Preparation method and application of hard carbon material

By mixing biomass with additives such as resin acid for cross-linking and polymerization and carbonization, high-performance hard carbon materials are prepared, which solves the problems of reversible capacity and low Coulomb efficiency in sodium and potassium ion batteries. It realizes high-performance applications in lithium, sodium and potassium ion batteries.

CN119038525AInactive Publication Date: 2024-11-29UNIV OF SCI & TECH OF CHINA

Patent Information

Application Number
CN202411239276.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The reversible capacity and first-time Coulomb efficiency of existing hard carbon materials in sodium and potassium ion batteries are not ideal, and are affected by surface defects and interface side reactions, which limits their application in soft-pack and cylindrical full batteries.

Method used

By mixing biomass with a total content of cellulose and hemicellulose with resin acid or other additives, carbonizing after cross-linking polymerization, hard carbon materials rich in pore structure are prepared, which is suitable for large-scale industrial production.

Benefits of technology

The hard carbon material produced has high reversible capacity and high first-time Coulomb efficiency, suitable for lithium, sodium, potassium ion batteries or capacitors, significantly improving its performance in these applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a hard carbon material, and belongs to the technical field of materials. The preparation method of the hard carbon material comprises the following steps: 1) mixing biomass with the total content of cellulose and hemicellulose being greater than 50% with a raw material A, and heating to carry out cross-linking polymerization reaction to obtain an intermediate product; 2) carbonizing and crushing the intermediate product to obtain a hard carbon material; the raw material A is selected from an additive and / or wood with the resin acid content of 1%-50%. The preparation method is easily available in raw materials, simple, efficient and suitable for large-scale industrial production. The hard carbon material prepared by the method disclosed by the invention is rich in pore structure, and has relatively high reversible specific capacity and relatively high initial coulombic efficiency when being applied to lithium, sodium and potassium ion batteries or capacitors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to a preparation method and application of a hard carbon material. Background Art

[0002] The large-scale implementation of renewable energy requires cheap and efficient large-scale energy storage technologies. Lithium-ion batteries are widely used as power sources for portable electronic devices, electric vehicles, and hybrid vehicles due to their high energy density and high power density. However, limited lithium resources and uneven geographical distribution hinder the application of lithium batteries in large-scale energy storage. Therefore, there is an urgent need to find cheaper alternative energy storage technologies. Recently, sodium and potassium ion batteries have attracted more and more attention from researchers due to their low cost and high earth abundance.

[0003] At present, biomass hard carbon materials are considered to be ideal sodium and potassium ion negative electrode materials due to their high capacity, low cost and wide sources. Biomass hard carbon materials can be used in secondary batteries or capacitors. However, the reversible capacity of existing hard carbon materials is still not ideal, and the irreversible ion storage caused by surface defects and interface side reactions also makes the first coulomb efficiency low, which seriously hinders the application of hard carbon materials in soft-pack and cylindrical full batteries.

[0004] Therefore, researching and developing a new method for preparing hard carbon so that the hard carbon material has high capacity in a low voltage region is of great significance for the application of sodium and potassium ion batteries. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a preparation method and application of a hard carbon material. The preparation method has readily available raw materials, is simple and efficient, and is suitable for large-scale industrial production. The prepared hard carbon material has the advantages of high reversible capacity and high first coulombic efficiency.

[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] The present invention provides a method for preparing a hard carbon material, characterized by comprising the following steps:

[0008] 1) mixing biomass having a total content of cellulose and hemicellulose greater than 50% with raw material A, heating and performing cross-linking polymerization to obtain an intermediate product;

[0009] 2) carbonizing and crushing the intermediate product to obtain a hard carbon material;

[0010] The raw material A is selected from wood with an additive and / or resin acid content of 1%-50%.

[0011] The additive is selected from one or more of resin acid, oleic acid, formic acid, acetic acid, lactic acid, oxalic acid, succinic acid, maleic acid, and rosin acid; more preferably, one or more of oleic acid, formic acid, and rosin acid.

[0012] Preferably, in the present invention, the biomass having a total cellulose and hemicellulose content greater than 50% is selected from one or more of lychee wood, camphor wood, apricot wood, poplar wood, oak, elm wood, olive kernel, walnut shell, cotton, bamboo, bagasse, waste paper, and waste cotton yarn; more preferably, it is one or more of lychee wood, bamboo, waste paper, and bagasse.

[0013] The wood with a resin acid content of 1%-50% is selected from one or more of pine, fir, cypress, and walnut; more preferably, pine or fir.

[0014] More preferably, the raw material of the porous structure-rich hard carbon is selected from pine and bamboo; further preferably, the resin content of the pine is 10 wt %; further preferably, the mass ratio of the pine to bamboo is 1: (10-20).

[0015] More preferably, the raw material of the porous hard carbon is selected from waste paper and oleic acid;

[0016] Further preferably, the oleic acid is (10-20) wt % of the waste paper.

[0017] More preferably, the raw material of the porous structure-rich hard carbon is selected from an ethanol solution of rosin acid and lychee wood; further preferably, the content of rosin acid is 10wt%; further preferably, the rosin acid is (10-30)wt% of the lychee wood.

[0018] More preferably, the raw material of the porous structure-rich hard carbon is selected from fir and bagasse; further preferably, the resin content of the fir is 5 wt%; further preferably, the mass ratio of the fir to bagasse is 1:(50-80).

[0019] The preparation method of the present invention controls the type of raw materials and the heating temperature so that the hard carbon material undergoes cross-linking polymerization reaction, carbonization and pulverization in sequence to obtain the hard carbon material.

[0020] Preferably, the heating temperature in step 1) is 150°C-290°C. In some specific embodiments of the present invention, it is 250°C, 290°C, 200°C or 150°C.

[0021] In the above cross-linking polymerization reaction, the resin in the wood softens and flows under heating and is grafted onto the polymer chains of cellulose or hemicellulose in the biomass; or, the additive grafts onto the polymer chains of cellulose or hemicellulose in the biomass under heating; or, the resin in the wood and the additive graft onto the polymer chains of cellulose or hemicellulose in the biomass, thereby forming an intermediate product with increased carbon content, improved stability and enhanced hydrophobicity.

[0022] Preferably, in the step 1), the mass ratio of the biomass having a total cellulose and hemicellulose content greater than 50% to the raw material A is (0.1-100):1; more preferably (3-80):1; further preferably 10:1 or 3:1 or 80:1.

[0023] Preferably, in the step 1), when the raw material A contains additives, the additives are 1%-50% of the mass of the biomass with a total cellulose and hemicellulose content greater than 50%; more preferably (10%-30%): 1.

[0024] Preferably, the additive further comprises a solvent;

[0025] The solvent is selected from one or more of ethanol, acetaldehyde, acetone and benzene; more preferably, ethanol.

[0026] Preferably, the temperature of the carbonization in step 2) is 700°C-2000°C, more preferably 1200°C-1500°C. In some specific embodiments of the present invention, it is preferably 1400°C, 1500°C, 1300°C or 1200°C.

[0027] The carbonization in step 2) is carried out under an inert atmosphere;

[0028] The inert atmosphere includes, but is not limited to, one or more of nitrogen, helium, neon, argon, krypton, and xenon.

[0029] The pulverization is selected from one or more of air flow pulverization, disc pulverization, ball mill pulverization and ultrasonic pulverization.

[0030] After the above pulverization, the hard carbon material is sieved.

[0031] The preparation method prepares the hard carbon material through biomass, wood and the additive, the raw materials are easily available, and the method is simple and efficient.

[0032] The present invention also provides a hard carbon material prepared by the above preparation method.

[0033] Preferably, the specific surface area of ​​the hard carbon material is 1-50 m 2 g -1The total volume of open and closed pores is 0.001-0.12 cm 3 g -1 , the porosity is 1%-20%.

[0034] The present invention also provides a lithium, sodium, potassium ion battery or capacitor, which uses the hard carbon material as a negative electrode material.

[0035] In some specific embodiments of the present invention, the reversible capacity of the sodium ion battery reaches 367-402 mAh g -1 , the first discharge capacity reaches 432-486 mAh g -1 , for the first time, the Coulombic efficiency reached 80%-91%.

[0036] Compared with the prior art, the preparation method of the hard carbon material provided by the present invention comprises the following steps: 1) mixing biomass having a total content of cellulose and hemicellulose greater than 50% with raw material A, heating and performing a cross-linking polymerization reaction to obtain an intermediate product; 2) carbonizing and crushing the intermediate product to obtain a hard carbon material; the raw material A is selected from wood having an additive and / or a resin acid content of 1%-50%. The preparation method has easy-to-obtain raw materials, is simple and efficient, and is suitable for large-scale industrial production. The hard carbon material prepared by the method of the present invention is rich in pore structure, and is applied to lithium, sodium, potassium ion batteries or capacitors, and has a high reversible specific capacity and a high first coulombic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Flow chart for preparing hard carbon in Example 1;

[0038] Figure 2 Figure a is a SEM image of the intermediate product prepared in Example 1 and Figure b is a SEM image of the hard carbon with a rich porous structure prepared in Example 1;

[0039] Figure 3 XRD pattern of the hard carbon with rich pore structure prepared in Example 1;

[0040] Figure 4 This is a charge and discharge curve of a sodium ion half-cell assembled with hard carbon having a rich porous structure prepared in Example 1;

[0041] Figure 5 This is a flow chart for preparing hard carbon in Example 2. DETAILED DESCRIPTION

[0042] In order to further illustrate the present invention, the preparation method and application of the hard carbon provided by the present invention are described in detail below in conjunction with examples.

[0043] Example 1

[0044] (I) Method for preparing hard carbon with rich pore structure (process as follows Figure 1 ), including the following steps:

[0045] Step S1, mixing: put pine wood (resin content 10%) and bamboo in a mass ratio of 1:10 into a medicinal material crusher at room temperature, physically crush them into particles of 0.1-2 mm in size and mix them to obtain a precursor coarse powder.

[0046] Step S2, preparation of intermediate product: 100 g of the above-mentioned precursor coarse powder is placed in a glass evaporating dish and covered, then placed in a blast oven and heated to 250° C. at a heating rate of 10° C. / min, kept warm for 10 hours, and cooled to room temperature to obtain an intermediate product, i.e., a cross-linked polymerization product.

[0047] Step S3, high temperature carbonization: Place the above intermediate product in a box furnace, heat it to 1400℃ at a heating rate of 5℃ / min under argon protection for 4 hours, and take it out after cooling to room temperature. Pour the product into a jet mill for crushing and classification to obtain hard carbon with a porous structure with a particle size of 1~80μm. Its specific surface area is 16 m 2 g -1 , the total volume of open and closed pores is 0.09 cm 3 g -1 , the porosity is 15%.

[0048] The SEM images of the intermediate product prepared above and the SEM images of the hard carbon with a porous structure are shown in FIG. Figure 2 As shown in Figure a and Figure b. Figure b shows that the crushed hard carbon is in irregular granular form with a size between 1 and 80 μm. (ii) Assembly of lithium, sodium, and potassium ion batteries: The hard carbon with a porous structure prepared as described above is used as the positive electrode, and lithium / sodium / potassium metal is used as the negative electrode. The battery assembly is carried out in an argon-protected glove box (water and oxygen contents are both less than 0.1 ppm). The electrolyte used is 1 mol / L LiPF 6 / NaPF 6 / KPF 6 The solution (solvent includes ethylene carbonate EC and diethyl carbonate DEC) is used in an amount of 60 μL, and the separator is Glass Fiber. A CR2032 button cell is assembled in an argon-protected glove box (water and oxygen contents are both less than 1 ppm).

[0049] Figure 3 This is the XRD pattern of the hard carbon with rich pore structure prepared in Example 1. The results show that the hard carbon has only two broad diffraction peaks, indicating that it is an amorphous material. The diffraction peaks at about 23 degrees and 43 degrees correspond to the (002) and (100) crystal planes of the amorphous carbon layer, respectively.

[0050] Figure 4The charge and discharge curve of the sodium ion half-cell assembled with hard carbon rich in pore structure prepared in Example 1, the first discharge capacity reaches 442 mAh g -1 , the reversible capacity reaches 402 mAh g -1 , the first Coulombic efficiency was 91%.

[0051] Example 2

[0052] Please refer to the preparation process Figure 5 , which is different from Example 1 in that:

[0053] In step S1, instead of using resin-containing wood to mix with the biomass organic raw material, an additive is used to directly soak the biomass organic raw material. Specifically, the following steps are included:

[0054] Step S1, mixing, physically crushing the waste paper into a particle size of 0.1-1 mm, and then soaking it in oleic acid, the total mass of oleic acid being 10% of the mass of the waste paper, and stirring overnight to fully soak it. The soaked waste paper coarse powder is taken out to obtain a precursor coarse powder.

[0055] Step S2, preparation of intermediate product: 50 g of the above-mentioned precursor coarse powder is put into a quartz crucible and covered, then put into a muffle furnace and heated to 290° C. at a heating rate of 5° C. / min, kept warm for 6 hours, and cooled to room temperature to obtain an intermediate product, i.e., a cross-linked polymerization product.

[0056] Step S3, high temperature carbonization: Place the above intermediate product in a tubular furnace, heat it to 1500°C at a heating rate of 3°C / min under nitrogen protection for 2 hours, and take it out after cooling to room temperature. Pour the product into a jet mill for crushing and classification to obtain hard carbon with a porous structure and a particle size of 1~70μm. Its specific surface area is 14 m 2 g -1 , the total volume of open and closed pores is 0.07 cm 3 g -1 , the porosity is 10%.

[0057] The sodium ion battery was assembled according to the method of Example 1. The test results showed that in the voltage range of 0-2.5 V and at a current density of 0.1C, the first discharge capacity of the sodium ion battery reached 452 mAh g -1 , the reversible capacity reaches 398 mAhg -1 , the first Coulombic efficiency is 88%.

[0058] Example 3

[0059] The difference from Example 1 is:

[0060] In step S1, instead of mixing the resin-containing wood with the biomass organic raw material, a solution containing additives is used to soak the biomass organic raw material. Specifically, the steps include:

[0061] The litchi wood was physically crushed into a particle size of 0.1-4 mm, and then immersed in an ethanol solution containing 10% rosin acid by mass, wherein the total content of rosin acid in the solution was 30% of the mass of the litchi wood, and stirred overnight for full infiltration. The infiltrated litchi wood coarse powder was taken out and placed in a 60°C vacuum oven to completely remove excess ethanol solvent, and then dried to obtain a precursor coarse powder.

[0062] Step S2, preparation of intermediate product: 70 g of the above-mentioned precursor coarse powder is put into a corundum crucible and covered, then put into a muffle furnace and heated to 200° C. at a heating rate of 10° C. / min, kept warm for 12 hours, and cooled to room temperature to obtain an intermediate product, i.e., a cross-linked polymerization product.

[0063] Step S3, high temperature carbonization: Place the above intermediate product in a box furnace, heat it to 1300℃ at a heating rate of 2℃ / min under helium protection for 6 hours, and take it out after cooling to room temperature. Pour the product into a jet mill for crushing and classification to obtain hard carbon with a porous structure and a particle size of 1~50μm. Its specific surface area is 10 m 2 g -1 , the total volume of open and closed pores is 0.05 cm 3 g -1 , the porosity is 8%.

[0064] The sodium ion battery was assembled according to the method of Example 1. The test results showed that in the voltage range of 0-2.5 V and at a current density of 0.1C, the first discharge capacity of the sodium ion battery reached 432 mAh g -1 , the reversible capacity reaches 367 mAhg -1 , the first Coulombic efficiency is 85%.

[0065] Example 4

[0066] The difference from Example 1 is:

[0067] In step S1, not only the resin-containing wood is mixed with the biomass organic raw material, but also the additive is used to soak the biomass organic raw material. Specifically, it includes:

[0068] Put fir (resin content 5 wt%) and bagasse in a mass ratio of 1:80 into a medicinal material crusher at room temperature, physically crush to 0.1~3 mm particle size and mix, then soak in formic acid, the total mass of formic acid is 50% of the mass of the coarse powder, stir overnight to fully infiltrate. Take out the infiltrated coarse powder to obtain the precursor coarse powder.

[0069] Step S2, preparation of intermediate product: 70 g of the above-mentioned precursor coarse powder is put into a corundum crucible and covered, then put into a vacuum oven and heated to 150°C at a heating rate of 10°C / min, kept warm for 12 hours, and cooled to room temperature to obtain an intermediate product, i.e., a cross-linked polymerization product.

[0070] Step S3, high temperature carbonization: Place the above intermediate product in a tubular furnace, heat it to 1200°C at a heating rate of 1°C / min under nitrogen protection for 2 hours, and take it out after cooling to room temperature. Pour the product into a jet mill for crushing and classification to obtain hard carbon with a porous structure and a particle size of 1~50μm. Its specific surface area is 20 m 2 g -1 , the total volume of open and closed pores is 0.12 cm 3 g -1 , the porosity is 18%.

[0071] The sodium ion battery was assembled according to the method of Example 1. The test results showed that in the voltage range of 0-2.5 V and at a current density of 0.1C, the first discharge capacity of the sodium ion battery reached 486 mAh g -1 , the reversible capacity reaches 388 mAhg -1 , the first Coulombic efficiency is 80%.

[0072] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a hard carbon material, characterized in that: The following steps are involved: 1) mixing biomass having a total content of cellulose and hemicellulose greater than 50% with raw material A, heating and performing cross-linking polymerization to obtain an intermediate product; 2) carbonizing and crushing the intermediate product to obtain a hard carbon material; The raw material A is selected from wood with an additive and / or resin acid content of 1%-50%; The additive is selected from one or more of resin acid, oleic acid, formic acid, acetic acid, lactic acid, oxalic acid, succinic acid, maleic acid, and rosin acid.

2. The preparation method according to claim 1, characterized in that: The biomass having a total content of cellulose and hemicellulose greater than 50% is selected from one or more of lychee wood, camphor wood, apricot wood, poplar wood, oak, elm wood, olive kernel, walnut shell, cotton, bamboo, bagasse, waste paper, and waste cotton yarn; The wood with a resin acid content of 1%-50% is selected from one or more of pine, fir, cypress and walnut.

3. The preparation method according to claim 1, characterized in that: The heating temperature in step 1) is 150°C-290°C.

4. The preparation method according to claim 1, characterized in that: In the step 1), the mass ratio of the biomass having a total cellulose and hemicellulose content greater than 50% to the raw material A is (0.1-100):

1.

5. The preparation method according to claim 1, characterized in that: When the raw material A in step 1) contains additives, the additives are 1%-50% of the mass of the biomass with a total content of cellulose and hemicellulose greater than 50%.

6. The preparation method according to claim 1, characterized in that: The additives also include solvents; The solvent is selected from one or more of ethanol, acetaldehyde, acetone and benzene.

7. The preparation method according to claim 1, characterized in that: The temperature of the carbonization in step 2) is 700°C-2000°C.

8. A hard carbon material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.

9. The hard carbon material according to claim 7, characterized in that The specific surface area of ​​the hard carbon material is 1-50 m 2 g -1 The total volume of open and closed pores is 0.001-0.12 cm 3 g -1 , the porosity is 1%-20%.

10. A lithium, sodium or potassium ion battery or capacitor, characterized in that: The hard carbon material according to claim 8 or 9 is used as the negative electrode material.

Citation Information

Patent Citations

  • Pyrolysis hard carbon material with longitudinal pore structure and preparation method and application thereof

    CN108315028A

  • Lignocellulose biomass-based hard carbon negative electrode material and preparation method thereof

    CN117613268A

  • Biomass hard carbon material, method for preparing biomass hard carbon material through pre-crosslinking modification and application of biomass hard carbon material

    CN118289738A

Cited By

  • Resin-based sodium ion battery hard carbon material and preparation method thereof

    CN119612494A