Solid-phase bonding device and method for removing impurities

By controlling the pressure shaft and electrodes of the solid-state bonding device, and utilizing load changes and current flow, the problem of impurities in the bonding of over-surface-treated metals is solved, achieving a high-quality bonding effect.

CN119035740APending Publication Date: 2024-11-29OSAKA UNIVERSITY +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410674765.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In existing technologies, when bonding surface-treated metals, impurities such as plating layers become a problem, leading to a decline in bonding quality and making it difficult to maintain a high-quality bonding effect.

Method used

A solid-state bonding device consisting of a pair of pressure shafts and electrodes is used. By controlling the load change of the pressure shafts and the current flow of the electrodes, tiny protrusions are first formed. Then, the pressure is unloaded and current is applied to remove impurities. Finally, bonding is performed at the protrusion positions.

Benefits of technology

It effectively removes impurities from the metal surface, ensures bonding quality, avoids the influence of residual plating layer, and achieves high-quality solid-phase bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035740A_ABST
    Figure CN119035740A_ABST
Patent Text Reader

Abstract

The invention relates to a solid-phase bonding apparatus and a method for removing impurities. A solid-phase bonding device is provided with: a pair of pressing shafts for pressing a first workpiece and a second workpiece containing a surface-treated metal from both sides in the thickness direction; a pair of electrodes respectively disposed around the pair of pressurizing shafts; and a control device. The control device controls the pair of pressurizing shafts so as to apply a first load to each of the first workpiece and the second workpiece, then controls the pair of pressurizing shafts so as to unload the pressurizing force so as to apply a second load smaller than the first load to the first workpiece and the second workpiece, and then applies a current to the pair of electrodes so as to remove impurities on the metal surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a solid phase bonding apparatus and a method for removing impurities on a metal surface using the solid phase bonding apparatus. Background Art

[0002] International Publication No. 2021 / 182444 discloses a solid-phase point joining device having a pressing portion and a pair of welding electrodes. The pressing portion can press two metal plates in a direction orthogonal to the metal plates. A pair of welding electrodes heats each metal plate by applying electricity to the two metal plates in a state where the two metal plates are clamped from both sides in the thickness direction. In this specification, a joining method such as International Publication No. 2021 / 182444, which prevents a decrease in strength caused by melting of the metal due to a large current by joining the metal in a solid phase state in a low temperature range without melting, is referred to as "solid-phase joining".

[0003] International Publication No. 2021 / 182444 does not consider the joining of metals whose surfaces have been treated by plating or the like. In the joining of metals that have been surface treated, the quality of the joining will be reduced because the plating layer on the metal surface or the like becomes an impurity during joining, and it is sometimes difficult to maintain a high joining quality. In the joining of metals that have been surface treated, it is desirable to join after removing impurities. Summary of the invention

[0004] An object of the present disclosure is to provide a solid phase bonding apparatus capable of removing impurities on the surface of a surface-treated metal and a method for removing impurities on the surface of a metal using the solid phase bonding apparatus.

[0005] The solid phase bonding device of one aspect of the present disclosure comprises: a pair of pressure shafts for pressing a first workpiece and a second workpiece containing a surface-treated metal from both sides in the thickness direction; a pair of electrodes respectively arranged around the pair of pressure shafts; and a control device. The control device controls the pair of pressure shafts so that a first load acts on the first workpiece and the second workpiece respectively, then controls the pair of pressure shafts to unload the pressure so that a second load smaller than the first load acts on the first workpiece and the second workpiece, and then removes impurities on the metal surface by passing an electric current through the pair of electrodes.

[0006] The method for removing impurities in one aspect of the present disclosure is the same as the method for removing impurities from a metal surface using a solid-phase bonding device, wherein the solid-phase bonding device comprises: a pair of pressure shafts for pressing a first workpiece and a second workpiece containing a surface-treated metal from both sides in the thickness direction; a pair of electrodes, respectively arranged around the pair of pressure shafts; and a control device. The control device performs the following steps: by controlling the pair of pressure shafts, a first load is applied to the first workpiece and the second workpiece, respectively; then, by controlling the pair of pressure shafts, the pressure is unloaded so that a second load smaller than the first load is applied to the first workpiece and the second workpiece; then, by passing an electric current through the pair of electrodes, impurities on the metal surface are removed.

[0007] The foregoing and other objects, features, aspects and advantages of the present invention will become more apparent from the following detailed description of the present invention when taken in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 This is a diagram schematically showing a current supply process in the solid phase bonding apparatus according to one embodiment of the present disclosure.

[0009] Figure 2 This is a diagram for explaining a bonding step including removal of impurities on a metal surface in a solid phase bonding apparatus according to an embodiment of the present disclosure.

[0010] Figure 3 This is a diagram schematically showing how electricity is supplied when there is a difference in load.

[0011] Figure 4 This is a graph showing changes in current, load, and stroke with respect to time.

[0012] Figure 5 It is a flowchart showing the control contents executed by the control device.

[0013] Figure 6 It is a diagram showing the change of current with respect to time, the change of load, and the change of stroke in a modification example. DETAILED DESCRIPTION

[0014] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In addition, the same reference numerals are given to the same or corresponding parts in the drawings, and their description will not be repeated.

[0015] Figure 1This is a diagram schematically showing a current supply process in a solid phase bonding apparatus 1 of one embodiment of the present disclosure. The solid phase bonding apparatus 1 is an apparatus that supplies current to a plurality of overlapping workpieces W10 and W20 to form a softened region at the interface of the plurality of workpieces W10 and W20, and plastically deforms the softened region so that the plurality of workpieces W10 and W20 are bonded while maintaining a solid phase state without melting each other.

[0016] The plurality of workpieces W10 and W20 include a first workpiece W10 and a second workpiece W20. Each workpiece W10 and W20 contains a metal such as iron or aluminum. Each workpiece W10 and W20 is formed in a flat plate shape, for example. The metal surface of each workpiece W10 and W20 is processed by plating or the like.

[0017] like Figure 1 As shown, the solid phase bonding apparatus 1 includes a pair of pressurizing shafts 11 and 12 , a pair of electrodes 21 and 22 , a control device 30 , and a sensor 40 .

[0018] The pair of pressurizing shafts 11 and 12 can pressurize the first workpiece W10 and the second workpiece W20 from both sides in the thickness direction of the overlapping plate-like workpieces. The pair of pressurizing shafts 11 and 12 are driven by a driving source (servo press, etc.) not shown in the figure. The pair of pressurizing shafts 11 and 12 include a first pressurizing shaft 11 and a second pressurizing shaft 12.

[0019] The first pressure shaft 11 has a Figure 1 The first pressure shaft 11 is a shape that extends longer (in the direction of the arrow F in FIG. 1 ). The first pressure shaft 11 can press the first workpiece W10 so that the first workpiece W10 is plastically deformed. Specifically, the first pressure shaft 11 can press the first workpiece W10 so that a protrusion W11 can be formed on the first workpiece W10. The first pressure shaft 11 contains, for example, tungsten carbide. In the present embodiment, the first pressure shaft 11 is formed in a cylindrical shape. The first pressure shaft 11 has a pressing surface 11a that presses the first workpiece W10. The pressing surface 11a is an end surface of the first pressure shaft 11. The pressing surface 11a is formed in a circular shape.

[0020] The second pressure shaft 12 has the same structure as the first pressure shaft 11. The second pressure shaft 12 is arranged in a posture where the central axis of the second pressure shaft 12 is located on the extension line of the central axis of the first pressure shaft 11 and the pressing surface 12a of the second pressure shaft 12 is opposite to the pressing surface 11a of the first pressure shaft 11. In addition, the first pressure shaft 11 and the second pressure shaft 12 may also be shapes other than cylindrical.

[0021] The sensor 40 is provided, for example, on the first pressurizing shaft 11. In the present embodiment, a load cell is used as the sensor 40. In addition, the installation location of the sensor 40 is not limited to the first pressurizing shaft 11.

[0022] The pair of electrodes 21 and 22 can energize the first workpiece W10 and the second workpiece W20 while in contact with the first workpiece W10 and the second workpiece W20. Voltage and current are supplied from a power supply unit (not shown) to the pair of electrodes 21 and 22. The pair of electrodes 21 and 22 includes a first electrode 21 and a second electrode 22.

[0023] The first electrode 21 can contact a portion of the first workpiece W10 around a portion pressurized by the first pressure shaft 11. In the present embodiment, the first electrode 21 is formed into a cylindrical shape surrounding the first pressure shaft 11. A gap is provided between the inner peripheral surface of the first electrode 21 and the outer peripheral surface of the first pressure shaft 11. The first electrode 21 contains, for example, copper. The first electrode 21 has a contact surface 21a that contacts the first workpiece W10. The contact surface 21a is formed into a circular ring shape. In addition, the shape of the contact surface 21a is not limited to a circular ring shape.

[0024] The second electrode 22 has the same structure as the first electrode 21. The second electrode 22 can contact a portion of the second workpiece W20 around a portion pressed by the second pressurizing shaft 12. The second electrode 22 is arranged in a posture where the central axis of the second electrode 22 is located on an extension line of the central axis of the first electrode 21 and the contact surface 22a of the second electrode 22 faces the contact surface 21a of the first electrode 21.

[0025] The control device 30 includes a CPU 31 (Central Processing Unit), a memory 32 (ROM (Read Only Memory) and RAM (Random Access Memory)), and an input and output device (not shown) for inputting and outputting various signals. The CPU 31 functions as a processing circuit that expands and executes the program stored in the ROM in the RAM, etc. The program stored in the ROM is a program that records the processing steps of the control device 30. The control device 30 controls each device according to these programs. Regarding this control, it is not limited to software processing, and can also be processed by dedicated hardware (electronic circuit).

[0026] The control device 30 controls the pair of pressurizing shafts 11, 12 and the pair of electrodes 21, 22. Specifically, the control device 30 controls the load applied to the first workpiece W10 and the second workpiece W20 from the pair of pressurizing shafts 11, 12, the load applied to the first workpiece W10 and the second workpiece W20 from the pair of electrodes 21, 22, the voltage applied to the pair of electrodes 21, 22, and the amount of pressing of the pair of pressurizing shafts 11, 12 and the pair of electrodes 21, 22. The control device 30 controls the current supplied to the pair of electrodes 21, 22 by controlling the voltage applied to the pair of electrodes 21, 22.

[0027] The control device 30 operates as follows: a load F (see FIG. 1 ) is applied to the first workpiece W10 and the second workpiece W20 from the pair of pressurizing shafts 11 and 12. Figure 1 ) so that protrusions W11 and W21 that contact each other are formed on the first workpiece W10 and the second workpiece W20, respectively. The control device 30 also performs the following operation: energize the first workpiece W10 and the second workpiece W20. Specifically, the control device 30 performs the following operation: a load F is applied to the first workpiece W10 and the second workpiece W20 from a pair of pressure shafts 11 and 12, and the first workpiece W10 and the second workpiece W20 are energized in a state where the contact surface 21a of the first electrode 21 contacts the portion of the first workpiece W10 around the portion pressurized by the first pressure shaft 11, and the contact surface 22a of the second electrode 22 contacts the portion of the second workpiece W20 around the portion pressurized by the second pressure shaft 12. The control device 30 controls so that the current X shown by the dotted line flows between the pair of electrodes 21 and 22 via each protrusion W11 and W21.

[0028] Each protrusion W11, W21 is softened by passing a current X. In the present embodiment, the control device 30 passes a current X to soften each protrusion W11, W21, and simultaneously applies a load F to the first workpiece W10 and the second workpiece W20. Thus, in the present embodiment, the first workpiece W10 and the second workpiece W20 can be joined at the positions of each protrusion W11, W21.

[0029] Next, the joining process including the removal of impurities on the metal surface will be described. The impurities are, for example, the plating layer of the metal steel plate subjected to surface treatment. Figure 2 FIG. 1 is a diagram for explaining a bonding process including removal of impurities on a metal surface in a solid phase bonding apparatus 1 according to an embodiment of the present disclosure. Figure 2 The bonding process is performed in the order of (A) to (F). Figure 2As shown in (A), the pair of electrodes 21 and 22 are fixed to the pair of pressure shafts 11 and 12 by the spring 50. The urging force of the spring 50 acts on the workpieces W10 and W20 via the pair of electrodes 21 and 22. Figure 2 In the drawings after (B), the spring 50 is omitted.

[0030] like Figure 2 As shown in (A), the control device 30 moves a pair of pressure shafts 11, 12 toward each workpiece W10, W20. At this time, each workpiece W10, W20 is clamped by a pair of electrodes 21, 22. A contact load of, for example, 1 [kN] is applied to each workpiece W10, W20 as the force of the spring 50. The pair of electrodes 21, 22 are applied to a position that is approximately 1 [mm] beyond the pair of pressure shafts 11, 12 toward each workpiece W10, W20. The pair of pressure shafts 11, 12 and the pair of electrodes 21, 22 are a mechanism that is driven as a whole by a driving source (servo press, etc.) not shown in the figure.

[0031] from Figure 2 From the state of (A), Figure 2 As shown in (B), the control device 30 moves a pair of press shafts 11 and 12 toward each workpiece W10 and W20, and applies a pressing load to each workpiece W10 and W20 to form micro protrusions W11' and W21'. The micro protrusions W11' and 21' with small contact areas are formed on each workpiece W10 and W20 by applying a pressing load.

[0032] Next, if Figure 2 As shown in (C), the control device 30 unloads the pressure of the pair of pressure shafts 11 and 12 so that a load smaller than the pressing load acts on each workpiece W10 and W20 from the pair of pressure shafts 11 and 12. The so-called "unloading" means removing at least a part of the load acting on each workpiece W10 and W20. Figure 2 In (C), the pressing force of the pair of pressing shafts 11 and 12 is unloaded to 0 [kN]. In addition, the contact load of 1 [kN] is maintained from the pair of electrodes 21 and 22 to each of the workpieces W10 and W20.

[0033] The control device 30 performs control so that Figure 2 As shown in (C), when the pressing force of the pair of pressing shafts 11 and 12 is unloaded, current flows through each of the micro protrusions W11' and W21' between the pair of electrodes 21 and 22. By flowing current through each of the micro protrusions W11' and W21', impurities remaining on the surface of each of the surface-treated workpieces W10 and W20 can be removed.

[0034] Next, if Figure 2As shown in (D), the control device 30 increases the pressing force of the pair of pressurizing shafts 11 and 12 so that a protrusion forming load larger than the pressing load is applied to each workpiece W10 and W20 from the pair of pressurizing shafts 11 and 12. Each workpiece W10 and W20 is provided with the protrusion forming load to form each protrusion W11 and W21. Each protrusion W11 and W21 is a protrusion having a larger contact area with each workpiece W10 and W20 than each micro protrusion W11' and W21'.

[0035] Next, if Figure 2 As shown in (E), the control device 30 unloads the pressure of the pair of pressure shafts 11 and 12 so that a load smaller than the protrusion forming load acts on each workpiece W10 and W20 from the pair of pressure shafts 11 and 12. Figure 2 In (E), the pressure of the pair of pressure shafts 11 and 12 is unloaded to 0 [kN]. By unloading the pressure of the pair of pressure shafts 11 and 12, the contact area between the protrusions W11 and W21 can be reduced. In addition, the contact load of 1 [kN] is maintained from the pair of electrodes 21 and 22 to each workpiece W10 and W20.

[0036] like Figure 2 As shown in (E), the control device 30 controls so that current flows between the pair of electrodes 21 and 22 through the protrusions W11 and W21 in a state where the pressing force of the pair of pressing shafts 11 and 12 is relieved. When the current flows through the protrusions W11 and W21, the protrusions W11 and W21 soften.

[0037] Next, if Figure 2 As shown in (F), the control device 30 increases the pressure of the pair of pressure shafts 11 and 12 so that a joining load larger than the protrusion forming load is applied to each workpiece W10 and W20 from the pair of pressure shafts 11 and 12. The workpieces W10 and W20 are joined to each other at the positions of the protrusions W11 and W21 by applying the joining load. Specifically, the softened area (including the area at the interface of the contact portion of the workpiece W10 and the workpiece W20) in each protrusion W11 and W21 is joined while maintaining the solid phase state while being plastically deformed.

[0038] Next, the difference between the comparative example in which the load is not unloaded and the embodiment of the present disclosure in which the load is unloaded will be described. Figure 3 This is a diagram schematically showing how electricity is supplied when there is a difference in load. Figure 3 (A) is a diagram showing a power-on state when the load is not unloaded. Figure 3 (B) is a diagram for explaining the state when the power is turned on when the load is not unloaded. Figure 3 (C) is a diagram showing a joined state after energization when the load is not unloaded. Figure 3 (D) is a diagram showing the situation of power supply when the load is unloaded. Figure 3 (E) is a diagram for explaining the state of power-on when the load is unloaded. Figure 3 (F) is a diagram showing a joined state after energization when the load is unloaded.

[0039] like Figure 3 As shown in (A) of FIG. 1 , the current X in the comparative example flows at positions closer to the outside than the center of the microprotrusions W11 ′ and W21 ′. Figure 3 As shown in (D) of FIG. 1 , the current X in the embodiment of the present disclosure flows in a position close to the center of the microprotrusions W11 ′ and W21 ′.

[0040] Specifically, in the comparative example, Figure 3 As shown in (B) of FIG. 1 , the contact area S of each workpiece W10, W20 is in a wide range. In contrast, in the embodiment of the present disclosure, Figure 3 As shown in (E), the contact area S of each workpiece W10, W20 becomes smaller than that of the comparative example. The current X flowing through the pair of electrodes 21, 22 flows through the shortest path in each micro protrusion W11', W21' between the pair of electrodes 21, 22. Figure 3 In the comparative example (B), the central portion which is pressed by the pair of pressure shafts 11 and 12 is difficult to flow current and becomes a low-heating area B, and the outer portion of the low-heating area B becomes a high-heating area A that is easy to flow current. Figure 3 In the embodiment of the present disclosure of (E), the central portion becomes the high heat generation area A by unloading the load of the pair of pressurizing shafts 11 and 12 .

[0041] In the comparative example, Figure 3 As shown in (C), since it is difficult for the current X to flow in the central portion, impurities from the plating treatment on the metal surface will remain in the central portion. In contrast, in the embodiment of the present disclosure, Figure 3 As shown in (F), by passing the current X through the central portion, impurities in the plating process on the metal surface are discharged from the central portion to the periphery, and it is possible to prevent impurities from remaining in the central portion.

[0042] Next, use graphs to illustrate the change in current with respect to time, the change in load, and the change in travel. Figure 4 It is a graph showing the change of current with respect to time, the change of load and the change of stroke. Figure 4 The stroke in denoted as 1 means that the pressurizing shaft 11 and the pressurizing shaft 12 move with the same stroke amount. Figure 4 The load in indicates that the same load acts on the pressurizing shaft 11 and the pressurizing shaft 12 .

[0043] like Figure 4 As shown, the control device 30 brings the front end of the solid phase bonding device 1 close to each workpiece W10, W20 from time T0 to time T1, and at time T1, the distance between the front end of the solid phase bonding device 1 and each workpiece W10, W20, that is, the stroke, is set to 0 [mm]. At time T1, a pair of electrodes 21, 22 are in contact with each workpiece W10, W20. The control device 30 applies a contact load to each workpiece W10, W20 from a pair of electrodes 21, 22 from time T1 to time T2. At this time, although the stroke and current do not change, the load increases by the amount of the contact load 1 [kN] when the pair of electrodes 21, 22 are in contact with each workpiece W10, W20.

[0044] Next, the control device 30 presses the pair of pressurizing shafts 11 and 12 into the workpieces W10 and W20 by 0.3 [mm] from time T2 to T3, thereby forming micro protrusions W11' and W21'. At this time, the stroke changes, and the pressing load when the pair of pressurizing shafts 11 and 12 are pressed into the workpieces W10 and W20 becomes 3 [kN]. From time T2 to T3, the current does not change.

[0045] Next, the control device 30 unloads the pressure of the pair of pressure shafts 11 and 12 from time T3 to time T4. As a result, the stroke changes to 0 [mm], and the load becomes only 1 [kN] of the contact load. At this time, the control device 30 flows a 4 [kA] current through the micro protrusions W11' and W21', thereby discharging impurities on the metal surface from the central part to the periphery. As a result, the solid phase bonding device 1 can remove surface impurities in the metal that has been surface treated.

[0046] Next, the control device 30 forms protrusions W11 and W21 by pressing the pair of pressurizing shafts 11 and 12 into the workpieces W10 and W20 by 1.4 [mm] from time T4 to time T5. At this time, the stroke changes, and the protrusion forming load when the pair of pressurizing shafts 11 and 12 are pressed into the workpieces W10 and W20 becomes 35 [kN]. The control device maintains the pressurization of the protrusion forming load from time T5 to time T6. In addition, the current does not change from time T4 to time T6.

[0047] Next, the control device 30 unloads the pressure of the pair of pressure shafts 11 and 12 from time T6 to time T7. As a result, the stroke changes to 0 [mm], and the load becomes only 1 [kN] which is the contact load. At this time, the control device 30 flows a current of 11 [kA] through the protrusions W11 and W21 to soften each protrusion W11 and W21.

[0048] Next, the control device 30 presses the pair of pressure shafts 11 and 12 into each workpiece W10 and W20 by 2.4 [mm] from time T7 to time T8, thereby joining the protrusions W11 and W21 to each other. At this time, the stroke changes, and the joining load when the pair of pressure shafts 11 and 12 are pressed into each workpiece W10 and W20 becomes 40 [kN]. The control device continuously flows a current of 11 [kA] through each protrusion W11 and W21 from time T7 to time T8. As a result, while the softened area in each protrusion W11 and W21 is plastically deformed, the area can be joined while maintaining the solid phase state unchanged. Next, the control device 30 reduces the stroke and load from time T8 to time T9, and maintains the current at 0 [kA].

[0049] Next, the processing executed by the control device 30 will be described in detail. Figure 5 : is a flowchart showing the control content executed by the control device 30. Figure 5 The processing of the flowchart is repeatedly called out and executed as a subroutine from a main routine in the control of the control device 30. The control device 30 first moves the pair of pressurizing shafts 11 and 12 toward the first workpiece W10 and the second workpiece W20 in step S (hereinafter simply indicated as "S") 1.

[0050] Next, the control device 30 determines whether the pair of pressure shafts 11 and 12 are in contact with the first workpiece W10 and the second workpiece W20 (S2). For example, the control device 30 obtains the detection value of the sensor 40, and determines that the pair of pressure shafts 11 and 12 are in contact with the first workpiece W10 and the second workpiece W20 based on the increase in the detection value. The control device 30 stores the contact position as the reference position in S2. When the control device 30 determines that the pair of pressure shafts 11 and 12 are not in contact with the first workpiece W10 and the second workpiece W20 (No in S2), the control device 30 returns to the processing of S1. When the control device 30 determines that the pair of pressure shafts 11 and 12 are in contact with the first workpiece W10 and the second workpiece W20 (Yes in S2), the control device 30 transfers to the processing of S3.

[0051] In S3, the control device 30 presses the pair of pressurizing shafts 11 and 12 to the formation position of the micro protrusions W11' and W21' as the first protrusions. Next, the control device 30 unloads the pressurizing force of the pair of pressurizing shafts 11 and 12 (S4). Next, the control device 30 performs a process of passing current to the micro protrusions W11' and W21' for removing impurities such as plating on the metal surface (S5).

[0052] Next, the control device 30 presses the pair of pressure shafts 11 and 12 to the formation position of the protrusions W11 and W21 as the second protrusion (S6). Next, the control device 30 determines whether the pair of pressure shafts 11 and 12 have reached the formation position of the second protrusion (S7). The control device 30 may, for example, determine whether the pair of pressure shafts 11 and 12 have moved from the contact position stored in S2 to the formation position of the second protrusion where the protrusions W11 and W21 are formed on the first workpiece W10 and the second workpiece W20. The control device 30 stores the formation position of the second protrusion as the reference position in S7. When the control device 30 determines that the pair of pressure shafts 11 and 12 have not reached the formation position of the second protrusion (No in S7), it returns to the processing of S6.

[0053] When the control device 30 determines that the pair of pressurizing shafts 11 and 12 have reached the formation position of the second projection (Yes in S7 ), the control device 30 proceeds to the process of S8 . In the process of S8 , the control device 30 releases the pressurizing force of the pair of pressurizing shafts 11 and 12 .

[0054] Next, the control device 30 performs power-on for joining and presses the pair of pressure shafts 11 and 12 into the joining position (S9). Next, the control device 30 determines whether the protrusions W11 and W21 in the first workpiece W10 and the second workpiece W20 have been softened based on the detection value of the sensor 40 (S10). The control device 30 determines whether the protrusions W11 and W21 have been softened, for example, by determining whether the detection value of the sensor 40 is below a predetermined threshold. When it is determined that the protrusions W11 and W21 have not been softened (when the detection value of the sensor 40 is greater than the threshold), the control device 30 returns to S9. When it is determined that the protrusions W11 and W21 have been softened (when the detection value of the sensor 40 is below the threshold), the control device 30 transfers to the processing of S11.

[0055] The control device 30 determines in S11 whether the pair of pressurizing shafts 11 and 12 have reached the joining position. For example, the control device 30 may determine whether the pair of pressurizing shafts 11 and 12 have moved from the second protrusion formation position stored in S7 to the joining position for joining the first workpiece W10 and the second workpiece W20.

[0056] If the control device 30 determines that the pair of pressurizing shafts 11 and 12 have not reached the engagement position (No in S11), the control device 30 returns to the process of S9. If the control device 30 determines that the pair of pressurizing shafts 11 and 12 have reached the engagement position (Yes in S11), the process returns from the subroutine to the main routine.

[0057] like Figure 5As shown, the solid phase bonding apparatus 1 of this embodiment performs unloading and energization in S4 and S5 after the micro protrusions W11' and W21' are formed. Thus, current can be passed through the center of the micro protrusions W11' and W21', and impurities on the surface of the surface treated metal can be effectively removed.

[0058] Next, the change of current with respect to time, the change of load, and the change of stroke in the case of a modified example in which the pair of pressurizing shafts 11, 12 and the pair of electrodes 21, 22 are driven by different drive sources (servo press, etc.) are described using graphs. The control device 30 controls the movement of the pair of pressurizing shafts 11, 12 by the first drive source, and controls the movement of the pair of electrodes 21, 22 by the second drive source, for example. Figure 6 It is a diagram showing the change of current with respect to time, the change of load, and the change of stroke in a modification example.

[0059] exist Figure 6 Regarding the stroke and current, due to Figure 4 Regarding the load, the pressure shaft load (solid line) corresponding to the pair of pressure shafts 11 and 12 and the electrode contact load (dashed line) corresponding to the pair of electrodes 21 and 22 are shown on the same graph. Figure 6 As shown, the electrode contact load is 0 [kN] from time T0 to time T3, and becomes 1 [kN] from time T3 to time T4. Thereafter, the electrode contact load becomes 0 [kN] from time T4 to time T6, becomes 1 [kN] from time T6 to time T8, and becomes 0 [kN] from time T8 to time T9.

[0060] In this way, the electrode contact load takes any value between 0 [kN] and 1 [kN]. The current flows from time T3 to time T4 and from time T6 to time T8 when the electrode contact load is 1 [kN]. In addition, when the electrode is moved by a different actuator, the electrode contact load also becomes 0 [kN] or 1 [kN]. Specifically, in the case of a spring type, by adopting a floating mechanism, the electrode contact load can be set to 0 [kN] or 1 [kN].

[0061] like Figure 6As shown, the pressure shaft load is 1 [kN] from time T1 to time T2, and becomes 3 [kN] from time T2 to time T3. After that, the pressure shaft load becomes 0 [kN] due to unloading from time T3 to time T4. After that, the pressure shaft load increases to 35 [kN] from time T4 to time T5, and maintains a load of 35 [kN] from time T5 to time T6. After that, the pressure shaft load becomes 0 [kN] due to unloading from time T6 to time T7. After that, the pressure shaft load increases to 40 [kN] from time T7 to time T8, and the load decreases from time T8 to time T9.

[0062] like Figure 6 As shown, even when a pair of pressurizing shafts 11, 12 and a pair of electrodes 21, 22 are driven by different drive sources, the control device 30 can change the current, load and stroke in the same way as when a pair of pressurizing shafts 11, 12 and a pair of electrodes 21, 22 are driven by one drive source.

[0063] In the above-mentioned embodiment, the detection value of the force sensor as the sensor 40 is used, but the softening of each workpiece W10, W20 can also be detected by a sensor different from the force sensor. As such a sensor, a camera that can capture the contact portion between the protrusions W11, W21 can also be used. In this case, the control device 30 determines whether each workpiece W10, W20 has softened based on the brightness of the contact portion. As such a sensor, a contact or non-contact thermometer can be used. The control device 30 can determine whether each workpiece W10, W20 has softened based on the temperature of the contact portion. Alternatively, the control device 30 can also determine whether each workpiece W10, W20 has softened based on the result of the heat calculation of each workpiece W10, W20 obtained in advance and the timer of the power supply.

[0064] <Summary>

[0065] (1) The solid phase bonding apparatus 1 of the present disclosure comprises: a pair of pressurizing shafts 11 and 12 for pressing a first workpiece W10 and a second workpiece W20 containing a surface-treated metal from both sides in the thickness direction; a pair of electrodes 21 and 22 respectively arranged around the pair of pressurizing shafts 11 and 12; and a control device 30. The control device 30 controls the pair of pressurizing shafts 11 and 12 so that a first load acts on the first workpiece W10 and the second workpiece W20, respectively, and then controls the pair of pressurizing shafts 11 and 12 to unload the pressurizing force so that a second load smaller than the first load acts on the first workpiece W10 and the second workpiece W20, and then removes impurities on the metal surface by passing an electric current through the pair of electrodes 21 and 22.

[0066] (2) In the solid phase bonding apparatus 1 of (1), the control device 30 supplies current to the pair of electrodes 21 and 22 in a state where the pair of pressurizing shafts 11 and 12 are moved to positions not in contact with the first workpiece W10 and the second workpiece W20 .

[0067] (3) The solid phase bonding apparatus 1 of (1) or (2) further comprises a driving source for driving the pair of pressurizing shafts 11, 12 and the pair of electrodes 21, 22. The control device 30 controls the driving source to move the pair of pressurizing shafts 11, 12 and the pair of electrodes 21, 22.

[0068] (4) In any one of the solid phase bonding devices 1 of (1) to (3), after removing impurities from the metal surface, a pair of pressure shafts 11 and 12 are controlled so that a third load greater than the first load is applied to the first workpiece W10 and the second workpiece W20, respectively, while current is passed through a pair of electrodes 21 and 22.

[0069] (5) The impurity removal method disclosed in the present invention is related to a method for removing impurities from a metal surface using a solid phase bonding apparatus 1, wherein the solid phase bonding apparatus 1 comprises: a pair of pressurizing shafts 11, 12 for pressing a first workpiece W10 and a second workpiece W20 containing a surface-treated metal from both sides in a thickness direction; a pair of electrodes 21, 22, respectively arranged around the pair of pressurizing shafts 11, 12; and a control device 30. The control device 30 performs the following steps: controlling the pair of pressurizing shafts 11, 12 so that a first load is applied to the first workpiece W10 and the second workpiece W20, respectively; then, unloading the pressurizing force by controlling the pair of pressurizing shafts 11, 12 so that a second load smaller than the first load is applied to the first workpiece W10 and the second workpiece W20; and then, removing impurities from the metal surface by passing an electric current through the pair of electrodes 21, 22.

[0070] According to the solid phase bonding apparatus 1 and the method for removing impurities from the metal surface using the solid phase bonding apparatus 1 disclosed in the present invention, after the first load is applied to the first workpiece W10 and the second workpiece W20, respectively, the pressure is unloaded by controlling the pair of pressure shafts 11 and 12 so that the second load smaller than the first load is applied to the first workpiece W10 and the second workpiece W20, and current is passed through the pair of electrodes 21 and 22. Thus, current can flow through the central portion of the metal that has been surface treated, and impurities on the metal surface can be removed.

[0071] Although the embodiments of the present invention have been described, the embodiments disclosed this time should be considered to be illustrative in all aspects and not restrictive. The scope of the present invention is indicated by the claims, and it is intended to include all modifications within the meaning and scope equivalent to the claims.

Claims

1. A solid phase bonding device comprising: A pair of pressurizing shafts presses a first workpiece and a second workpiece including a surface-treated metal from both sides in a thickness direction; a pair of electrodes, respectively disposed around the pair of pressurizing shafts; and Control device, The control device performs the following processing: The pair of pressurizing shafts are controlled so that a first load acts on the first workpiece and the second workpiece, respectively. Next, the pair of pressurizing shafts are controlled to unload the pressurizing force so that a second load smaller than the first load acts on the first workpiece and the second workpiece. Next, impurities on the metal surface are removed by passing an electric current through the pair of electrodes.

2. The solid phase bonding device according to claim 1, wherein: The control device supplies current to the pair of electrodes in a state where the pair of pressurizing shafts are moved to positions where they are not in contact with the first workpiece and the second workpiece.

3. The solid phase bonding device according to claim 1 or 2, wherein: The solid phase bonding device further includes a driving source, and the driving source drives the pair of pressurizing shafts and the pair of electrodes. The control device moves the pair of electrodes while moving the pair of pressurizing shafts by controlling the driving source.

4. The solid phase bonding device according to claim 1 or 2, wherein: After removing impurities from the metal surface, the control device controls the pair of pressurizing shafts so that a third load greater than the first load acts on each of the first workpiece and the second workpiece, and simultaneously supplies current to the pair of electrodes.

5. A method for removing impurities from a metal surface using a solid phase bonding apparatus, wherein: The solid phase bonding device comprises: A pair of pressurizing shafts presses a first workpiece and a second workpiece including a surface-treated metal from both sides in a thickness direction; a pair of electrodes, respectively disposed around the pair of pressurizing shafts; and Control device, The control device performs the following steps: The first load is applied to the first workpiece and the second workpiece respectively by controlling the pair of pressurizing shafts; Next, the pressing force is unloaded by controlling the pair of pressing shafts so that a second load smaller than the first load acts on the first workpiece and the second workpiece; and Next, impurities on the metal surface are removed by passing an electric current through the pair of electrodes.

Citation Information

Patent Citations

  • Solid-phase spot-welding method and solid-phase spot-welding device