Preparation method of biodegradable antibacterial hot melt adhesive
Through the esterification and polycondensation methods of end carboxylic flexible random copolyester and end hydroxy rigid block polyester, combined with inorganic antibacterial components, the problem of insufficient antibacterial properties of hot melt adhesives in the medical industry is solved, and biodegradable antibacterials is achieved The preparation of hot melt adhesive has excellent antibacterial properties and composting degradation properties, reducing environmental pollution and energy waste.
Patent Information
- Application Number
- CN202310608394.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-27
- Publication Date
- 2024-11-29
AI Technical Summary
The existing hot melt adhesives lack antibacterial properties in the medical industry, and the application of biodegradable materials in the hot melt adhesive field is insufficient, resulting in environmental pollution and energy waste.
Using the esterification and polycondensation method of end carboxylic flexible random copolyester and end hydroxy rigid block polyester, combined with inorganic antibacterial components, a biodegradable antibacterial hot melt adhesive has biodegradable and diverse forms. The advantages of no environmental pollution, high-efficiency and long-term antibacterial effects.
The prepared hot melt adhesive has excellent antibacterial properties and composting degradation properties, avoids environmental pollution and energy waste, is suitable for discarded packaging in the medical industry, and has a low cost.
Smart Images

Figure CN119039920A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a hot melt adhesive, and in particular to a method for preparing a biodegradable antibacterial hot melt adhesive. Background Art
[0002] Hot melt adhesive is an environmentally friendly solvent-free solid adhesive with a solid content of 100%. It melts at the operating temperature and becomes a fluid adhesive, which acts as an adhesive after re-solidification. Because of its advantages such as easy use, no volatile organic compounds, and a wide range of applications, it has become the mainstream adhesive in industries such as packaging production lines, disposable products, and medical sterilization packaging. As it is mostly used in the field of disposable products that are discarded after use, its biodegradability has been increasingly valued, but its antibacterial properties have rarely been valued. In fact, these industries, especially disposable packaging in the medical industry, have antibacterial needs.
[0003] Although hot melt adhesive itself does not contain toxic organic solvents and volatile organic compounds compared to other adhesives, there is still a lot of room for improvement. With the development of science and technology and social progress, environmentally friendly biodegradable materials have attracted more and more attention from the international community, especially disposable packaging and other products. The polymers usually used have extremely strong stability. Landfill treatment will exist in the natural environment for hundreds or thousands of years, and incineration treatment will produce dioxins and cause energy waste. Therefore, its disposable nature will cause irreversible harm to the environment. In recent years, biodegradable materials have emerged. In addition to bio-based PLA and petroleum-based PBAT, common biodegradable materials also include easily overlooked aliphatic polyesters, copolyesters, polypropylene carbonate and other environmentally friendly polymers that can be completely decomposed into water and carbon dioxide. At present, the application areas of biodegradable materials are mainly concentrated in the plastic market, the glass transition temperature of the latter does not match, but in the field of hot melt adhesives, it may be able to play its inherent characteristics and functions.
[0004] Research in the field of degradable hot melt adhesives is a current hot topic. Chinese patent CN112300747A discloses a polyester amide degradable hot melt adhesive, which includes 40-60 parts by weight of thermoplastic starch, 20-50 parts by weight of benzyl plant fiber and 80-120 parts by weight of polyester amide, and has excellent waterproof effect, but its degradation performance has not been evaluated; Chinese patent CN108841352A discloses a biodegradable polylactic acid hot melt adhesive, which includes 20-80 parts by weight of polylactic acid, 0.5-40 parts by weight of toughening resin and 5-70 parts by weight of tackifying resin, but the materials used are finished products, which may increase costs in industrial production; Chinese patent CN106800906 B discloses a biodegradable polypropylene carbonate hot melt adhesive, including 100 parts by weight of polypropylene carbonate, 3-30 parts by weight of a biodegradable plasticizer, 5-30 parts by weight of a tackifying resin, 0.3-0.6 parts by weight of a thermal stabilizer and 0-0.6 parts by weight of an antioxidant. When the molecular weight is less than 50,000, it has good bonding properties and thermal stability. However, the preparation method of polypropylene materials has never been disclosed, and there is also the problem of lack of degradation testing.
[0005] There are two methods for preparing polyester hot melt adhesives: biological fermentation and chemical synthesis. The polyester obtained by biological fermentation has a large molecular weight, but the cost is high and it is not suitable for large-scale industrial production. The chemical synthesis method is not only low-cost, but also allows the molecules to be designed during the synthesis process to obtain polyester with a narrow molecular weight distribution coefficient. However, in the polycondensation process of the chemical synthesis method, untimely water separation and catalyst selection will affect the increase in the molecular weight of the product. In the later stage, when the high-temperature polycondensation exceeds 200°C, it is often accompanied by side reactions such as thermal degradation, decarboxylation, and thermal oxidation. As a result, a large amount of time is invested to obtain the ideal high-molecular-weight polyester, which will further affect the performance of the hot melt adhesive product. Summary of the invention
[0006] In view of the shortcomings of the existing methods and the above-mentioned technologies, according to an embodiment of the present invention, it is intended to provide a method for preparing a biodegradable antibacterial hot melt adhesive that effectively combines soft and hard segment adjustment, hydroxyl and carboxyl end-capping, and antibacterial functions. The prepared hot melt adhesive has the advantages of being biodegradable, having diverse product forms, a wide range of uses, no environmental pollution, and having high efficiency and long-lasting antibacterial properties.
[0007] To achieve the above objectives, the present invention provides a method for preparing a biodegradable antibacterial hot melt adhesive, comprising the following steps:
[0008] (1) preparing carboxyl-terminated flexible random copolyester A;
[0009] (2) preparing a hydroxyl-terminated rigid block polyester B;
[0010] (3) Esterification and polycondensation of A and B;
[0011] (4) Mixing and discharging the inorganic antibacterial component.
[0012] Furthermore, step (1) is specifically as follows:
[0013] (1.1) 130-170 parts of 1,4-butanediol, 50-70 parts of adipic acid, and 20-30 parts of terephthalic acid are mixed and added to an esterification reaction kettle, the temperature is raised to 150-170° C., 0.05-0.2% by weight of a catalyst of the total reactants is added, and the esterification reaction is carried out at 300-500 Pa for 1-3 hours;
[0014] (1.2) After monitoring that almost no water is distilled out, the reaction is terminated and the flexible random copolyester A is obtained.
[0015] Preferably, the catalyst in step (1) is at least one of tetrabutyl titanate, stannous chloride and antimony trioxide.
[0016] Furthermore, step (2) is specifically as follows:
[0017] (2.1) Add 80-120 parts of 6-caprolactone, 0.01-0.04 parts of diethylene glycol, and 0.01-0.04 parts of a catalyst into an esterification reaction kettle, raise the temperature to 110-130° C., and carry out an esterification reaction at 100-150 Pa for 2-4 hours. When the water output reaches more than 95% of the theoretical value, the reaction is terminated and the hydroxy-terminated caprolactone prepolymer is obtained;
[0018] (2.2) The temperature in the reactor containing 200-250 parts of lactic acid and 0.01-0.05 parts of catalyst is raised to 80-120°C, the vacuum degree is 500-1000Pa, and the dehydration reaction is carried out for 1-3 hours, during which the reduced pressure distillation is promoted to promote the positive reaction. The temperature is raised to 150-190°C, the vacuum degree is 1000-2000Pa, and the depolymerization reaction is carried out for 1-2 hours to obtain lactide;
[0019] (2.3) Add the terminal hydroxyl caprolactone prepolymer, lactide, and 0.05-0.1 part of antioxidant into a polycondensation reaction kettle, raise the temperature to 210-240°C, and carry out a polycondensation reaction at 300-700 Pa for 0.5-1.5 h to obtain a carboxyl-terminated rigid block polyester B.
[0020] Preferably, the catalyst in step (2) is at least one of scandium trifluoromethanesulfonate, titanium glycolate, antimony glycolate, antimony acetate, stannous chloride, tin tetrachloride, and zinc chloride. The antioxidant is at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris[2.4-di-tert-butylphenyl]phosphite, and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl alcohol.
[0021] Furthermore, step (3) is specifically as follows:
[0022] (3.1) Add the prepared carboxyl-terminated flexible random copolyester A and hydroxyl-terminated rigid block polyester B into a reaction kettle at a mass ratio of 1.1-1.3, add a catalyst, raise the temperature to 130-150° C., and carry out esterification reaction at 300-500 Pa. When the monitored water output reaches more than 95% of the theoretical value, stop the reaction;
[0023] (3.2) After nitrogen is passed through, an antioxidant is added, the pressure is reduced to below 100 Pa, and the polycondensation reaction is carried out at 220-240°C. The power of the agitator increases with the molecular weight of the polymer, and polymers of different viscosities are obtained.
[0024] Preferably, the catalyst in step (3) is at least one of dibutyltin laurate, stannous octoate, p-toluenesulfonic acid, and tetraisobutyl titanate. The antioxidant is at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tris[2.4-di-tert-butylphenyl]phosphite, and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.
[0025] Furthermore, step (4) is specifically as follows:
[0026] (4.1) The polymer obtained in step (3) is immediately transferred into an internal mixer preheated to 100-130°C and mixed at a speed of 30-60 r / min for 5 min;
[0027] (4.2) Add 10-20% of the total mass of the polymer of a degradable tackifier, a degradable plasticizer, and an inorganic antibacterial agent, and continue stirring for 20-50 minutes before producing a glue.
[0028] Preferably, the degradable tackifier in step (4) is at least one of rosin, polymerized rosin glycerol ester, terpene resin, and coumarone resin. The degradable plasticizer is at least one of triethyl citrate, tributyl citrate, and castor oil. The inorganic antibacterial agent is at least one of nano silver (AGP-ZP003, particle size 15nm), nano copper (HCU-P100, particle size > 200nm), and nano zinc oxide (ZNO-P100, particle size 20-30nm) produced by Shanghai Huzheng Industrial Co., Ltd.
[0029] Compared with the prior art, the preparation of the biodegradable antibacterial hot melt adhesive of the present invention includes the preparation, esterification and polycondensation of two degradable thermoplastic materials, namely, carboxyl-terminated flexible random copolyester and hydroxyl-terminated rigid block polyester, and further filling of antibacterial functional materials to produce glue. The inorganic antibacterial material not only avoids environmental pollution, but also has a theoretical permanent antibacterial effect. The prepared adhesive can be further processed into various forms such as rubber blocks, rubber sticks, rubber particles, and rubber films, and is widely used in the fields of industry, books, clothing, shoe materials, medical packaging, etc. The industrial production process is solvent-free, avoiding VOCS pollution and water pollution. The prepared hot melt adhesive has excellent bonding properties and also has an antibacterial effect, avoiding bacterial contamination of items in sealed packages, and is particularly suitable for disposable packaging in the medical industry.
[0030] Compared with the prior art, the system of the biodegradable antibacterial hot melt adhesive of the present invention includes soft segment polyester and hard segment polyester, which overcomes the defect of poor mechanical properties of traditional hot melt adhesives. The terminal hydroxyl and terminal carboxyl groups of the two polyesters are of high purity, and with the assistance of antioxidants, side reactions such as decarboxylation, thermal degradation, and thermal oxidation are avoided in the subsequent esterification and polycondensation processes.
[0031] The colloid prepared by the present invention can be further processed into hot melt adhesive blocks by extrusion, processed into hot melt adhesive rods by extrusion and cooling, processed into hot melt adhesive particles by granulation, and processed into hot melt adhesive films by casting or calendering.
[0032] Compared with the prior art, the present invention has the following advantages:
[0033] (1) The overall formula used in the present invention is reasonable, the equipment is simple, the operation is basic, there is no solvent, no environmental pollution risk, and the production and molding processing surplus and scraps can be recycled and reused. The esterification, polycondensation, mixed extrusion and other technologies involved are the mainstream preparation methods in the current chemical industry, which are easy to operate, economical and efficient, and have universal applicability in mass production.
[0034] (2) The present invention synthesizes polymers of different molecular weights by reacting two end-capped polyesters under different temperature, pressure, catalyst and time conditions. The obtained hot melt adhesive can be used in scenarios with different viscosity requirements.
[0035] (3) The biodegradable antibacterial hot melt adhesive prepared by the present invention has excellent antibacterial properties and compost degradation properties, will not degrade under the conditions of use, and has high added value such as safety, environmental protection, and stability.
[0036] (4) The hot melt adhesive prepared by the present invention has good mechanical properties and biodegradability, with a softening point of 50-70°C, a working temperature of 130-150°C, an intrinsic viscosity of 0.8-1.2 dL / g, a melt viscosity of 2000-4000 cps, and does not degrade under normal use conditions. It can be degraded under composting conditions, and the degradation time can be adjusted according to the preparation process and molecular weight, thereby avoiding the defects of starch-based biodegradable hot melt adhesives on the market, such as poor weather resistance, thermal oxidation degradation, and poor mechanical properties.
[0037] (5) The hot melt adhesive prepared by the present invention adopts a step-by-step method to prepare two types of polyesters, alcohol-terminated and ester-terminated, thereby avoiding the problems of complex reactions and the generation of by-products in the subsequent esterification and polycondensation processes, and directional design of high-purity hot melt adhesives.
[0038] (6) The cost of the raw materials of the biodegradable hot melt adhesive prepared by the method of the present invention is about RMB 7,000-12,000 / ton, which is lower than the common PLA and PBAT biodegradable materials on the market. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the esterification route of carboxyl-terminated flexible random copolyester A.
[0040] Figure 2 Route for the depolymerization and ring-opening polymerization of hydroxyl-terminated rigid block polyester B from 6-caprolactone and lactic acid.
[0041] Figure 3 This is the esterification and polycondensation route of copolyester A and polyester B. DETAILED DESCRIPTION
[0042] The following is combined with Figure 1-3 The present invention is further described with specific embodiments. These embodiments should be understood to be only used to illustrate the present invention and not to limit the protection scope of the present invention. After reading the contents described in the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent changes and modifications also fall within the scope defined by the claims of the present invention.
[0043] The raw materials used in the following examples of the present invention are not particularly limited in their sources and can be purchased from the market or prepared according to conventional methods well known to those skilled in the art.
[0044] Example 1
[0045] (1) Preparation of carboxyl-terminated flexible random copolyester A:
[0046] (1.1) Weigh 130 g of 1,4-butanediol, 50 g of adipic acid, and 20 g of terephthalic acid, mix them evenly, and add them to an esterification reactor. Heat the reactor to 150°C, add 0.1 g of tetrabutyl titanate, and carry out the esterification reaction at 300 Pa for 3 h.
[0047] (1.2) After monitoring that almost no water is distilled out, the reaction is terminated and the flexible random copolyester A is obtained.
[0048] (2) Preparation of hydroxyl-terminated rigid block polyester B:
[0049] (2.1) 80 g of 6-caprolactone, 0.01 g of diethylene glycol, and 0.01 g of titanium glycolate catalyst were added to an esterification reaction kettle, the temperature was raised to 110° C., and the esterification reaction was carried out at 150 Pa for 4 h. When the water output reached more than 95% of the theoretical value, the reaction was terminated and the terminal hydroxyl caprolactone prepolymer was obtained;
[0050] (2.2) The temperature in the reactor containing 200g lactic acid and 0.01g zinc chloride was raised to 80°C, the vacuum degree was 1000Pa, and the dehydration reaction was carried out for 3h, during which the reduced pressure distillation promoted the forward reaction. Then the temperature was raised to 190°C, the vacuum degree was 2000Pa, and the depolymerization reaction was carried out for 2h to obtain lactide;
[0051] (2.3) Add terminal hydroxyl caprolactone prepolymer, lactide, and 0.05 g of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] into a polycondensation reaction kettle, raise the temperature to 210°C, and carry out a polycondensation reaction at 700 Pa for 1.5 hours to obtain terminal carboxyl rigid block polyester B.
[0052] (3) Esterification and polycondensation of copolyester A and polyester B:
[0053] (3.1) 200 g of carboxyl-terminated flexible random copolyester A and 220 g of hydroxyl-terminated rigid block polyester B were added to a reaction kettle, 0.4 g of dibutyl tin laurate was added, the temperature was raised to 130° C., and the esterification reaction was carried out at 500 Pa. The reaction was stopped when the monitored water output reached more than 95% of the theoretical value;
[0054] (3.2) After nitrogen was introduced, 0.2 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate was added, the pressure was reduced to 80 Pa again, and a polycondensation reaction was carried out at 220°C.
[0055] (4) Mixing and discharging of inorganic antibacterial components:
[0056] (4.1) The polymer obtained in step (3) was immediately transferred into an internal mixer preheated to 130°C and mixed at a speed of 30 r / min for 5 min;
[0057] (4.2) Add 23g of rosin tackifier, 20g of triethyl citrate plasticizer, and 1g of nanosilver (AGP-ZP003, 15nm) antibacterial agent, continue stirring for 20min and then produce glue.
[0058] Example 2
[0059] (1) Preparation of carboxyl-terminated flexible random copolyester A:
[0060] (1.1) Weigh 150 g of 1,4-butanediol, 60 g of adipic acid, and 30 g of terephthalic acid, mix them evenly, and add them into an esterification reaction kettle. Heat the mixture to 160°C, add 0.24 g of stannous chloride catalyst, and carry out esterification reaction at 500 Pa for 1 h.
[0061] (1.2) After monitoring that almost no water is distilled out, the reaction is terminated and the flexible random copolyester A is obtained.
[0062] (2) Preparation of hydroxyl-terminated rigid block polyester B:
[0063] (2.1) 100 g of 6-caprolactone, 0.03 g of diethylene glycol, and 0.03 g of scandium trifluoromethanesulfonate catalyst were added to an esterification reaction kettle, the temperature was raised to 115° C., and the esterification reaction was carried out at 135 Pa for 3 h. When the water output reached more than 95% of the theoretical value, the reaction was terminated and the terminal hydroxyl caprolactone prepolymer was obtained;
[0064] (2.2) The temperature in the reactor containing 220 g lactic acid and 0.04 g stannous chloride catalyst was raised to 100°C, the vacuum degree was 800 Pa, and the dehydration reaction was carried out for 2 hours, during which the reduced pressure distillation promoted the forward reaction. The temperature was raised to 170°C, the vacuum degree was 1800 Pa, and the depolymerization reaction was carried out for 2 hours to obtain lactide;
[0065] (2.3) Add terminal hydroxyl caprolactone prepolymer, lactide, and 0.08 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate octadecyl ester into a polycondensation reaction kettle, heat to 230°C, and carry out polycondensation reaction at 500 Pa for 1 hour to obtain terminal carboxyl rigid block polyester B.
[0066] (3) Esterification and polycondensation of copolyester A and polyester B:
[0067] (3.1) 240 g of carboxyl-terminated flexible random copolyester A and 290 g of hydroxyl-terminated rigid block polyester B were added to a reaction kettle, 0.6 g of p-toluenesulfonic acid catalyst was added, the temperature was raised to 140° C., and the esterification reaction was carried out at 400 Pa. The reaction was stopped when the monitored water output reached more than 95% of the theoretical value;
[0068] (3.2) After nitrogen was introduced, 0.3 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate was added, the pressure was reduced to 90 Pa again, and a polycondensation reaction was carried out at 230°C.
[0069] (4) Mixing and discharging of inorganic antibacterial components:
[0070] (4.1) The polymer obtained in step (3) was immediately transferred into an internal mixer preheated to 120°C and mixed at a speed of 50 r / min for 5 min;
[0071] (4.2) Add 24 g of terpene resin tackifier, 19 g of tributyl citrate plasticizer, and 2 g of nano copper (HCU-P100, >200 nm) antibacterial agent, continue stirring for 40 min, and then produce glue.
[0072] Example 3
[0073] (1) Preparation of carboxyl-terminated flexible random copolyester A:
[0074] (1.1) Weigh 170 g of 1,4-butanediol, 70 g of adipic acid, and 30 g of terephthalic acid, mix them evenly, and add them into an esterification reaction kettle. Heat the mixture to 170°C, add 0.3 g of antimony trioxide catalyst, and carry out esterification reaction at 400 Pa for 2 h.
[0075] (1.2) After monitoring that almost no water is distilled out, the reaction is terminated and the flexible random copolyester A is obtained.
[0076] (2) Preparation of hydroxyl-terminated rigid block polyester B:
[0077] (2.1) 120 g of 6-caprolactone, 0.04 g of diethylene glycol, and 0.04 g of ethylene glycol antimony catalyst were added to an esterification reaction kettle, the temperature was raised to 130° C., and the esterification reaction was carried out at 140 Pa for 4 h. When the water output reached more than 95% of the theoretical value, the reaction was terminated and the terminal hydroxyl caprolactone prepolymer was obtained;
[0078] (2.2) The temperature in the reactor containing 250g lactic acid and 0.05g tin tetrachloride catalyst was raised to 120°C, the vacuum degree was 900Pa, and the dehydration reaction was carried out for 3h, during which the reduced pressure distillation promoted the forward reaction. The temperature was raised to 190°C, the vacuum degree was -2000Pa, and the depolymerization reaction was carried out for 1h to obtain lactide;
[0079] (2.3) Add terminal hydroxyl caprolactone prepolymer, lactide, and 0.1 g of tri[2,4-di-tert-butylphenyl]phosphite into a polycondensation reaction kettle, raise the temperature to 240°C, and carry out a polycondensation reaction at 700 Pa for 1.5 hours to obtain terminal carboxyl rigid block polyester B.
[0080] (3) Esterification and polycondensation of copolyester A and polyester B:
[0081] (3.1) 270 g of carboxyl-terminated flexible random copolyester A and 350 g of hydroxyl-terminated rigid block polyester B were added to a reactor, tetraisobutyl titanate catalyst was added, the temperature was raised to 150° C., and the esterification reaction was carried out at 500 Pa. The reaction was stopped when the monitored water output reached more than 95% of the theoretical value;
[0082] (3.2) After nitrogen was introduced, 0.3 g of tris[2,4-di-tert-butylphenyl]phosphite was added, the pressure was reduced to below 100 Pa again, and a polycondensation reaction was carried out at 240°C.
[0083] (4) Mixing and discharging of inorganic antibacterial components:
[0084] (4.1) The polymer obtained in step (3) was immediately transferred into an internal mixer preheated to 130°C and mixed at a speed of 50 r / min for 5 min;
[0085] (4.2) Add 60g of coumarone resin tackifier, 60g of castor oil biodegradable plasticizer, and 4g of nano zinc oxide (ZNO-P100, 20-30nm) inorganic antibacterial agent, continue stirring for 20-50min and then produce glue.
[0086] Test Example 1
[0087] Referring to Section 7.1.2 of GB / T 22235-2008, the melt viscosity of the examples was tested by the rotational viscometer method. 500 ml of pre-melted examples 1 to 3 were respectively put into the barrel of the viscometer, kept at the working temperature (130-150° C.) for 5 minutes, and the reading was taken after the rotor rotated for 30-60 seconds.
[0088] With reference to Part 5 of GB / T 16998-1997, the thermal stability of the hot melt adhesive was measured. The samples of Example 1 to Example 3 were heated at the melting temperature for 2 hours to reach thermal equilibrium. Samples were taken every 2 hours to observe the phase separation.
[0089] Referring to Section 5.1 of GB / T 15332-1994, fill the container with distilled water at a temperature 10°C lower than the estimated softening point, with the water surface 50mm higher than the sample ring. After keeping the temperature constant for 15 minutes, place a steel ball at the same temperature on the positioning ring, and evenly raise the temperature by 5±1°C until the steel ball enters the sample. Record the temperature when the steel ball touches the lower support plate of the ring frame, which is the softening point of the embodiment.
[0090] The test results of melt viscosity, thermal stability and softening point of Examples 1-3 are recorded in Table 1.
[0091] Table 1
[0092] Melt viscosity cps Thermal stability Softening point℃ Example 1 2147 No phase separation 59 Example 2 4021 No phase separation 72 Example 3 3658 No phase separation 66
[0093] Test Example 2
[0094] According to the test steps of Part 8 of the method for determining the ultimate aerobic biodegradability of materials under controlled composting conditions of GB / T 19277.1-2011, the mixed gas at the outlet of the test container was continuously measured using an infrared carbon dioxide analyzer, the amount of carbon dioxide released was collected and calculated, and the biodegradation rate was continuously measured during the 6-month composting age. The biodegradation rates of the embodiments of the present invention at 45 days, 90 days, and 180 days are recorded in Table 2. The data results show that embodiments 1-3 all have good biodegradability under controlled composting conditions, with embodiment 3 being the best, and the decomposition rate of its test sample at 180 days reaches more than 99, which basically meets the complete degradation standard.
[0095] Table 2
[0096] 45-day biodegradability 90-day biodegradability 180-day biodegradability Example 1 26% 70% 97% Example 2 35% 73% 95% Example 3 33% 78% 99%
Claims
1. A method for preparing a biodegradable antibacterial hot melt adhesive, characterized in that: The following steps are included: (1) preparing carboxyl-terminated flexible random copolyester A; (2) preparing a hydroxyl-terminated rigid block polyester B; (3) Esterification and polycondensation of A and B; (4) Mixing and discharging the inorganic antibacterial component.
2. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 1, characterized in that: Step (1) comprises the following steps: (1.1) 130-170 parts of 1,4-butanediol, 50-70 parts of adipic acid, and 20-30 parts of terephthalic acid are mixed and added to an esterification reaction kettle, the temperature is raised to 150-170° C., 0.05-0.2% by weight of a catalyst of the total reactants is added, and the esterification reaction is carried out at 300-500 Pa for 1-3 hours; (1.2) When the water output reaches more than 95% of the theoretical value, the reaction is terminated and the flexible random copolyester A is obtained.
3. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 2, characterized in that: The catalyst in step (1.1) is at least one of tetrabutyl titanate, stannous chloride and antimony trioxide.
4. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 1, characterized in that: Step (2) comprises the following steps: (2.1) adding 80-120 parts of 6-caprolactone, 0.01-0.04 parts of diethylene glycol, and 0.01-0.04 parts of a catalyst into an esterification reaction kettle, heating to 110-130° C., and carrying out an esterification reaction at 100-150 Pa for 2-4 hours. When the water output is detected to be more than 95% of the theoretical value, the reaction is terminated, and a hydroxy-terminated caprolactone prepolymer is obtained; (2.2) The temperature in the reactor containing 200-250 parts of lactic acid and 0.01-0.05 parts of catalyst is raised to 80-120° C., the vacuum degree is 500-1000 Pa, and the dehydration reaction is carried out for 1-3 hours, during which the reduced pressure distillation is carried out to promote the forward reaction; the temperature is raised to 150-190° C., the vacuum degree is 1000-2000 Pa, and the depolymerization reaction is carried out for 1-2 hours to obtain lactide; (2.3) Add terminal hydroxyl caprolactone prepolymer, lactide and 0.05-0.1 part of antioxidant into a polycondensation reaction kettle, raise the temperature to 210-240°C, and carry out polycondensation reaction at 300-700 Pa for 0.5-1.5 h to obtain terminal carboxyl rigid block polyester B.
5. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 4, characterized in that: The catalyst in step (2.1) and step (2.2) is at least one of scandium trifluoromethanesulfonate, titanium glycol, antimony glycol, antimony acetate, stannous chloride, tin tetrachloride and zinc chloride; the antioxidant in step (2.3) is at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tris[2.4-di-tert-butylphenyl] phosphite and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.
6. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 1, characterized in that: Step (3) comprises the following steps: (3.1) Add the prepared carboxyl-terminated flexible random copolyester A and hydroxyl-terminated rigid block polyester B into a reaction kettle at a mass ratio of 1.1-1.3, add a catalyst, raise the temperature to 130-150° C., and carry out esterification reaction at 300-500 Pa. When the monitored water output reaches more than 95% of the theoretical value, stop the reaction; (3.2) After nitrogen is passed through, an antioxidant is added, the pressure is reduced to below 100 Pa, and the polycondensation reaction is carried out at 220-240°C. The power of the agitator increases with the molecular weight of the polymer, and polymers of different viscosities are obtained.
7. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 6, characterized in that: The catalyst in step (3.1) is at least one of dibutyltin laurate, stannous octoate, p-toluenesulfonic acid and tetraisobutyl titanate; the antioxidant in step (3.2) is at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, tris[2.4-di-tert-butylphenyl] phosphite and β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate.
8. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 1, characterized in that: Step (4) comprises the following steps: (4.1) The polymer obtained in step (3) is immediately transferred into an internal mixer preheated to 100-130°C and mixed at a speed of 30-60 r / min for 5 min; (4.2) Add 10-20% of the total mass of the polymer of a degradable tackifier, a degradable plasticizer, and an inorganic antibacterial agent, and continue stirring for 20-50 minutes before producing a glue.
9. The method for preparing the biodegradable antibacterial hot melt adhesive according to claim 8, characterized in that: The degradable tackifier in step (4.2) is at least one of rosin, polymerized rosin glycerol ester, terpene resin and coumarone resin; the degradable plasticizer in step (4.2) is at least one of triethyl citrate, tributyl citrate and castor oil; the inorganic antibacterial agent in step (4.2) is at least one of nano silver AGP-ZP003 with a particle size of 15 nm, nano copper HCU-P100 with a particle size of >200 nm and nano zinc oxide ZNO-P100 with a particle size of 20-30 nm produced by Shanghai Huzheng Industrial Co., Ltd.
10. A biodegradable antibacterial hot melt adhesive, characterized in that: The biodegradable antibacterial hot melt adhesive is prepared by the preparation method described in any one of claims 1-9.