Method and device for vapor phase growth of silicon carbide single crystals

By using turbine rectifier radiator rotation technology in silicon carbide single crystal growth technology, the problem of insufficient crystal radial temperature and backward heat dissipation uniformity is solved, and the growth rate is improved. and crystallization mass.

CN119041014APending Publication Date: 2024-11-29BEIJING LATTICE SEMICONDUCTOR CO LTD

Patent Information

Application Number
CN202411535919.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the existing single crystal growth technology of silicon carbide, the crystal radial temperature uniformity and backward heat dissipation uniformity are insufficient, resulting in unsatisfactory crystallization quality and low growth rate, which limits large-scale applications.

Method used

The turbine rectifier radiator is installed outside the growth crucible, and the high-temperature airflow is gathered to the center of the crucible by rotating, optimizing the radial temperature distribution and backward heat dissipation of the crystal, and dynamically adjusting the rotation speed of the turbine rectifier radiator to adapt to the insulation performance of the insulation material during growth process change.

Benefits of technology

Improve the crystal growth quality, increase the crystal size, achieve high-quality growth of large-size (≥6 inches) SiC single crystal, improve the growth rate and yield rate, and ensure the uniformity of the radial temperature distribution and the backward direction of the crystal. The stability of heat dissipation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041014A_ABST
    Figure CN119041014A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of silicon carbide single crystals, in particular to a method and a device for vapor phase growth of silicon carbide single crystals. The embodiment of the invention provides a method for vapor phase growth of silicon carbide single crystals. The method comprises the following steps: arranging a turbine rectification radiator on the outer side of a growth crucible and at a position corresponding to a silicon carbide seed crystal in the growth crucible; wherein the turbine rectification radiator faces the seed crystal, and the size of the turbine rectification radiator is larger than or equal to the size of the seed crystal; rotating the growth crucible; and the turbine rectification radiator is rotated, so that air flow around the turbine rectification radiator is converged to the center and then discharged towards the back direction. The embodiment of the invention provides a method and a device for vapor phase growth of silicon carbide single crystals, and can provide a technology for optimizing the radial temperature uniformity and the backward heat dissipation uniformity of crystals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of silicon carbide single crystals, and in particular to a method and a device for vapor phase growth of silicon carbide single crystals. Background Art

[0002] As one of the typical representatives of wide bandgap semiconductors, silicon carbide has excellent properties such as large bandgap width, high breakdown field strength, high saturated electron mobility, high thermal conductivity, good thermal stability and chemical stability. It is an ideal substrate material for making high-frequency, high-voltage, high-efficiency, radiation-resistant, high-temperature resistant high-power devices and blue light-emitting diodes, which makes it have important and huge application prospects in new energy vehicles, high-speed rail transit, aerospace, high-voltage smart grids and clean energy. Therefore, it has received widespread attention from academia and governments of various countries.

[0003] At present, the crystal quality and manufacturing cost of silicon carbide single crystal substrates are still one of the main factors limiting their large-scale application. Improving the crystal growth yield, growth rate and increasing the crystal size are the key to further reducing the price of silicon carbide single crystal substrates. The current mainstream technology for growing silicon carbide single crystals is physical vapor transport (PVT). Although this method has achieved large-scale industrial production, there are still problems such as unsatisfactory crystal quality, low growth rate and low yield.

[0004] When growing silicon carbide single crystals using the PVT method, the uniformity of the crystal's radial temperature field and the uniformity of the crystal's back heat dissipation will directly affect the crystal's crystallization quality, and in severe cases will cause stress cracking of the crystal. The back heat dissipation rate of the crystal will directly affect the crystal's growth rate. As the crystal size increases, the crystal's radial temperature uniformity and heat dissipation uniformity will significantly deteriorate, posing a huge challenge to improving the crystal's quality. In addition, the PVT method uses extremely high temperatures, and the thermal insulation performance of the thermal insulation material degrades rapidly during the growth process, resulting in poor long-term stability of the crystal growth. Therefore, there is an urgent need to develop a technology that optimizes the uniformity of the crystal's radial temperature and back heat dissipation. Summary of the invention

[0005] The embodiments of the present invention provide a method and an apparatus for vapor phase growth of a silicon carbide single crystal, which can provide a technology for optimizing the radial temperature uniformity and the back heat dissipation uniformity of the crystal.

[0006] In a first aspect, an embodiment of the present invention provides a method for vapor phase growth of a silicon carbide single crystal, comprising: A turbine rectifying radiator is arranged outside the growth crucible at a position corresponding to the silicon carbide seed crystal inside the crucible; wherein the turbine rectifying radiator faces the seed crystal, and the size of the turbine rectifying radiator is greater than or equal to the size of the seed crystal; rotating the growth crucible; The turbine rectifying radiator is rotated so that the airflow around it is gathered to the center and then discharged toward the back.

[0007] In a possible design, the step of rotating the turbine rectifier radiator so that the airflow around the turbine rectifier radiator converges to the center and then discharges it backward includes: In the first stage, the timing is taken as 0h when the silicon carbide crystal starts to grow. From 0h to 4-6h, the turbine rectifier radiator and the growth crucible rotate in the same direction at a rotation speed of 10-60rpm.

[0008] In a possible design, after the first stage, the method further includes: In the second stage, from 4 to 6 hours to 18 to 22 hours, the speed of the turbine rectifier radiator is uniformly changed to 30 to 300 rpm, which rotates in the opposite direction to the growth crucible; wherein the speed change rate of the turbine rectifier radiator is 10 to 600 rpm / h.

[0009] In a possible design, after the second stage, the method further includes: In the third stage, from 18 to 22 hours to 33 to 37 hours, the turbine rectifier radiator rotates at a speed of 30 to 300 rpm.

[0010] In a possible design, after the third stage, the method further includes: In the fourth stage, from 33 to 37 hours to 78 to 82 hours, the speed of the turbine rectifier radiator is dynamically adjusted to 10 to 150 rpm according to the change in the insulation performance of the insulation material outside the growth crucible; wherein the speed change rate of the turbine rectifier radiator is -0.1 to -120 rpm / h.

[0011] In a possible design, after the fourth stage, the following is further included: In the fifth stage, from 78 to 82 hours to 83 to 87 hours, the rotation speed of the turbine rectifier radiator is uniformly reduced to 0, and the growth is ended; wherein, the rotation conversion rate of the turbine rectifier radiator is -20 ~ -800 rpm / h.

[0012] In a possible design, before rotating the growth crucible, the method further includes: The temperature of the growth crucible is increased to 2100-2500° C., and the gas pressure of the growth furnace outside the growth crucible is reduced to 180-220 Pa.

[0013] In a possible design, the distance between the bottom of the turbine rectifier radiator and the growth crucible is 1-50 mm.

[0014] In one possible design, rotating the growth crucible includes: The growth crucible was rotated at a speed of 5-30 rpm.

[0015] In a second aspect, an embodiment of the present invention further provides a device for vapor phase growth of silicon carbide single crystals, for implementing any of the above methods, the device comprising a growth furnace, a growth crucible, a turbine rectifier radiator and an induction coil; The growth furnace is arranged outside the growth crucible, a seed crystal is arranged on the top inner side of the growth crucible, the growth crucible is filled with silicon carbide powder inside, and the outside is wrapped with insulation material, the insulation material is provided with holes matching the shape of the turbine rectifier radiator, the turbine rectifier radiator penetrates the insulation material through the holes and is arranged above the growth crucible, a first rotating lifting shaft is connected to the upper part of the turbine rectifier radiator, the insulation material is placed on a support tray, a second rotating lifting shaft is arranged at the bottom of the support tray, and the induction coil is arranged on the outside of the insulation material.

[0016] Compared with the prior art, the present invention has at least the following beneficial effects: In the present invention, by rotating the turbine rectifier radiator, the high-temperature airflow at the edge can flow quickly, evenly and continuously to the central area of ​​the crucible where the temperature is relatively low, thereby making the radial temperature distribution of the crystal in the growth crucible more uniform, thereby improving the quality of crystal growth. In addition, the rotation of the turbine rectifier radiator can also effectively eliminate turbulence, making the heat flow in the back heat dissipation process of the crystal more uniform, smooth and stable. The preparation method provided by the present application can prepare large-size (≥6 inches) SiC single crystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 1 is a schematic structural diagram of a device for vapor phase growth of silicon carbide single crystals provided in an embodiment of the present invention; Figure 2 The present invention provides a schematic diagram of a rotating process of a turbine rectifier radiator and a growth crucible; Figure 3 It is a schematic diagram of the rotation process selected in Examples 1 and 2 of the present invention.

[0019] In the figure: 1-first rotating lifting axis; 2-growth furnace; 3-insulating material; 4-turbine rectifier radiator; 5-seed crystal; 6-growth crucible; 7-induction coil; 8-silicon carbide powder; 9-support tray; 10-second rotating lifting axis. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0021] In the description of the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance; unless otherwise specified or explained, the term "multiple" refers to two or more; the terms "connected" and "fixed" should be understood in a broad sense, for example, "connected" can be a fixed connection, a detachable connection, an integral connection, or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0022] In the description of this specification, it should be understood that the directional words such as "upper" and "lower" described in the embodiments of the present invention are described at the angles shown in the drawings and should not be understood as limiting the embodiments of the present invention. In addition, in the context, it should also be understood that when it is mentioned that an element is connected to another element "upper" or "lower", it can not only be directly connected to another element "upper" or "lower", but also indirectly connected to another element "upper" or "lower" through an intermediate element.

[0023] like Figure 1 and Figure 2 As shown, an embodiment of the present invention provides a method for vapor phase growth of silicon carbide single crystal, comprising: A turbine rectifying radiator is arranged outside the growth crucible at a position corresponding to the silicon carbide seed crystal inside the crucible; wherein the turbine rectifying radiator faces the seed crystal, and the size of the turbine rectifying radiator is greater than or equal to the size of the seed crystal; Rotating growth crucible; The turbine rectifier radiator is rotated to converge the airflow around it to its center and then discharge it to its back.

[0024] In the present invention, by rotating the turbine rectifier radiator, the high-temperature airflow at the edge can flow quickly, evenly and continuously to the central area of ​​the crucible where the temperature is relatively low, thereby making the radial temperature distribution of the crystal in the growth crucible more uniform, thereby improving the quality of crystal growth. In addition, the rotation of the turbine rectifier radiator can also effectively eliminate turbulence, making the heat flow in the back heat dissipation process of the crystal more uniform, smooth and stable. The preparation method provided by the present application can prepare large-size (≥6 inches) SiC single crystals.

[0025] In some embodiments of the present invention, the turbine rectifier radiator is rotated so that the airflow around it converges to the center and then is discharged toward the back thereof, including: In the first stage, the timing is taken as 0h when the growth of silicon carbide crystal begins. From 0h to 4-6h, the turbine rectifier radiator and the growth crucible rotate in the same direction at a speed of 10-60rpm.

[0026] In the first stage, i.e. 0h to 4~6h, the turbine rectifier radiator and the growth crucible rotate at a constant speed of 10~60rpm in the same direction. Compared with the case without a turbine rectifier radiator, the heat dissipation rate on the back of the seed crystal is reduced, and the crystal growth is controlled at a lower growth rate in the initial stage, thereby ensuring the crystallization quality in the initial stage of growth.

[0027] In some embodiments of the present invention, after the first stage, the method further includes: In the second stage, from 4 to 6 hours to 18 to 22 hours, the speed of the turbine rectifier radiator is uniformly changed to 30 to 300 rpm, which rotates in the opposite direction to the growth crucible; wherein the speed change rate of the turbine rectifier radiator is 10 to 600 rpm / h.

[0028] In the second stage, i.e. 4~6h to 18~22h, the rotation speed of the radiator is uniformly changed from 10~60rpm in the same direction to 30~300rpm in the opposite direction, uniformly and slowly increasing the heat dissipation rate on the back of the seed crystal to slowly increase the crystal growth rate.

[0029] In some embodiments of the present invention, after the second stage, the method further includes: In the third stage, from 18~22h to 33~37h, the turbine rectifier radiator keeps rotating at 30~300rmp.

[0030] In the third stage, i.e. 18~22h to 33~37h, the speed of the turbine rectifier radiator is kept at a constant speed of 30~300rmp to ensure a continuous and stable heat dissipation rate to maintain a stable growth rate.

[0031] In some embodiments of the present invention, after the third stage, the method further includes: In the fourth stage, from 33 to 37 hours to 78 to 82 hours, the speed of the turbine rectifier radiator is dynamically adjusted to 10 to 150 rpm according to the change in the insulation performance of the insulation material outside the growth crucible; wherein the speed change rate of the turbine rectifier radiator is -0.1 to -120 rpm / h.

[0032] As the growth progresses, in the fourth stage, the thermal insulation performance of the thermal insulation material continues to decline at high temperatures, which will cause the heat dissipation to become faster. Therefore, according to the attenuation curve of the thermal insulation performance of the thermal insulation material, the speed of the radiator is reduced accordingly for dynamic compensation to maintain a stable heat dissipation rate.

[0033] In some embodiments of the present invention, after the fourth stage, the method further includes: In the fifth stage, from 78 to 82 hours to 83 to 87 hours, the rotation speed of the turbine rectifier radiator drops evenly to 0, and the growth ends; wherein, the rotation conversion rate of the turbine rectifier radiator is -20 to -800 rpm / h.

[0034] In the fifth stage, that is, 78~82h to 83~87h, the growth has basically ended, and the rotation speed is slowly reduced to reduce the growth rate, thereby ending the growth.

[0035] In some embodiments of the present invention, before rotating the growth crucible, the method further comprises: The temperature of the growth crucible is increased to 2100-2500°C, and the gas pressure of the growth furnace outside the growth crucible is reduced to 180-220Pa.

[0036] In this embodiment, when the temperature rises to 2100-2500° C. and the gas pressure drops to 180-220 Pa, the growth conditions are met and the growth of silicon carbide single crystal begins.

[0037] In some embodiments of the present invention, the distance between the bottom of the turbine rectifier radiator and the growth crucible is 1-50 mm.

[0038] In this embodiment, the distance between the turbine rectifier radiator and the growth crucible is within the above range to ensure a better heat dissipation control effect.

[0039] In some embodiments of the present invention, the rotating growth crucible comprises: The growth crucible was rotated at a speed of 5-30 rpm.

[0040] The embodiment of the present invention further provides a device for vapor phase growth of silicon carbide single crystal, which is used to implement any of the above methods, and the device includes a growth furnace, a growth crucible (preferably a graphite crucible), a turbine rectifier radiator and an induction coil; The growth furnace is arranged outside the growth crucible, a seed crystal is arranged on the top inner side of the growth crucible, silicon carbide powder is filled inside the growth crucible, and the outside is wrapped with a thermal insulation material, the thermal insulation material is provided with holes matching the shape of the turbine rectifier radiator, the turbine rectifier radiator penetrates the thermal insulation material through the holes and is arranged above the growth crucible, a first rotating lifting shaft is connected to the upper part of the turbine rectifier radiator, the thermal insulation material is placed on a support tray, a second rotating lifting shaft is arranged at the bottom of the support tray, and an induction coil is arranged on the outside of the thermal insulation material.

[0041] In this embodiment, a rotating lifting device is provided outside the furnace chamber of the growth furnace, which can drive the first rotating lifting shaft to rotate and move up and down, wherein the direction and speed of rotation and movement can be manually controlled, specifically, the top of the first rotating lifting shaft is connected to the rotating lifting device, and the bottom is connected to the turbine rectifier radiator, wherein the bottom end of the first rotating lifting shaft is provided with a tongue and groove structure for matching and connecting with the turbine rectifier radiator. The turbine rectifier radiator is a turbine structure including a large number of turbine blades, wherein a tongue and groove structure for matching and connecting with the first rotating lifting shaft is provided at the top axis center.

[0042] The blade structural parameters of the turbine rectifier radiator can be adjusted and optimized according to the actual process requirements. The maximum diameter of the turbine rectifier radiator is 6 to 16 inches, and the distance between the turbine rectifier radiator and the crucible cover is 1 to 50 mm. The first rotating lifting shaft and the turbine rectifier radiator are connected by a mortise and tenon structure, and the mortise and tenon structure includes all mortise and tenon structures that can simultaneously limit axial relative rotation and movement. Preferably, it includes all mortise and tenon structures that can simultaneously limit axial relative rotation and movement. Preferably, a mortise and tenon structure in the shape of "T" or "Dry" or "Y" or "L" or "F" is selected.

[0043] In order to more clearly illustrate the technical solutions and advantages of the present invention, several embodiments are described in detail below.

[0044] Example 1 This embodiment uses the device and method for rapidly growing large-size, high-quality silicon carbide single crystals by a vapor phase method provided by the present invention to grow a 6-inch silicon carbide single crystal, including the following steps: (1) Place high-purity silicon carbide powder into a growth crucible, and ensure that the distance between the silicon carbide powder surface and the top of the crucible cover is 20 mm; (2) affixing a silicon carbide seed crystal with a diameter of 155 mm to the inner top surface of the crucible cover, and then fixing the crucible cover on the crucible; (3) Connecting the turbine rectifier radiator to the bottom end of the first rotating lifting shaft and placing it above the growth crucible cover; (4) Arrange the heat-insulating material around the crucible, and then connect the top end of the first rotary lifting shaft to the rotary lifting device at the top of the furnace chamber of the growth furnace, while ensuring that the turbine rectifier radiator does not contact the crucible cover, and control the gap between the turbine rectifier radiator and the crucible cover to be 5 mm; (5) closing the furnace chamber of the growth furnace, configuring the growth protective atmosphere and heating the crucible; (6) After the crucible temperature rises to 2300 °C, the gas pressure in the growth furnace chamber is reduced to 200 Pa, and crystal growth begins; (7) During the crystal growth process, the rotating device of the control equipment makes the crucible and the turbine rectifier radiator respectively attached to Figure 3 The process shown is rotated.

[0045] (8) At the same time, the crucible and the turbine rectifier radiator are controlled to move upward slowly and synchronously at a speed of 1 mm / h; (9) After the growth is completed, the temperature is slowly lowered. When the temperature drops to room temperature, open the furnace chamber of the growth furnace, remove the turbine rectifier radiator, take out the crucible, open the crucible cover, and remove the crystal from the crucible cover.

[0046] In this example, a high-quality 6-inch silicon carbide crystal was successfully grown. The crystal growth surface was very bright and the convexity of the crystal growth surface was very small, indicating that the radial temperature distribution during crystal growth was very uniform. The crystal thickness was about 30 mm and the crystal growth rate was about 360 μm / h, which was significantly higher than the current general level.

[0047] Example 2 This embodiment uses the device and method for rapidly growing large-size, high-quality silicon carbide single crystals by vapor phase method provided by the present invention to grow 8-inch silicon carbide single crystals, including the following steps: (1) Place high-purity silicon carbide powder into a growth crucible, and ensure that the distance between the silicon carbide powder surface and the top of the crucible cover is 20 mm; (2) a silicon carbide seed crystal with a diameter of 200 mm is pasted onto the inner top surface of the crucible cover, and then the crucible cover is fixed on the crucible; (3) Connecting the turbine rectifier radiator to the bottom end of the first rotating lifting shaft and placing it above the growth crucible cover; (4) Arrange the heat-insulating material around the crucible, and then connect the top end of the first rotary lifting shaft to the rotary lifting device at the top of the furnace chamber of the growth furnace, while ensuring that the turbine rectifier radiator does not contact the crucible cover, and control the gap between the turbine rectifier radiator and the crucible cover to be 5 mm; (5) closing the furnace chamber of the growth furnace, configuring the growth protective atmosphere and heating the crucible; (6) After the crucible temperature rises to 2300 °C, the gas pressure in the growth furnace chamber is reduced to 200 Pa, and crystal growth begins; (7) During the crystal growth process, the rotating device of the control equipment makes the crucible and the turbine rectifier radiator respectively attached to Figure 3 The process shown is rotated; (8) At the same time, the crucible and the turbine rectifier radiator are controlled to move upward slowly and synchronously at a speed of 1 mm / h; (9) After the growth is completed, the temperature is slowly lowered. When the temperature drops to room temperature, open the furnace chamber of the growth furnace, remove the turbine rectifier radiator, take out the crucible, open the crucible cover, and remove the crystal from the crucible cover.

[0048] In this example, a high-quality 8-inch silicon carbide crystal was successfully grown. The crystal growth surface was very bright and the convexity of the crystal growth surface was very small, indicating that the radial temperature distribution during crystal growth was very uniform. The crystal thickness was about 20 mm and the crystal growth rate was about 240 μm / h.

[0049] Comparative Example 1 The device for growing silicon carbide crystal by gas phase method in this comparative example does not include Figure 1 The turbine rectifier radiator structure shown in the figure naturally cannot realize the attached Figure 2 In the in-situ heat dissipation control process shown, only the crucible rotates and moves during the growth process, and the other processes are basically consistent with Example 2.

[0050] The growth surface of the 8-inch silicon carbide crystal grown in this comparative example has a large convexity, indicating that the radial temperature distribution during the growth process is very uneven, and the temperature in the center area is significantly lower than the temperature in the edge area; in addition, the crystal cracks due to excessive thermal stress, and the growth rate of the crystal is only 100μm / h. It shows that without the device and method provided by the present invention, it is difficult to ensure that the radial temperature distribution maintains good uniformity during the growth of large-size crystals, and the heat dissipation efficiency is also poor, resulting in poor crystal growth quality and low growth rate.

[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for vapor phase growth of silicon carbide single crystals, characterized in that: include: A turbine rectifying radiator is arranged outside the growth crucible at a position corresponding to the silicon carbide seed crystal inside the crucible; wherein the turbine rectifying radiator faces the seed crystal, and the size of the turbine rectifying radiator is greater than or equal to the size of the seed crystal; rotating the growth crucible; The turbine rectifying radiator is rotated so that the airflow around it is gathered to the center and then discharged toward the back.

2. The method according to claim 1, characterized in that The step of rotating the turbine rectifier radiator so that the airflow around the turbine rectifier radiator converges to the center and then discharges it in a rear direction includes: In the first stage, the timing is taken as 0h when the silicon carbide crystal starts to grow. From 0h to 4-6h, the turbine rectifier radiator and the growth crucible rotate in the same direction at a rotation speed of 10-60rpm.

3. The method according to claim 2, characterized in that After the first stage, it also includes: In the second stage, from 4 to 6 hours to 18 to 22 hours, the speed of the turbine rectifier radiator is uniformly changed to 30 to 300 rpm, which rotates in the opposite direction to the growth crucible; wherein the speed change rate of the turbine rectifier radiator is 10 to 600 rpm / h.

4. The method according to claim 3, characterized in that After the second stage, it also includes: In the third stage, from 18 to 22 hours to 33 to 37 hours, the turbine rectifier radiator rotates at a speed of 30 to 300 rpm.

5. The method according to claim 4, characterized in that After the third stage, it also includes: In the fourth stage, from 33 to 37 hours to 78 to 82 hours, the speed of the turbine rectifier radiator is dynamically adjusted to 10 to 150 rpm according to the change in the insulation performance of the insulation material outside the growth crucible; wherein the speed change rate of the turbine rectifier radiator is -0.1 to -120 rpm / h.

6. The method according to claim 5, characterized in that After the fourth stage, it also includes: In the fifth stage, from 78 to 82 hours to 83 to 87 hours, the rotation speed of the turbine rectifier radiator is uniformly reduced to 0, and the growth ends; wherein, the rotation conversion rate of the turbine rectifier radiator is -20 to -800 rpm / h.

7. The method according to claim 1, characterized in that Before rotating the growth crucible, the method further comprises: The temperature of the growth crucible is increased to 2100-2500° C., and the gas pressure of the growth furnace outside the growth crucible is reduced to 180-220 Pa.

8. The method according to claim 1, characterized in that The distance between the bottom of the turbine rectifier radiator and the growth crucible is 1-50 mm.

9. The method according to claim 1, characterized in that: The rotating the growth crucible comprises: The growth crucible was rotated at a speed of 5-30 rpm.

10. An apparatus for vapor phase growth of silicon carbide single crystals, characterized in that: Used to implement the method described in any one of claims 1 to 9, the device comprises a growth furnace, a growth crucible, a turbine rectifier radiator and an induction coil; The growth furnace is arranged outside the growth crucible, a seed crystal is arranged on the top inner side of the growth crucible, the growth crucible is filled with silicon carbide powder inside, and the outside is wrapped with insulation material, the insulation material is provided with holes matching the shape of the turbine rectifier radiator, the turbine rectifier radiator penetrates the insulation material through the holes and is arranged above the growth crucible, a first rotating lifting shaft is connected to the upper part of the turbine rectifier radiator, the insulation material is placed on a support tray, a second rotating lifting shaft is arranged at the bottom of the support tray, and the induction coil is arranged on the outside of the insulation material.

Citation Information

Patent Citations

  • Growing device for high-quality silicon carbide crystals

    CN105040103A

  • Transformer heat dissipation device for photovoltaic power generation

    CN214476848U

  • Silicon carbide crystal growth furnace for growing crystals with uniform thickness

    CN217869174U

  • Apparatus for growing silicon carbide single crystal

    KR1020150043691A

Cited By

  • Device and method for diversion growth of silicon carbide single crystals

    CN121428669A