Acidification method of pseudo-boehmite as well as product and application of pseudo-boehmite

By controlling the acidification temperature and pH value, combined with the use of surfactants and polymers, nanoparticles with narrow particle size acidification phthalite was prepared, which solved the problems of incomplete acidification and poor stability in the prior art, and improved the catalyst performance and exhaust gas conversion rate.

CN119038583APending Publication Date: 2024-11-29FOSHAN LIPAI MOTORCYCLE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411157641.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing acidification methods of phthalidite have problems such as incomplete acidification, large acid consumption, wide particle size distribution, poor stability and high cost, and cannot effectively improve the performance of the catalyst.

Method used

An acidification method is adopted, including milling the pseudo-thin aluminite with deionized water balloons, adding cetyl trimethylammonium bromide to disperse, then heating to 47-53°C and adding dilute nitric acid solution, controlling the pH value to 2.8 ~3.2, add polyvinylpyrrolidone and polyvinyl alcohol to prepare nanoparticles with narrow particle size distribution to improve acidification and viscosity.

Benefits of technology

The acidified phthalite has high viscosity, large solid content and stable properties, which reduces acid consumption and preparation costs, and improves the performance of the catalyst and exhaust emission conversion rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005498170000121
    Figure BDA0005005498170000121
  • Figure BDA0005005498170000131
    Figure BDA0005005498170000131
  • Figure BDA0005005498170000132
    Figure BDA0005005498170000132
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of pseudo-boehmite, in particular to an acidification method of pseudo-boehmite as well as a product and application thereof. The acidification method of the pseudo-boehmite comprises the following steps that A, the pseudo-boehmite and deionized water are subjected to ball milling according to the volume ratio of 1: 1, cetyltrimethylammonium bromide is added to be ground and dispersed till the average particle size of the pseudo-boehmite is 2.5-3.5 micrometers, and the adding amount of the cetyltrimethylammonium bromide is 0.2% of the solid mass of the pseudo-boehmite; according to the acidification method of the pseudo-boehmite, the pseudo-boehmite can be acidified into nano-particles with narrower particle size distribution, so that the acidified pseudo-boehmite has the characteristics of high viscosity, high solid content, stable character and the like, the acidification is complete, the preparation cost is low, the acid consumption is low, and the method is suitable for industrial production. The technical problems that according to an existing acidification method of pseudo-boehmite, acidification is incomplete, acid consumption is large, particle size distribution is wide and can only reach the micron level, stability is poor, and cost is high are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pseudo-boehmite preparation, and in particular to an acidification method for pseudo-boehmite and a product and application thereof. Background Art

[0002] At present, various auto parts companies have begun to optimize materials, processes, production, etc., to reduce product costs as much as possible while having better performance. In the automotive field, there are two types of catalyst carriers: one is a metal carrier with iron, chromium, and aluminum as the main components, and the other is a cordierite ceramic carrier composed of magnesium, aluminum, and silicate. Regardless of which type of carrier the catalyst is coated on, an aluminum-containing gel is required as a high-temperature adhesive. One reason is that aluminum gel has high bonding strength, and the other is that it has the lowest cost. Currently, acidified pseudo-boehmite is commonly used as a high-temperature adhesive for vehicle exhaust treatment catalysts.

[0003] There are generally three types of preparation methods for acidified pseudo-boehmite: inorganic salt raw material method, powder dispersion acidification method and mixed dispersion acidification method. The inorganic salt raw material method requires the use of an alkaline precipitant to hydrolyze aluminum salts to form a precipitate, and then use acids to adjust the pH value. The disadvantages of this method are that the preparation cycle is long and the cost is relatively high. The powder dispersion acidification method is to add acid under high-speed dispersion conditions to form a thixotropic gel. The process is simple and the cost is low. The disadvantage is that it quickly agglomerates after being placed and has no stability. The mixed dispersion acidification method is to grind the pseudo-boehmite with the catalyst material and then acidify it under high-speed dispersion. It is also the current mainstream preparation method. The advantages are uniform dispersion, good stability and strong practicality. The disadvantages are incomplete acidification under the interference of other materials, large acid consumption, wide particle size distribution and can only reach the micron level, which cannot further improve the catalyst performance. Summary of the invention

[0004] In view of the problems raised by the background technology, the purpose of the present invention is to propose a method for acidifying pseudo-boehmite, which can acidify the pseudo-boehmite into nanoparticles with a narrow particle size distribution, so that the pseudo-boehmite has the characteristics of high viscosity, large solid content, stable properties, etc. after acidification. The acidification is complete, the preparation cost is low, and the acid consumption is small. The technical problems of the existing method for acidifying pseudo-boehmite, such as incomplete acidification, large acid consumption, wide particle size distribution that can only reach the micron level, poor stability and high cost, are solved.

[0005] Another object of the present invention is to provide an acidified pseudo-boehmite prepared by the above-described acidification method of pseudo-boehmite, which has the characteristics of high solid content, high viscosity, narrow particle size distribution, small particle size and good stability.

[0006] Another object of the present invention is to propose the use of acidified pseudo-boehmite prepared by the above-mentioned pseudo-boehmite acidification method in the preparation of automobile catalyst slurry. The use of acidified pseudo-boehmite in automobile catalyst slurry can greatly reduce the catalyst coating shedding rate. The acidified pseudo-boehmite has a large specific surface area and open porosity, which can effectively improve the catalyst performance and the exhaust emission conversion rate, thereby solving the problem that the existing acidified pseudo-boehmite cannot further improve the catalyst performance.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] A method for acidifying pseudo-boehmite comprises the following steps:

[0009] Step A, ball-milling pseudo-boehmite and deionized water in a volume ratio of 1:1, adding hexadecyltrimethylammonium bromide and grinding and dispersing until the average particle size of the pseudo-boehmite is 2.5-3.5 μm, and the amount of the hexadecyltrimethylammonium bromide added is 0.2% of the solid mass of the pseudo-boehmite;

[0010] Step B, quickly dispersing the mixed solution obtained by grinding in step A, heating it to 47-53° C., adding a dilute nitric acid solution, stopping adding the dilute nitric acid solution when the pH value of the mixed solution reaches 2.8-3.2, and continuing to quickly disperse the mixed solution until the D90 of the pseudo-boehmite in the mixed solution reaches 100-130 nm;

[0011] Step C, adding polyvinyl pyrrolidone and polyvinyl alcohol to the mixed solution, wherein the amount of polyvinyl pyrrolidone added is 0.2% of the solid mass of the pseudo-boehmite, and the amount of polyvinyl alcohol added is 12% of the solid mass of the pseudo-boehmite, and acidified pseudo-boehmite is obtained after dispersion.

[0012] To further illustrate, in step A, the volume ratio of pseudo-boehmite to deionized water is (97-103): (97-103).

[0013] To further illustrate, in step A, the volume ratio of pseudo-boehmite to deionized water is 1:1.

[0014] To further illustrate, in step B, rapid dispersion is performed under heating conditions in a water bath or an oil bath.

[0015] To further illustrate, in step B, the rotation speed for rapid dispersion is 1300-1440 r / min.

[0016] It is further explained that the dispersion time in step C is 5 to 10 minutes.

[0017] Further, the peptization index of the pseudo-boehmite is ≥95%, and the specific surface area is ≥240m 2 / g, loss on ignition ≤35%.

[0018] Acidified pseudo-boehmite is prepared by using the acidification method of pseudo-boehmite.

[0019] The invention discloses an application of the acidified pseudo-boehmite prepared by the pseudo-boehmite acidification method in the preparation of automobile catalyst slurry.

[0020] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:

[0021] 1. By heating to 47-53°C during the acidification process, the pseudo-boehmite has moderate activity at 47-53°C. The particle size distribution of the acidified pseudo-boehmite obtained at this heating temperature is narrow, the acidification rate is ≧95%, and the viscosity is 500-1500 centipoise higher than that of room temperature acidification.

[0022] 2. By controlling the process parameters and the pH value after acidification, the pseudo-boehmite is acidified into nanoparticles with a narrow particle size distribution. The nanoparticles are small in mass and high in viscosity, so they are not easy to stratify. By adding hexadecyltrimethylammonium bromide (CTAB), the cationic surfactant with positive charge is used to make the acidified pseudo-boehmite particles repel each other and prevent agglomeration. After adding 0.2% CTAB, the potential measured by the Zeta potential analyzer is in the range of 30-40mv. The non-ionic surfactant polyvinylpyrrolidone (PVP) is evenly distributed between the acidified pseudo-boehmite molecules after dissolution to balance the repulsion and attraction generated during the Brownian motion of the molecules. The reason for adding polyvinyl alcohol (PVA) is that the PVA solution contains a large number of hydroxyl groups, which form a large number of stable hydrogen bonds with water, and have good water retention at room temperature to ensure that there is no stratification. The present invention controls the pH after adding the dilute nitric acid solution in step B to be in the range of 2.8-3.2, so that the acidified pseudo-boehmite can achieve the characteristics of narrow distribution, nanoparticle level, and stable non-stratification. The particles are ground to a size of 2.5 to 3.5 μm before acidification, and the CTAB cationic surfactant added during grinding has a dispersing and anti-agglomeration effect. The particles after acidification cannot agglomerate into large particles under high-speed dispersion. After adding a dilute nitric acid solution and quickly dispersing, the particle size D90 of the pseudo-boehmite in the mixed solution can reach a nanometer range of 100 to 130 nm.

[0023] 3. Pseudo-boehmite is first acidified separately and then directly added as needed during the preparation of automobile catalyst slurry. The mixed dispersion acidification method is no longer used, thus avoiding the problem of poor stability when the mixture is prepared and used immediately.

[0024] 4. By acidifying the pseudo-boehmite separately and using heating to assist in increasing the acidification rate, no excessive nitric acid is added, and the amount of nitric acid used is reduced by 45-55%, effectively reducing costs. The solid content of the obtained acidified pseudo-boehmite is increased, and the solid content of the catalyst slurry is also increased, which is beneficial to the stability of the slurry viscosity and is conducive to coating use. A large batch can be prepared for multiple use, saving time and effort. DETAILED DESCRIPTION

[0025] A method for acidifying pseudo-boehmite comprises the following steps:

[0026] Step A, ball-milling pseudo-boehmite and deionized water in a volume ratio of 1:1, adding hexadecyltrimethylammonium bromide and grinding and dispersing until the average particle size of the pseudo-boehmite is 2.5-3.5 μm, and the amount of the hexadecyltrimethylammonium bromide added is 0.2% of the solid mass of the pseudo-boehmite;

[0027] Step B, quickly dispersing the mixed solution obtained by grinding in step A, heating it to 47-53° C., adding a dilute nitric acid solution, stopping adding the dilute nitric acid solution when the pH value of the mixed solution reaches 2.8-3.2, and continuing to quickly disperse the mixed solution until the D90 of the pseudo-boehmite in the mixed solution reaches 100-130 nm;

[0028] Step C, adding polyvinyl pyrrolidone and polyvinyl alcohol to the mixed solution, wherein the amount of polyvinyl pyrrolidone added is 0.2% of the solid mass of the pseudo-boehmite, and the amount of polyvinyl alcohol added is 12% of the solid mass of the pseudo-boehmite, and acidified pseudo-boehmite is obtained after dispersion.

[0029] The acidification method of pseudo-boehmite of the present invention has the following characteristics:

[0030] (1) Acidification heating and temperature control: The existing acidification method, the mixed dispersion acidification method, is carried out at room temperature. The acidification method of the pseudo-boehmite of the present invention needs to be heated to 47-53°C (i.e., heating is required during the acidification process of step B). The inventors have conducted experiments and found that when the heating temperature is higher than 60°C, the pseudo-boehmite has high activity and the acidification rate is too high, which easily makes the pseudo-boehmite particle size distribution wide and uneven. However, the activity of pseudo-boehmite at room temperature is relatively low, the reaction rate is too slow, and the acidification rate cannot reach the parameter value of 95%, and the high viscosity index cannot be achieved. Pseudo-boehmite has moderate activity at 47-53°C. The particle size distribution of the acidified pseudo-boehmite obtained at this heating temperature is narrow, the acidification rate is ≧95%, and the viscosity is 500-1500 centipoise higher than that of room temperature acidification.

[0031] (2) Process parameter control: Conventional aluminum gels currently used often control the acidified pH to a range of 0.5 to 1, with excessive nitric acid and a wide distribution of particle sizes in the micrometer range. The inventors first conducted experiments at pH = 2, 4, and 6. The results showed that when the pH was 6, a large amount of pseudo-boehmite was not acidified and precipitated when the acidification time and temperature remained unchanged. When the pH was 4, there was no obvious precipitate but the transparency was insufficient, there were also large suspended particles, and the particle size was not appropriate. When pH = 2, the pseudo-boehmite was completely acidified and transparent, and the particle size was small. After determining the pH range, the experiments were conducted again at pH = 2.5, 3.0, and 3.5. The pseudo-boehmite was acidified to be completely transparent, but it was obvious that the particle size distribution was the smallest and narrowest when the pH was about 3. Analyzing the test data, when the pH reached around 3 and the nitric acid solution was continued to be added, the diameter of the resulting particles no longer decreased, but began to gradually increase. During the entire acidification process, when the pH value is greater than 3 in the early stage, the white particles in the solution are visible to the naked eye. The large particle size and wide distribution are because the acidification is still in progress. The large particles are pseudo-boehmite that has not been completely acidified. When the pH reaches about 3, the white particles are no longer visible, and it is a translucent and slightly blue solution. At this time, the particle size is small and the distribution is narrow, and the dissolution equilibrium has been reached. When the pH reaches about 3 and the dilute nitric acid solution is continued to be added, the particle size is detected and found to begin to increase and the distribution becomes wider. This is because the pseudo-boehmite after acidification itself is a network structure. After continuing to add acid to reduce the pH value, cross-linking and agglomeration occur to form larger particle gel. Therefore, the widening of the particle size distribution during the test is due to the formation of a part of the gel in the solution.

[0032] Nanoparticles are small in mass and high in viscosity, so they are not easy to stratify. The present invention adds hexadecyltrimethylammonium bromide (CTAB) and utilizes this cationic surfactant with positive charge to make the acidified pseudo-boehmite particles repel each other and prevent agglomeration. After adding 0.2% CTAB, the potential measured by the Zeta potential analyzer is in the range of 30-40mv. The non-ionic surfactant polyvinylpyrrolidone (PVP) is evenly distributed between the acidified pseudo-boehmite molecules after dissolution, balancing the repulsion and attraction generated during the Brownian motion of the molecules. Polyvinyl alcohol (PVA) is added because the PVA solution contains a large number of hydroxyl groups, which form a large number of stable hydrogen bonds with water, and have good water retention at room temperature to ensure that there is no stratification. The present invention controls the pH after adding the dilute nitric acid solution in step B to be in the range of 2.8 to 3.2, so that the acidified pseudo-boehmite can achieve the characteristics of narrow distribution, nanoparticle level, and stable non-stratification.

[0033] In addition, in step A, a CTAB cationic surfactant is added as a dispersant in the grinding process, and a particle size test is performed after grinding. When the average particle size of the pseudo-boehmite is 2.5 to 3.5 μm, the grinding requirement is met. If the grinding is directly acidified before reaching the particle size, the surface of the pseudo-boehmite particles will be wrapped by the gel acidified first, and the interior cannot be completely acidified, thereby reducing the yield. Since the particles have been ground to a range of 2.5 to 3.5 μm before acidification, and the CTAB cationic surfactant added during grinding has a dispersing and anti-agglomeration effect, the acidified particles cannot agglomerate into large particles under high-speed dispersion. After adding a dilute nitric acid solution and quickly dispersing, the particle size D90 of the pseudo-boehmite in the mixed solution can reach a nanometer range of 100 to 130 nm. If the particle size D90 of the pseudo-boehmite in the mixed solution after dispersion in step B is higher than 100 to 130 nm, it is necessary to appropriately extend the dispersion time so that the remaining small amount of particles can be acidified before proceeding to the next step.

[0034] (3) Separate dispersion: Pseudo-boehmite is first acidified separately and then added directly as needed during the preparation of the automotive catalyst slurry. The mixed dispersion acidification method is no longer used, thus avoiding the problem of poor stability when the mixture is prepared and used immediately.

[0035] (4) Reduce costs: The presence of other materials in the mixed dispersion acidification method affects the acidification rate of pseudo-boehmite, and only excessive nitric acid can be added to ensure the acidification quality. The present invention acidifies the pseudo-boehmite alone and adopts heating to help improve the acidification rate. Excessive nitric acid is no longer added, so that the amount of nitric acid used is reduced by 45-55%. The solid content of the acidified pseudo-boehmite is increased, and the solid content of the catalyst slurry is also increased accordingly, which is beneficial to the stability of the slurry viscosity and is conducive to coating use. A large batch can be prepared for multiple uses, saving time and labor.

[0036] In the past, the pseudo-boehmite was acidified by mixing and dispersing with other catalyst materials at room temperature, but the acidification was incomplete. The present invention uses pseudo-boehmite as a raw material, grinds, disperses at high speed, adds dilute nitric acid under heating temperature conditions, and adds CTAB, PVP, and PVA to prepare acidified pseudo-boehmite that is highly practical, stable, and completely acidified, so that the pseudo-boehmite acidification rate reaches more than 95%, and the pseudo-boehmite is acidified into nanoparticles with a narrow particle size distribution, so that the pseudo-boehmite has the characteristics of high viscosity, large solid content, stable properties, etc. after acidification. Compared with the previous acidification method, the viscosity is increased by 500 to 1500 centipoise, and it can be used as a high-temperature adhesive with stable performance. After the viscosity is increased, it can be used in the later stage of automobile catalyst slurry slurrying to reduce the amount of acidified pseudo-boehmite by 2 to 4%, and can also achieve the target viscosity to increase the solid content of the slurry, which is conducive to coating and more environmentally friendly. After a large batch is produced at one time, it can be used multiple times.

[0037] Compared with the traditional aluminum gel, the narrow distribution nanometer particle acidified pseudo-boehmite prepared by the present invention has an acidification rate of 95% and a viscosity of 500-1500 centipoise higher than before due to the improved acidification process. It is added to the catalyst slurry in proportion and evenly dispersed before being coated on the carrier. The carrier is dried by heating to 100-120°C and the temperature is gradually raised to 500-600°C for calcination. At low temperature, the gas and water vapor generated by the decomposition of water, acid and organic active agent in the catalyst slurry coating are all volatilized away. At high temperature, the acidified pseudo-boehmite loses water and phase changes to generate γ-alumina to form a mesoporous structure. Because the acidification process of the present invention completely acidifies the pseudo-boehmite, the number of mesopores formed at high temperature increases. When the amount of the substance does not change, the number of mesopores increases, and the total specific surface area of ​​the acidified pseudo-boehmite increases. When the exhaust gas discharged by the engine passes through the catalyst coating, the probability of intermolecular contact increases, which is conducive to improving the exhaust gas emission conversion rate. The smaller the particle diameter, the smaller the mass of the particle itself, and it is not easy to precipitate and precipitate water, so the stability is higher. The acidified pseudo-boehmite prepared by the present invention is used in automobile catalyst slurry, which can greatly reduce the catalyst coating shedding rate. The acidified pseudo-boehmite has a large specific surface area and open porosity, which can effectively improve the catalyst performance and improve the tail gas emission conversion rate.

[0038] Preferably, in step A, the volume ratio of pseudo-boehmite to deionized water is (97-103): (97-103).

[0039] If too much pseudo-boehmite is added, the pseudo-boehmite will be difficult to disperse and the grinding time will be increased. If too much deionized water is added, the solid content will be reduced.

[0040] Preferably, in step A, the volume ratio of pseudo-boehmite to deionized water is 1:1.

[0041] Specifically, in the step A, pseudo-boehmite and deionized water are added into a ball mill in a volume ratio of 1:1 for ball milling.

[0042] To further illustrate, in step B, rapid dispersion is performed under heating conditions in a water bath or an oil bath.

[0043] Preferably, in step B, the rotation speed of rapid dispersion is 1300-1440 r / min.

[0044] The mixed solution is quickly dispersed to prevent solid precipitation and ensure that the temperature and concentration in the solution are balanced. Specifically, the mixed solution obtained by grinding in step A is quickly dispersed in a high-speed disperser, the mass fraction of the dilute nitric acid solution in step B is 20%, and the pH value of the mixed solution is monitored using a pH meter. When the pH value of the mixed solution reaches 2.8 to 3.2, the addition of the dilute nitric acid solution is stopped, and the rapid dispersion is continued for 20 to 30 minutes.

[0045] It is further explained that the dispersion time in step C is 5 to 10 minutes.

[0046] Agglomeration can be prevented by adding polyvinyl pyrrolidone (PVP) and polyvinyl alcohol (PVA) before dispersion.

[0047] Further, the mass fraction of polyvinyl alcohol in step C is 20%. In step C, the mass of polyvinyl alcohol needs to be weighed accurately to prevent excessive or insufficient addition from causing the total solid content of the finally obtained acidified pseudo-boehmite to fluctuate.

[0048] Further, the peptization index of the pseudo-boehmite is ≥95%, and the specific surface area is ≥240m 2 / g, loss on ignition ≤35%.

[0049] The pseudo-boehmite with this parameter has better adsorption performance, catalytic performance and stability.

[0050] Acidified pseudo-boehmite is prepared by using the acidification method of pseudo-boehmite.

[0051] The invention uses pseudo-boehmite as a raw material, grinds it, disperses it at a high speed under the heating condition of a water bath or an oil bath, adds a dilute nitric acid solution for acidification, monitors the pH value through a pH meter, and when the pH reaches 2.8-3.2, tests the particle size so that the D90 of the pseudo-boehmite in the mixed solution reaches 100-130nm, then adds PVP and PVA solutions for uniform dispersion, and obtains uniform and stable acidified pseudo-boehmite.

[0052] The acidified pseudo-boehmite prepared by the acidification method of the pseudo-boehmite of the present invention has a solid content of 29-31%, a viscosity of 15000-17000 cP, a particle size D90 of the pseudo-boehmite ≤130 nm, a water absorption rate of ≤6% after 30 days, a particle size D90 of the pseudo-boehmite ≤200 nm after 30 days, good colloid stability, and low raw material cost.

[0053] The invention discloses an application of the acidified pseudo-boehmite prepared by the pseudo-boehmite acidification method in the preparation of automobile catalyst slurry.

[0054] When the acidified pseudo-boehmite of the present invention is used in the preparation of automobile catalyst slurry, modified alumina loaded with metal oxides of platinum, palladium and rhodium, rare earth element composite oxides and polyethylene glycol are ground with water to form catalyst slurry, 4 to 20% of the acidified pseudo-boehmite is added according to the later carrier coating amount (80 to 220 g / L), and the slurry is evenly dispersed at high speed and coated on a metal or ceramic carrier.

[0055] The acidified pseudo-boehmite of the present invention is used in automobile catalyst slurry, which can greatly reduce the catalyst coating shedding rate. The acidified pseudo-boehmite has a large specific surface area and a high porosity, which can effectively improve the catalyst performance and the tail gas emission conversion rate. The catalyst coating shedding rate (550°C, 2h) is ≤1%, and the specific surface area of ​​the prepared acidified pseudo-boehmite is ≥210m 2 / g, when other auxiliary materials and working conditions remain unchanged, the tail gas emission conversion rate is increased by 4-7%. The national standard stipulates that the shedding rate of automobile catalyst products is less than 3%. After using the narrow distribution nanoparticle acidified pseudo-boehmite of the present invention as a high-temperature adhesive, the shedding rate is controlled within the range of 1%. The performance of the acidified pseudo-boehmite is reflected in the narrow distribution range, the particle diameter is nanometer-level, and the stability is good. The specific surface area of ​​the acidified pseudo-boehmite reaches 210m 2 / g or above.

[0056] In order to facilitate the understanding of the present invention, the present invention is described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0057] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0058] Example 1

[0059] A method for acidifying pseudo-boehmite comprises the following steps:

[0060] Step A, adding pseudo-boehmite and deionized water in a volume ratio of 1:1 into a ball mill for ball milling, adding hexadecyltrimethylammonium bromide to grind and disperse until the average particle size of the pseudo-boehmite is 2.5-3.5 μm, the amount of the hexadecyltrimethylammonium bromide added is 0.2% of the solid mass of the pseudo-boehmite, the peptization index of the pseudo-boehmite is ≥95%, and the specific surface area is ≥240m 2 / g, loss on ignition ≤35% (using high-viscosity pseudo-boehmite of model HV-D-03 produced by Shandong Shanlu Yifeng Aluminum-based New Materials Co., Ltd.);

[0061] Step B, the mixed solution obtained by grinding in step A is quickly dispersed in a high-speed disperser at a speed of 1400 r / min, heated to 50° C. in a water bath, and a dilute nitric acid solution (the mass fraction of the dilute nitric acid solution is 20%) is added, and the pH value of the mixed solution is monitored using a pH meter. When the pH value of the mixed solution reaches 3.0, the addition of the dilute nitric acid solution is stopped, and the rapid dispersion is continued for 30 minutes, so that the D90 of the pseudo-boehmite in the mixed solution reaches 100-130 nm;

[0062] Step C, adding polyvinyl pyrrolidone and polyvinyl alcohol (the mass fraction of polyvinyl alcohol is 20%) to the mixed solution, wherein the amount of polyvinyl pyrrolidone added is 0.2% of the solid mass of pseudo-boehmite, and the amount of polyvinyl alcohol added is 12% of the solid mass of pseudo-boehmite, and acidified pseudo-boehmite is obtained after dispersion for 5 minutes.

[0063] Example 2

[0064] A method for acidifying pseudo-boehmite comprises the following steps:

[0065] Step A, adding pseudo-boehmite and deionized water in a volume ratio of 1:1 into a ball mill for ball milling, adding hexadecyltrimethylammonium bromide to grind and disperse until the average particle size of the pseudo-boehmite is 2.5-3.5 μm, the amount of the hexadecyltrimethylammonium bromide added is 0.2% of the solid mass of the pseudo-boehmite, the peptization index of the pseudo-boehmite is ≥95%, and the specific surface area is ≥240m 2 / g, loss on ignition ≤35% (using high-viscosity pseudo-boehmite of model HV-D-03 produced by Shandong Shanlu Yifeng Aluminum-based New Materials Co., Ltd.).

[0066] Step B, the mixed solution obtained by grinding in step A is quickly dispersed in a high-speed disperser at a speed of 1300 r / min, heated to 47° C. in a water bath, and a dilute nitric acid solution (the mass fraction of the dilute nitric acid solution is 20%) is added, and the pH value of the mixed solution is monitored using a pH meter. When the pH value of the mixed solution reaches 3.0, the addition of the dilute nitric acid solution is stopped, and the rapid dispersion is continued for 30 minutes, so that the D90 of the pseudo-boehmite in the mixed solution reaches 100-130 nm;

[0067] Step C, adding polyvinyl pyrrolidone and polyvinyl alcohol (the mass fraction of polyvinyl alcohol is 20%) to the mixed solution, wherein the amount of polyvinyl pyrrolidone added is 0.2% of the solid mass of pseudo-boehmite, and the amount of polyvinyl alcohol added is 12% of the solid mass of pseudo-boehmite, and acidified pseudo-boehmite is obtained after dispersion for 10 minutes.

[0068] Example 3

[0069] A method for acidifying pseudo-boehmite comprises the following steps:

[0070] Step A, adding pseudo-boehmite and deionized water in a volume ratio of 1:1 into a ball mill for ball milling, adding hexadecyltrimethylammonium bromide to grind and disperse until the average particle size of the pseudo-boehmite is 2.5-3.5 μm, the amount of the hexadecyltrimethylammonium bromide added is 0.2% of the solid mass of the pseudo-boehmite, the peptization index of the pseudo-boehmite is ≥95%, and the specific surface area is ≥240m 2 / g, loss on ignition ≤35% (using P-DF-03-LS pseudo-boehmite from Shandong Naite Aluminum Co., Ltd.).

[0071] Step B, rapidly dispersing the mixed solution obtained by grinding in step A in a high-speed disperser at a speed of 1440 r / min, heating to 53° C. in a water bath, adding a dilute nitric acid solution (the mass fraction of the dilute nitric acid solution is 20%), and monitoring the pH value of the mixed solution using a pH meter. When the pH value of the mixed solution reaches 3.0, stop adding the dilute nitric acid solution, and continue to rapidly disperse for 30 minutes, so that the D90 of the pseudo-boehmite in the mixed solution reaches 100 to 130 nm;

[0072] Step C, adding polyvinyl pyrrolidone and polyvinyl alcohol (the mass fraction of polyvinyl alcohol is 20%) to the mixed solution, wherein the amount of polyvinyl pyrrolidone added is 0.2% of the solid mass of pseudo-boehmite, and the amount of polyvinyl alcohol added is 12% of the solid mass of pseudo-boehmite, and acidified pseudo-boehmite is obtained after dispersion for 10 minutes.

[0073] Example 4

[0074] Compared with Example 1, in step A of this example, pseudo-boehmite and deionized water are added into a ball mill at a volume ratio of 97:103 for ball milling, and the rest of the formula and preparation method are consistent with Example 1, thereby obtaining an acidified pseudo-boehmite.

[0075] Example 5

[0076] Compared with Example 1, in step A of this example, pseudo-boehmite and deionized water are added into a ball mill at a volume ratio of 103:97 for ball milling, and the rest of the formula and preparation method are consistent with Example 1, thereby obtaining an acidified pseudo-boehmite.

[0077] The following performance tests were performed on Examples 1 to 5, and the test methods and test results are as follows:

[0078] (1) Solid content test: The solid content of the acidified pseudo-boehmite obtained in Examples 1 to 5 was tested using the existing solid content test method. The test results are shown in Table 1 below:

[0079] Table 1 Solid content of acidified pseudo-boehmite of Examples 1 to 5

[0080]

[0081] (2) Water precipitation rate test: The acidified pseudo-boehmite obtained in Examples 1 to 5 was placed in a 100 ml colorimetric tube and covered with a lid to prevent water from volatilizing. The tube was left standing and observed regularly at 1 day, 7 days, 15 days, and 30 days. The amount of the supernatant liquid on the 30th day was recorded. The precipitation rate was calculated as (the amount of the supernatant liquid / 100)*100%. The test results are shown in Table 2 below:

[0082] Table 2 Water separation rate of acidified pseudo-boehmite of Examples 1 to 5

[0083]

[0084] (3) Viscosity stability test: After the acidified pseudo-boehmite obtained in Examples 1 to 5 was cooled to room temperature, the initial viscosity was tested using an NDJ-1 rotational viscometer. The viscosity was tested again after 24 hours, one week, 15 days, and 30 days. The test results are shown in Table 3 below:

[0085] Table 3 Viscosity stability test of Examples 1 to 5

[0086]

[0087] As shown in Example 1, the initial viscosity is 15000 centipoise. After 24 hours, the viscosity is still 15000 centipoise when tested again. After one week, the viscosity is still 15000 centipoise. The viscosity is 15250 centipoise when tested on the 15th day. The viscosity is 15500 centipoise when tested again on the 30th day. The transparency remains unchanged, which proves that it has good stability at room temperature and is easy to store.

[0088] (4) Particle size D90 stability test: The initial D90 of Examples 1 to 5, and the D90 after 24 h, 7 d, 15 d and 30 d of storage were tested using a nanoparticle size and Zeta potential analyzer. The test results are shown in Table 4 below:

[0089] Table 4 Viscosity stability test of Examples 1 to 5

[0090]

[0091] As shown in Example 1, the D90 of the obtained acidified pseudo-boehmite is 107.6nm. After being placed at room temperature for 24 hours, the D90 is still 113.2nm when tested again. After one week, the D90 is 118.3nm. The D90 is 119.2 when tested on the 15th day, and 126.6nm when tested again on the 30th day, which proves that the acidified pseudo-boehmite obtained by the present invention has good colloid stability. The particle size variation data of Examples 2 to 5 with the extension of storage time are tested respectively. As shown in the table above, the initial D90 of Examples 1 to 5 are all within the range of 100 to 130nm, and the particle size D90 of the pseudo-boehmite after 30 days is ≤200nm, which proves that the D90 stability of the obtained acidified pseudo-boehmite is good.

[0092] (5) Coating shedding rate test: Weigh three parts of the same weight of the automotive catalyst slurry containing modified alumina loaded with metal oxides of platinum, palladium, rhodium, rare earth element composite oxides, and polyethylene glycol, and add 4% of the acidified pseudo-boehmite prepared in Example 1 to the first part, 6% to the second part, and 8% to the third part. And coat three 58*100(90)300LS model carriers at a weight of 160 grams per liter, and conduct a shedding rate test using the ultrasonic oscillation method in Section 5.3.7 of the technical requirements for pollution control devices for gasoline vehicles of the group standard T / CAEPI 36.1-2021. The specific steps are as follows: 1. The constant weight mass m2 of the sample after the catalyst coating is subtracted from the constant weight mass m1 of the blank carrier to obtain the total coating amount Mtotal. 2. Place the sample in an ultrasonic cleaning machine, add deionized water to just completely submerge the sample, and ultrasonically oscillate for 10 minutes at a frequency of 40kHz and a water temperature of 25±5°C. 3. Take out the sample, dry it, and weigh it again to get the mass m3 of the sample after ultrasonic cleaning. 4. (m2-m3) / Mtotal*100% to get the shedding rate result. The shedding rate of the sample with 4% acidified pseudo-boehmite is 0.84%, the shedding rate of the sample with 6% acidified pseudo-boehmite is 0.74%, and the shedding rate of the sample with 8% acidified pseudo-boehmite is 0.67%. The experimental results confirm that the shedding rate decreases with the increase of the amount of acidified pseudo-boehmite added, and is far below the national standard upper limit of 3%.

[0093] (6) Example 1 Specific surface area test of acidified pseudo-boehmite: A fully automatic multi-station specific surface and pore analyzer was used to measure the specific surface area of ​​the solid substance using the gas adsorption BET method. The test result was 218.76 m 2 / g, the specific surface area of ​​the obtained acidified pseudo-boehmite is ≥210m 2 / g.

[0094] (7) Only the pH value parameter of step B in Examples 1 to 5 was changed, and the change of D90 under the change of pH value in step B of Examples 1 to 5 was tested to verify that the particle size of acidified pseudo-boehmite was the smallest when the pH was equal to 3. First, the three points of pH = 2, 4, and 6 were tested. The results showed that when pH = 6, a large amount of pseudo-boehmite was not acidified and precipitated when the acidification time and temperature remained unchanged. When pH = 4, there was no obvious precipitate but the transparency was not enough, there were larger suspended particles, and the particle size was not appropriate. At pH = 2, it was completely acidified and transparent, and the particle size was small. After determining the pH range, the results of pH = 2.5, 3.0, and 3.5 were obtained again, showing that they were all acidified to be completely transparent, but the particle size was the smallest when the pH was obviously around 3.

[0095] The pH parameter of step B in Examples 1 to 5 was changed to 2.0, and comparative examples a1, a2, a3, a4 and a5 were obtained respectively. The particle size test results are shown in Table 5 below:

[0096] Table 5 Particle size test results at pH 2

[0097] Test items D10(nm) D50(nm) D90(nm) Comparative Example a1 32.5 54.3 90.5 Comparative Example a2 35.6 63.9 114.7 Comparative Example a3 37.1 66.7 120.0 Comparative Example a4 37.0 68.8 127.8 Comparative Example a5 34.5 67.9 136.2

[0098] The pH parameter of step B in Examples 1 to 5 was changed to 2.5, and comparative examples b1, b2, b3, b4 and b5 were obtained respectively. The particle size test results are shown in Table 6 below:

[0099] Table 6 Particle size test results at pH 2.5

[0100] Test items D10(nm) D50(nm) D90(nm) Comparative Example b1 39.2 58.7 87.8 Comparative Example b2 38.8 60.0 92.8 Comparative Example b3 39.9 66.2 110.0 Comparative Example b4 40.9 68.4 114.5 Comparative Example b5 42.0 74.6 132.6

[0101] The particle size test results when the pH value parameter of step B in Examples 1 to 5 is 3.0 are shown in Table 7 below:

[0102] Table 7 Particle size test results at pH 3.0

[0103]

[0104]

[0105] The pH parameter of step B in Examples 1 to 5 was changed to 3.5, and comparative examples c1, c2, c3, c4 and c5 were obtained respectively. The particle size test results are shown in Table 8 below:

[0106] Table 8 Particle size test results at pH 3.5

[0107] Test items D10(nm) D50(nm) D90(nm) Comparative Example c1 37.2 65.5 115.5 Comparative Example c2 36.6 65.9 119.0 Comparative Example c3 34.0 64.9 123.1 Comparative Example c4 38.6 73.9 141.6 Comparative Example c5 37.3 77.7 162.2

[0108] The pH parameter of step B in Examples 1 to 5 was changed to 4.0, and comparative examples d1, d2, d3, d4 and d5 were obtained respectively. The particle size test results are shown in Table 9 below:

[0109] Table 9 Particle size test results at pH 4.0

[0110]

[0111]

[0112] The pH parameter of step B in Examples 1 to 5 was changed to 6.0, and comparative examples e1, e2, e3, e4 and e5 were obtained respectively. The particle size test results are shown in Table 10 below:

[0113] Table 10 Particle size test results at pH 6.0

[0114] Test items D10(nm) D50(nm) D90(nm) Comparative Example e1 99.0 119.1 144.3 Comparative Example e2 114.9 141.1 172.8 Comparative Example e3 159.5 200.4 250.2 Comparative Example e4 173.8 226.6 296.0 Comparative Example e5 198.8 276.0 381.9

[0115] (8) Particle size distribution comparison test: Acidified pseudo-boehmite was prepared by mixed dispersion acidification method. High-viscosity pseudo-boehmite, modified alumina loaded with metal oxides of platinum, palladium and rhodium, rare earth composite oxides, and polyethylene glycol were mixed and ground, and then acidification was completed by adding dilute nitric acid under high-speed dispersion conditions. The acidified pseudo-boehmite prepared by mixed dispersion acidification method was compared with the acidified pseudo-boehmite prepared in Example 1. The test equipment used a nanoparticle size and ZETA potential analyzer. The test was carried out with reference to the standard GBT 38431-2019 static multiple light scattering method. Test steps: put the sample material into a clean sample cell and seal it, turn on the nanoparticle size analyzer for preheating for more than 30 minutes, put the sample cell into the equipment and keep it at a constant temperature for 5 minutes, and then measure it, and record and save at least 3 test results. The particle size distribution span is the data of the left starting point and right landing point of the parabola on the coordinate axis of the curve graph. The particle size distribution of aluminum colloid obtained by the mixed dispersion method is mainly in the range of 550 nanometers to 2500 nanometers, and the distribution span reaches 2000 nanometers. The particle size distribution of narrow-distribution nanoparticle acidified pseudo-boehmite is mainly between 10 nanometers and 200 nanometers, and the distribution span is about 200 nanometers. Therefore, the particle size distribution span of the acidified pseudo-boehmite obtained by the present invention is narrow.

[0116] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for acidifying pseudo-boehmite, characterized in that: The following steps are involved: Step A, ball-milling pseudo-boehmite and deionized water in a volume ratio of 1:1, adding hexadecyltrimethylammonium bromide and grinding and dispersing until the average particle size of the pseudo-boehmite is 2.5-3.5 μm, and the amount of the hexadecyltrimethylammonium bromide added is 0.2% of the solid mass of the pseudo-boehmite; Step B, quickly dispersing the mixed solution obtained by grinding in step A, heating it to 47-53° C., adding a dilute nitric acid solution, stopping adding the dilute nitric acid solution when the pH value of the mixed solution reaches 2.8-3.2, and continuing to quickly disperse the mixed solution until the D90 of the pseudo-boehmite in the mixed solution reaches 100-130 nm; Step C, adding polyvinyl pyrrolidone and polyvinyl alcohol to the mixed solution, wherein the amount of polyvinyl pyrrolidone added is 0.2% of the solid mass of the pseudo-boehmite, and the amount of polyvinyl alcohol added is 12% of the solid mass of the pseudo-boehmite, and the acidified pseudo-boehmite is obtained after uniform dispersion.

2. The acidification method of pseudo-boehmite according to claim 1, characterized in that: In the step A, the volume ratio of pseudo-boehmite to deionized water is (97-103): (97-103).

3. The acidification method of pseudo-boehmite according to claim 2, characterized in that: In the step A, the volume ratio of pseudo-boehmite to deionized water is 1:

1.

4. The acidification method of pseudo-boehmite according to claim 1, characterized in that: In the step B, the mixture is rapidly dispersed under heating conditions in a water bath or an oil bath.

5. The acidification method of pseudo-boehmite according to claim 1, characterized in that: In the step B, the rotation speed of the rapid dispersion is 1300-1440 r / min.

6. The acidification method of pseudo-boehmite according to claim 1, characterized in that: The dispersion time in step C is 5 to 10 minutes.

7. The acidification method of pseudo-boehmite according to claim 1, characterized in that: The peptization index of the pseudo-boehmite is ≥95%, and the specific surface area is ≥240m 2 / g, loss on ignition ≤35%.

8. An acidified pseudo-boehmite, characterized in that: The method is prepared by using the acidification method of pseudo-boehmite as described in any one of claims 1 to 7.