum metal particles, reduce the gaps caused by the shrinkage of the liquid phase after cooling, form a tighter interface bonding layer, and improve the interface bonding strength and thermal conductivity. The above method uses a semi-solid slurry with high fluidity to avoid pores caused by the inability of the slurry to fully fill the mold, and solves the problem of a large number of shrinkage cavities in the cooling process of the semi-solid slurry with a low solid phase fraction.

[0008] Furthermore, the metal particles include large particles and small particles, the average particle size of the large particles is 10 μm, and the average particle size of the small particles is 5 μm. By using metal particles of various average particle sizes to form a gradation effect, the physical locking effect is further enhanced to provide interface bonding strength. Furthermore, the mass ratio of the large particles to the small particles is 1:(3-7). The metal particles of the above mass ratio can provide stronger interface bonding strength.

[0009] Furthermore, the semi-solid aluminum alloy slurry is prepared by ultrasonic stirring, the frequency of the ultrasonic wave is 20-35KHz, and the ultrasonic treatment time is 10-25s. The ultrasonic stirring method is helpful for dispersing metal particles in the semi-solid slurry.

[0010] Furthermore, the roughness Ra of the roughened surface is 10-20, and Rz is 15-25. Roughness Ra and Rz have a significant effect on the interface bonding strength and interface heat transfer coefficient.

[0011] Furthermore, the aluminum alloy is 6061 aluminum alloy. 6061 aluminum alloy has excellent corrosion resistance and processing performance, and the semi-solid slurry prepared has excellent fluidity and can reduce the generation of shrinkage cavities.

[0012] Furthermore, the roughening treatment is laser texturing treatment. Laser texturing treatment can accurately control the roughness of the rough surface, and through the laser beam heating, melting and re-solidification process of the rough surface, a tiny concave-convex structure can be formed, thereby improving the bonding strength of the bonding interface.

[0013] Furthermore, die casting includes: using a die casting machine for die casting, with a pressure of 400-500MPa, a speed of 800-1000mm / min, and a holding time of 20-30s. Under the above pressure and speed range, the generation of shrinkage cavities can be reduced, and a proper holding time can allow the materials on both sides of the interface layer to fully contact without causing excessive cooling of the metal to produce other adverse reactions.

[0014] Furthermore, the roughness Ra of the roughened surface is 17.8-18.3, and Rz is 24.3-24.9. The roughened surface can better form a physical interlocking structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a diagram of the heat sink interface organization structure of Example 1.

[0016] Figure 2 This is the interface organizational structure diagram of the heat sink of comparative example 1. DETAILED DESCRIPTION

[0017] For ease of understanding of the application, the application will be described more fully below. The application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.

[0018] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0020] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0021] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0022] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.

[0023] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.

[0024] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range of instrument control.

[0025] The "particles" mentioned in this application, or the materials with defined average particle size distribution, are not necessarily spherical in shape, but may be irregular, primary particles or secondary particles. The average particle size of irregular particles is the average of their maximum diameter and minimum diameter.

[0026] Example 1: Roughening treatment of copper plate: After T2 copper was cut and roughened on the abrasive belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness of the treated copper was Ra 18.2 and Rz 24.7. Then, it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40°C and the time was 5min; Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750° C. to obtain an aluminum alloy melt, cooling to 720° C. and then degassing and refining, and when the temperature of the melt is 10° C. above the liquidus, adding 0.5% by mass of copper metal particles with an average particle size of 5 μm (the material of the copper metal particles in all embodiments and comparative examples is T2 copper) into the melt, and keeping the melt warm for later use; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound, the ultrasonic frequency is 25 kHz, the ultrasonic time is 20 s, the power is 2000 W, and a semi-solid aluminum alloy slurry with a solid phase fraction of 35% is obtained; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0027] Example 2: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sand belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness Ra of the treated copper was 18.3 and Rz was 24.9. Then, it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40°C and the time was 5min; Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C and then degassing and refining, when the temperature of the melt is 20°C above the liquidus, adding 0.3% by mass of copper metal particles with an average particle size of 5 μm into the melt, and keeping the melt warm for later use; Copper plate preheating: the mold temperature is 330°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound, the ultrasonic frequency is 25 kHz, the ultrasonic time is 20 s, the power is 2000 W, and a semi-solid aluminum alloy slurry with a solid phase fraction of 35% is obtained; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of a preheated copper plate and die-casted by a die-casting machine at a pressure of 500 MPa, a speed of 1000 mm / min, and a holding time of 20 s to obtain a heat sink.

[0028] Example 3: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sand belt, one side was subjected to laser roughening treatment. The laser power density was set to 35kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness Ra of the treated copper was 10.4 and Rz was 15.3. Then, it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40°C and the time was 5min; Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C, degassing and refining, and when the temperature of the melt is 10°C above the liquidus, adding 0.5% by mass of copper metal particles with an average particle size of 5 μm into the melt, and keeping the melt warm for later use; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound, the ultrasonic frequency is 25 kHz, the ultrasonic time is 20 s, the power is 2000 W, and a semi-solid aluminum alloy slurry with a solid phase fraction of 35% is obtained; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0029] Example 4: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sand belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness of the treated copper was Ra 18.2 and Rz 24.7. Then, it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40°C and the time was 5min; Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C, degassing and refining, and when the temperature of the melt is 10°C above the liquidus, adding 0.5% by mass of copper metal particles with an average particle size of 10 μm into the melt, and keeping the melt warm for later use; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound, the ultrasonic frequency is 25 kHz, the ultrasonic time is 20 s, the power is 2000 W, and a semi-solid aluminum alloy slurry with a solid phase fraction of 35% is obtained; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0030] Example 5: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sand belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness of the treated copper was Ra 17.8 and Rz 24.2. Then, it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40°C and the time was 5min; Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C, degassing and refining, and when the temperature of the melt is 10°C above the liquidus, adding 0.5% by mass of copper metal particles (including small particles with an average particle size of 5 μm and large particles with an average particle size of 10 μm, with a mass ratio of 3:1) into the melt, and keeping it warm for later use; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound, the ultrasonic frequency is 25 kHz, the ultrasonic time is 20 s, the power is 2000 W, and a semi-solid aluminum alloy slurry with a solid phase fraction of 35% is obtained; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0031] Example 6: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sand belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness of the treated copper was Ra 17.9 and Rz 24.3. Then, it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40°C and the time was 5min; Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C, degassing and refining, and when the temperature of the melt is 10°C above the liquidus, adding 0.5% by mass of copper metal particles (including small particles with an average particle size of 5 μm and large particles with an average particle size of 10 μm, with a mass ratio of 7:1) into the melt, and keeping it warm for later use; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound, the ultrasonic frequency is 25 kHz, the ultrasonic time is 20 s, the power is 2000 W, and a semi-solid aluminum alloy slurry with a solid phase fraction of 35% is obtained; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0032] Example 7: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sand belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness of the treated copper was Ra 17.9 and Rz 24.3. Then, it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40°C and the time was 5min; Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C, degassing and refining, and when the temperature of the melt is 10°C above the liquidus, adding 0.5% by mass of copper metal particles (including small particles with an average particle size of 5 μm and large particles with an average particle size of 10 μm, with a mass ratio of 7:1) into the melt, and keeping it warm for later use; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound at an ultrasonic frequency of 25 kHz, an ultrasonic time of 12 s, and a power of 2000 W to obtain a semi-solid aluminum alloy slurry with a solid phase fraction of 15%; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0033] Comparative Example 1: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sanding belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness of the treated copper was Ra 18.2 and Rz 25. Then it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40℃ and the time was 5min. Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C, degassing and refining, and keeping warm for standby when the temperature of the melt is 10°C above the liquidus; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound, the ultrasonic frequency is 25 kHz, the ultrasonic time is 20 s, the power is 2000 W, and a semi-solid aluminum alloy slurry with a solid phase fraction of 35% is obtained; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0034] Comparative Example 2: Roughening treatment of copper plate: After T2 copper was cut and roughened on the sanding belt, one side was subjected to laser roughening treatment. The laser power density was set to 45kW / cm², the pulse frequency was set to 95Hz, and the laser scanning speed was set to 15mm / s. The surface roughness of the treated copper was Ra 18.2 and Rz 25. Then it was pickled and dried. The pickling formula (by volume percentage) was: 15% sulfuric acid, 1% glycolic acid, 2.5% citric acid, and the balance was water; the pickling temperature was 40℃ and the time was 5min. Preparation of aluminum alloy melt: heating 6061 aluminum alloy to 750°C to obtain aluminum alloy melt, cooling to 720°C, degassing and refining, and keeping warm for standby when the temperature of the melt is 10°C above the liquidus; Copper plate preheating: the mold temperature is 350°C, the copper plate after surface pretreatment is placed in the mold, and heated for 60 seconds under nitrogen protection; Ultrasonic preparation of semi-solid aluminum alloy slurry: placing an ultrasonic probe in the aluminum alloy melt to apply ultrasound at an ultrasonic frequency of 25 kHz, an ultrasonic time of 12 s, and a power of 2000 W to obtain a semi-solid aluminum alloy slurry with a solid phase fraction of 15%; Casting and die-casting: The semi-solid aluminum alloy slurry is cast on the rough surface of the preheated copper plate and die-casted by a die-casting machine at a pressure of 450 MPa, a speed of 900 mm / min, and a holding time of 30 s to obtain a heat sink.

[0035] The interface bonding force, tensile strength and thermal conductivity of the heat dissipation plates of Examples 1-7 and Comparative Examples 1-2 were tested.

[0036] Test methods: interface bonding strength (tested by referring to the peeling method in GJB 446-1988, the peeling strength is the interface bonding strength of this embodiment), thermal conductivity of copper-aluminum composite metal plate (measurement of thermal conductivity of copper-aluminum composite metal plate by ISO8301 AMD 1-2010). The test results are shown in Table 1: Table 1

[0037] According to the data in Table 1, the thermal conductivity and interface bonding strength of the heat sinks of Examples 1-2 and Examples 4-7 are higher than those of Comparative Example 1. This is because in the process of preparing the semi-solid aluminum alloy slurry, the present solution adds 0.3-0.5% of metal particles with an average particle size of 5-10 μm, and the metal particles contain copper. The metal particles are fully dispersed in the slurry during the slurry preparation process. During the casting process, the density of the metal particles is much greater than the density of the aluminum alloy, so the metal particles are deposited at the bottom of the slurry. The average particle size of the metal particles is smaller than the average particle size of the solid aluminum metal particles. The metal particles can replace part of the liquid phase to fill the gap between the rough surface and the solid aluminum metal particles, reduce the gaps caused by the contraction of the liquid phase after cooling, form a tighter interface bonding layer, and improve the interface bonding strength and thermal conductivity. Figure 1 As shown, no obvious bubbles were found at the interface of the heat sink in Example 1, the interface transition layer was uniform, and copper and aluminum were fully diffused to form an intermetallic compound layer and a diffusion layer. Figure 2As shown, obvious bubbles appeared at the interface of the heat sink in Example 2, because its higher liquid phase fraction produced shrinkage cavities in some areas during the cooling process. Comparative Example 2 used a semi-solid aluminum alloy slurry with a lower solid phase fraction than Comparative Example 1. Although it helped the slurry to be evenly distributed on the rough surface and fill the solid copper and aluminum solid phase particles, it was easy to produce shrinkage cavities at the interface after cooling, resulting in a decrease in interfacial bonding strength and thermal conductivity. Although Example 7 also used a semi-solid aluminum alloy slurry with a lower solid phase fraction, because its copper metal particles can replace part of the liquid phase to fill the gap between the rough surface and the solid aluminum metal particles, reducing the gaps caused by the shrinkage of the liquid phase after cooling, it can still obtain a heat sink with better thermal conductivity and interfacial bonding strength.

[0038] The roughness Ra and Rz of the rough surface of Example 3 are small, which is not conducive to forming a physical interlocking structure, resulting in poor thermal conductivity and interface bonding strength. Examples 5-6 have better performance than Examples 1 and 4, because by using metal particles of various average particle sizes to form a grading effect, the physical locking effect is further enhanced to provide interface bonding strength.

[0039] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0040] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a heat dissipation plate, characterized in that: The following steps are involved: At least one surface of a copper plate is roughened to obtain a roughened surface, the copper plate is placed in a mold for preheating, an aluminum alloy is heated to obtain an aluminum alloy melt having a temperature of 10-20°C above the liquidus, 0.3-0.5% by mass of metal particles having an average particle size of 5-10 μm are added to the aluminum alloy melt, the aluminum alloy melt is prepared into a semi-solid aluminum alloy slurry having a solid phase fraction of 15-35%, the metal particles containing copper, the semi-solid aluminum alloy slurry is poured on the roughened surface to form an aluminum layer, and the heat sink is obtained by die casting.

2. The preparation method according to claim 1, characterized in that The metal particles include large particles and small particles. The average particle size of the large particles is 10 μm, and the average particle size of the small particles is 5 μm.

3. The preparation method according to claim 2, characterized in that The mass ratio of the large particles to the small particles is 1:(3-7).

4. The preparation method according to claim 1, characterized in that The semi-solid aluminum alloy slurry is prepared by ultrasonic stirring, the frequency of ultrasonic waves is 20-35KHz, and the ultrasonic treatment time is 10-25s.

5. The preparation method according to claim 1, characterized in that The roughness Ra of the roughened surface is 10-20, and Rz is 15-25.

6. The preparation method according to claim 1, characterized in that The aluminum alloy melt is prepared into a semi-solid aluminum alloy slurry with a solid phase fraction of 15-20%.

7. The preparation method according to claim 1, characterized in that The aluminum alloy is 6061 aluminum alloy.

8. The preparation method according to claim 1, characterized in that The roughening process is laser texturing.

9. The preparation method according to claim 1, characterized in that The die casting comprises: using a die casting machine for die casting, with a pressure of 400-500 MPa, a speed of 800-1000 mm / min, and a holding time of 20-30 s.

10. The preparation method according to claim 1, characterized in that The roughness Ra of the roughened surface is 17.8-18.3, and Rz is 24.2-24.9.

Citation Information

Patent Citations

  • Semi-solid state communication heat radiation housing and production method thereof

    CN107787147A

  • Spherical intermetallic compound particle reinforced aluminum-based composite material and preparation method thereof

    CN115505798A

  • Copper-aluminum composite metal plate, casting forming method and application of copper-aluminum composite metal plate in radiator

    CN118180357A

  • Composite body and method for manufacturing the same

    JP2020011278A

  • Method for manufacturing copper aluminum clad material and method for manufacturing heat sink

    JP2023057722A

Cited By

  • Manufacturing method of copper-aluminum composite heat dissipation plate and copper-aluminum composite heat dissipation plate

    CN120619780A