Porous nano silicon-carbon composite material coated with carbon layer and preparation method of porous nano silicon-carbon composite material
The porous structure is formed by spray drying and carbonization, and then coated with the coal asphalt layer, which solves the problem of volume expansion and low conductivity of silicon-based negative electrode materials in lithium-ion batteries, and significantly improves the cycling stability and rate performance of the battery.
Patent Information
- Application Number
- CN202411029221.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-30
AI Technical Summary
In traditional lithium-ion batteries, volume expansion of silicon-based anode material during circulation leads to damage of conductive network, thickening of SEI film and increasing internal resistance, affecting battery performance. Nanosilicon materials are prone to oxidation and deterioration, making it difficult to ensure product yield and cycle stability. sex.
The nano-silicon particles are dispersed in the phenolic resin to form a porous structure, and then carbonized in an inert atmosphere, followed by adding coal asphalt for ball milling and high-temperature carbonization to form a porous nano-silicon carbon composite material coated with carbon layer, buffering Volume expansion and increase electron conductivity.
It significantly improves the cycle stability and rate performance of the battery, extends the battery life, reduces the risk of crushing and shedding of silicon particles, and improves the transmission efficiency of lithium ions.
Smart Images

Figure CN119050290A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery negative electrode materials, and in particular to a porous nano silicon-carbon composite material coated with a carbon layer and a preparation method thereof. Background Art
[0002] Over the past two decades, consumer electronics and electric vehicles have developed rapidly, making people's lives more convenient. Among them, the rise of electric vehicles has reduced a lot of carbon emissions compared to traditional fuel vehicles, greatly alleviating the greenhouse effect. Lithium-ion batteries have been used in 3C and EV, and even in the field of electric aircraft, due to their cycle performance and energy density advantages. However, the capacity of traditional graphite negative electrodes (372mAh g -1 ) has reached its limit and it is difficult to meet people's demand for battery life. Silicon is one of the most abundant substances on earth (the second largest in reserves), and it has an ultra-high energy density (4200mAh g -1 ), many researchers have been attracted by silicon-based negative electrodes. The lithium storage capacity of negative electrode materials determines the specific capacity of negative electrode materials. However, after the silicon negative electrode is embedded with lithium ions, its volume will expand (greater than 300%), resulting in a series of problems in application, such as silicon particle crushing, separation of negative electrode materials from the current collector, and SEI film generation consuming a large amount of lithium ions. After a long period of cycling, the conductive network of the negative electrode of the lithium battery will be destroyed and collapsed due to the crushing and separation of silicon particles, and lose electrical contact with the current collector. The repeated breakage and formation of the SEI film will lead to the continuous consumption of electrolytes and lithium ions, and ultimately cause the loss of specific capacity and affect battery performance. At the same time, Si is a semiconductor material with low electronic conductivity (1.56×10 -3 s / m), the electron transfer rate is slow and cannot meet the requirements of fast kinetic reactions.
[0003] In order to reduce the volume expansion of silicon negative electrodes, increase cycle life, and improve electronic conductivity, researchers designed to reduce silicon materials to the nanoscale, including silicon nanoparticles, silicon nanowires, nanosilicon films, porous silicon and other structures. Subsequently, conductive elements such as carbon, gold, and copper are coated on the surface of Si to lock the silicon particles in a rigid matrix. The surface coating of nano-silicon can be used to alleviate the problem of volume expansion during its charge and discharge process. In the prior art, phenolic resin is grown in situ on the surface of silicon particles and carbonized, so that a carbon layer can be formed on the surface of silicon particles, which plays a buffering and supporting role. However, the subsequent etching of silicon by hydrofluoric acid will cause irreversible expansion and contraction of silicon particles. This will cause the stable SEI film formed on the surface to continuously break and regenerate, resulting in thickening of the electrolyte interface layer (SEI) film, increased internal resistance of the battery and increased polarization. At present, there is also a technical solution that uses nano-silicon materials with smaller particle sizes and compounds them with graphite and carbon materials. This composite structure helps to shorten the transmission distance of lithium ions in the material, and can also better inhibit the volume expansion of silicon during the cycle process and reduce the material breakage caused by it. However, this regulation method using nano-silicon as raw material also has some potential problems in actual production. Nano-silicon materials are very easy to oxidize and deteriorate, which brings certain challenges to the guarantee of product yield. In addition, this composite material does not have a significant effect on improving the long-cycle stability of silicon-based negative electrode materials. Therefore, it is necessary to explore a better preparation process to solve the volume expansion problem of silicon-based negative electrode materials in order to improve the cycle stability and rate performance of the battery.
[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a porous nano-silicon-carbon composite material coated with a carbon layer and a preparation method thereof, aiming to solve the problem of how to reduce the volume expansion of silicon-based negative electrode materials so as to improve the cycle stability and rate performance of the battery.
[0006] The technical solution of the present invention is as follows:
[0007] A first aspect of the present invention provides a method for preparing a porous nano-silicon-carbon composite material coated with a carbon layer, comprising the following steps:
[0008] S1, dispersing nano silicon and phenolic resin in ethanol respectively to obtain nano silicon slurry and phenolic resin solution;
[0009] S2, mixing and stirring the nano-silicon slurry and the phenolic resin solution to form a mixed slurry, and then spray drying to disperse the nano-silicon particles in the phenolic resin to obtain a mixed powder;
[0010] S3, subjecting the mixed powder to a first carbonization treatment in an inert atmosphere to obtain nano-silicon carbon with a porous structure;
[0011] S4, adding coal tar into ethanol and stirring, then adding the porous nano silicon carbon and stirring to dissolve, ball milling and mixing, and then performing a second carbonization treatment to obtain the porous nano silicon carbon composite material coated with the carbon layer.
[0012] In step S1, optionally, the particle size of the nano-silicon is 10 to 200 nm.
[0013] Optionally, the mass ratio of the nano-silicon to the phenolic resin is (1:3) to (3:1).
[0014] In step S2, optionally, the process conditions of the spray drying are: the inlet temperature of the spray drying is 100-200°C, the outlet temperature is 50-150°C, and the spray drying time is 0.5-5h.
[0015] In step S3, optionally, the step of subjecting the mixed powder to a first carbonization treatment in an inert atmosphere specifically comprises: placing the mixed powder in a tubular furnace filled with argon gas, and heating the mixture in the following manner:
[0016] Raise the temperature from room temperature to the first temperature at a rate of 1 to 5°C / min, and keep warm for 0.5 to 2 hours;
[0017] Raise the temperature from the first temperature to the second temperature at a rate of 1 to 5°C / min and keep warm for 0.5 to 2 hours;
[0018] Raise the temperature from the second temperature to the third temperature at a rate of 1 to 5°C / min, and keep warm for 0.5 to 2 hours;
[0019] Raise the temperature from the third temperature to the first carbonization temperature at a rate of 3-10°C / min, and keep the temperature for 0.5-2h;
[0020] The first temperature is 80-120° C., the second temperature is 100-140° C., the third temperature is 120-180° C., and the third temperature is greater than the second temperature and greater than the first temperature.
[0021] Optionally, the first carbonization temperature is 500-900°C.
[0022] In step S4, optionally, the ratio of the mass of the coal tar pitch to the sum of the mass of the nano-silicon and the phenolic resin is 1:(30-150).
[0023] Optionally, the solvent is ethanol or toluene.
[0024] In step S4, optionally, the parameter conditions of the ball milling mixing are:
[0025] The ball-to-material ratio is (1:2) to (2:1);
[0026] The forward rotation rate is 300-700rpm, and the forward rotation time is 15-60min;
[0027] The reversal rate is 300-700 rpm, and the reversal time is 15-60 min.
[0028] In step S4, optionally, the heating method of the second carbonization treatment is:
[0029] Heating from room temperature to a fourth temperature at a heating rate of 5 to 30°C / min;
[0030] The temperature is raised from the fourth temperature to the second carbonization temperature at a heating rate of 5 to 30°C / min and kept at this temperature for 6 hours;
[0031] Wherein, the fourth temperature is 400-600°C.
[0032] Optionally, the second carbonization temperature is 800-1000°C.
[0033] The second aspect of the present invention provides a porous nano-silicon-carbon composite material coated with a carbon layer, which is prepared by the method for preparing a porous nano-silicon-carbon composite material coated with a carbon layer; the particle size of the porous nano-silicon-carbon composite material coated with a carbon layer is 0.1 to 10 μm.
[0034] Beneficial effects:
[0035] The present invention disperses small-particle nano-silicon in phenolic resin by spray drying to form a composite structure of nano-silicon-carbon materials, and then generates pores inside the nano-silicon-carbon through carbonization treatment of the phenolic resin to generate nano-silicon-carbon with a porous structure, which can effectively buffer the volume expansion of nano-silicon particles before and after the cycle, and avoid the crushing of silicon particles and the pulverization and shedding of materials from the pole piece. After the nano-silicon-carbon with a porous structure is coated with a carbon layer after carbonization of coal tar, the electronic conductivity is improved, and the removal and embedding of lithium ions are also easier, which significantly improves the stability of the porous nano-silicon-carbon composite material coated with the carbon layer, and the first coulomb efficiency and the cycle coulomb efficiency are greatly improved. At the same time, the preparation method provided by the present invention has low cost, simple production process, good product effect, and has a good commercial application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The present invention is a schematic flow chart of a method for preparing a porous nano-silicon-carbon composite material coated with a carbon layer.
[0037] Figure 2 Schematic diagram of the structure of the porous nano silicon-carbon composite material (Si@PF@CTP-500°C) coated with a carbon layer prepared in Example 1 of the present invention.
[0038] Figure 3 This is a scanning electron microscope (SEM) image of the porous nano-silicon carbon (Si@PF) prepared in Example 4 of the present invention.
[0039] Figure 4 This is a SEM image of the porous nano-silicon-carbon composite material (Si@PF@CTP-500°C) coated with a carbon layer prepared in Example 1 of the present invention.
[0040] Figure 5 This is an X-ray diffraction (XRD) pattern of the porous nano-silicon-carbon composite material (Si@PF@CTP-500°C) coated with a carbon layer prepared in Example 1 of the present invention.
[0041] Figure 6 The charge and discharge curves of the porous nano-silicon-carbon composite material coated with a carbon layer prepared in Examples 1-4 of the present invention and the nano-silicon-carbon material in Comparative Example 1.
[0042] Figure 7 These are the cycle test curves of the porous nano-silicon-carbon composite material coated with a carbon layer prepared in Examples 1-4 of the present invention and the nano-silicon-carbon material in Comparative Example 1. DETAILED DESCRIPTION
[0043] The present invention provides a porous nano-silicon-carbon composite material coated with a carbon layer and a preparation method thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0044] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0045] The present invention provides a method for preparing a porous nano-silicon-carbon composite material coated with a carbon layer, comprising the following steps:
[0046] S1, dispersing nano silicon and phenolic resin in ethanol respectively to obtain nano silicon slurry and phenolic resin solution;
[0047] S2, mixing and stirring the nano-silicon slurry and the phenolic resin solution to form a mixed slurry, and then spray drying to disperse the nano-silicon particles in the phenolic resin to obtain a mixed powder;
[0048] S3, subjecting the mixed powder to a first carbonization treatment in an inert atmosphere to obtain nano-silicon carbon with a porous structure;
[0049] S4, adding coal tar into ethanol and stirring, then adding the porous nano silicon carbon and stirring to dissolve, ball milling and mixing, and then performing a second carbonization treatment to obtain the porous nano silicon carbon composite material coated with the carbon layer.
[0050] The present invention first uses a spray drying method to evenly disperse nano silicon and phenolic resin together, and then carbonizes the phenolic resin. The hydrogen and oxygen elements in the phenolic resin are removed in the form of gas, leaving holes and pores of different sizes, and the carbon element is retained, thereby producing a porous nano silicon carbon (particle size is about 0.01 to 5 μm). The second carbonization is performed on the coal tar coated on the surface of the nano silicon carbon. The hydrogen and oxygen elements in the coal tar are removed by high temperature, leaving carbon and pores, ensuring that there can be a certain transmission path between the inside of the nano silicon carbon and the electrolyte. Finally, a porous nano silicon carbon composite material coated with a carbon layer is obtained.
[0051] In step S1, in some embodiments, the particle size of the nano-silicon is 10 to 200 nm.
[0052] The present invention adopts nano silicon with small particle size for dispersion, thus significantly reducing the volume expansion effect of silicon during the process of lithium insertion and extraction.
[0053] In some embodiments, the mass ratio of the nano-silicon to the phenolic resin is (1:3) to (3:1).
[0054] In step S2, in some embodiments, the process conditions of spray drying are: the inlet temperature of spray drying is 100-200°C, the outlet temperature is 50-150°C, and the spray drying time is 0.5-5h.
[0055] The present invention uses a spray drying method to disperse nano silicon particles in a phenolic resin matrix, and after carbonization treatment, some pores can be generated to form a porous structure.
[0056] In step S3, in some embodiments, the step of subjecting the mixed powder to a first carbonization treatment in an inert atmosphere specifically comprises: placing the mixed powder in a tubular furnace filled with argon gas, and heating the mixture by:
[0057] Raise the temperature from room temperature to the first temperature at a rate of 1 to 5°C / min, and keep warm for 0.5 to 2 hours;
[0058] Raise the temperature from the first temperature to the second temperature at a rate of 1 to 5°C / min and keep warm for 0.5 to 2 hours;
[0059] Raise the temperature from the second temperature to the third temperature at a rate of 1 to 5°C / min, and keep warm for 0.5 to 2 hours;
[0060] Raise the temperature from the third temperature to the first carbonization temperature at a rate of 3-10°C / min, and keep the temperature for 0.5-2h;
[0061] The first temperature is 80-120° C., the second temperature is 100-140° C., the third temperature is 120-180° C., and the third temperature is greater than the second temperature and greater than the first temperature.
[0062] In some embodiments, the first carbonization temperature is 500-900°C.
[0063] In the carbonization process of phenolic resin, the heating stage below the third temperature (120-180°C) is slow heating, the phenolic resin is preheated, and gradually begins to decompose. The phenolic resin on the surface of the mixed powder material first begins to carbonize to produce a certain number of micropores and pores. As the heating proceeds, the pores gradually extend into the material, and the number of pores increases. The temperature is kept warm for a certain period of time to prevent the sudden and rapid change of temperature from causing regional stress concentration to produce large cracks, resulting in the rupture and pulverization of the electrode material. The low-temperature slow treatment makes the size and distribution of the pores produced by carbonization more uniform, creating conditions for the subsequent growth and increase of pores. In the heating stage from the third temperature to the first carbonization temperature (500-900°C), the heating rate is accelerated, the decomposition of the phenolic resin is accelerated, the thermal weight loss is obvious, hydrogen and oxygen are removed in large quantities, and a large number of pores and pores are produced. After a period of heat preservation, the required porous carbon substrate material is obtained, including different numbers of micropores, mesopores, and macropores, which creates an effective path for the transmission of lithium ions and has a strong accommodating and inhibiting effect on the volume expansion of nano-silicon.
[0064] In step S4, in some embodiments, the ratio of the mass of the coal tar pitch to the sum of the mass of the nano-silicon and the phenolic resin is 1:(30-150). The solvent in the coal tar pitch solution may be ethanol or toluene, but is not limited thereto.
[0065] Coal tar pitch is a soft carbon. After carbonization, its structural stability is greatly improved. In order to reduce the occurrence of side reactions, avoid the etching of Si by HF acid in the electrolyte, and improve the electrode conductivity, industrially low-cost and easily available coal tar pitch is used for carbon coating and carbonization treatment, and then a layer of stable soft carbon is coated. After carbonization, the electronic conductivity is improved and the volume expansion is improved.
[0066] In step S4, in some embodiments, the parameter conditions of the ball milling mixing are:
[0067] The ball-to-material ratio is (1:2) to (2:1);
[0068] The forward rotation rate is 300-700rpm, and the forward rotation time is 15-60min;
[0069] The reversal rate is 300-700 rpm, and the reversal time is 15-60 min.
[0070] In step S4, in some embodiments, the heating method of the second carbonization treatment is:
[0071] Heating from room temperature to a fourth temperature at a heating rate of 5 to 30°C / min;
[0072] The temperature is raised from the fourth temperature to the second carbonization temperature at a heating rate of 5 to 30°C / min and kept at this temperature for 6 hours;
[0073] Wherein, the fourth temperature is 400-600°C.
[0074] In some embodiments, the second carbonization temperature is 800-1000°C.
[0075] During the carbonization process of coal tar, in the low-temperature carbonization stage below the fourth temperature (400-600°C), the coal tar first begins to undergo thermal cracking of molecules, producing a small amount of carbon and gas. As the temperature rises, the cracking rate of the coal tar increases, producing a large amount of carbon and gas. A carbon coating is gradually formed and some pores are generated, which is beneficial to the improvement of electrical conductivity and ion diffusion. The high-temperature carbonization at 800-1000°C has a very fast reaction speed, producing a large amount of carbon, gas, and pores, forming a complete carbon coating with microporous, mesoporous, and macroporous structures, which plays a role in buffering the volume expansion of nano-silicon and is beneficial to the improvement of electronic conductivity and ionic conductivity.
[0076] A second aspect of the present invention provides a porous nano-silicon-carbon composite material coated with a carbon layer, which is prepared by the method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer.
[0077] In some embodiments, the particle size of the porous nano-silicon-carbon composite material coated with the carbon layer is 0.1-10 μm.
[0078] The following describes it in detail through specific embodiments.
[0079] Example 1
[0080] Please refer to Figure 1 The schematic diagram of the process of preparing the nano-carbon-silicon composite material coated with the carbon layer is shown in the figure. The preparation process of this embodiment specifically includes the following steps:
[0081] (1) Si@PF composite powder
[0082] Nano silicon dispersion: homogenizer dispersion. Take 150g nano silicon and add 1350g anhydrous ethanol, stir and pre-disperse first, then add to the homogenizer, and disperse once at a pressure of 23000Psi;
[0083] Phenolic dissolution: add 300g phenolic resin to 2700g anhydrous ethanol and dissolve it by ultrasonic for 5min;
[0084] Compounding: Add the dispersed nano-silicon slurry and phenolic solution into a 5L double planetary stirring kettle, and set the parameters to 40rpm / 1000rpm / 30min;
[0085] Spray process parameters: inlet temperature 150℃, outlet temperature 90℃, atomizing disk 280Hz, fan 25Hz.
[0086] (2) Carbonization of phenolic resin
[0087] Ar (99.9%) gas was introduced into the reaction chamber of the tubular furnace at a rate of 100 ml / min, and the temperature was increased from room temperature to 1000°C at a rate of 2°C / min and kept warm for 1 h; the temperature was increased from 100°C to 120°C at a rate of 2°C / min and kept warm for 1 h, 120-150°C, and the temperature was increased from 120°C to 150°C at a rate of 2°C / min and kept warm for 1 h, and the temperature was increased from 150°C to 500°C at a rate of 5°C / min and kept warm for 1 h.
[0088] (3) Nano-silicon carbon coated with coal tar
[0089] Take 10g of coal tar, add 30g of anhydrous ethanol, stir and dissolve at room temperature for 10min, then add 20g of Si@PF sample and stir and dissolve for 10min.
[0090] (4) Ball milling
[0091] Ball to material ratio 2:1. Program: forward 15min / 500rpm, reverse 15min / 500rpm.
[0092] (5) Carbonization of coal tar
[0093] The temperature was raised from room temperature to 450°C at a heating rate of 15°C / min; the temperature was raised from 450 to 850°C at a heating rate of 10°C / min, and kept at 850°C for 6 h, and then naturally cooled to room temperature.
[0094] (6) The black powder was collected to obtain a porous nano-silicon-carbon composite material coated with a carbon layer, which was recorded as Si@PF@CTP-500°C.
[0095] like Figure 2 In the structural schematic diagram of the porous nano-silicon-carbon composite material (Si@PF@CTP-500℃) coated with a carbon layer shown in the figure: ① is the coal tar carbon coating layer, ② is the phenolic resin carbon substrate, ③ is the pores, and ④ is the nano-silicon particles.
[0096] Example 2
[0097] A porous nano-silicon-carbon composite material coated with a carbon layer was prepared by the same method as in Example 1, except that the maximum carbonization temperature of the phenolic resin was 700°C, and the porous nano-silicon-carbon composite material coated with a carbon layer was obtained, which was recorded as Si@PF@CTP-700°C.
[0098] Example 3
[0099] A porous nano-silicon-carbon composite material coated with a carbon layer was prepared by the same method as in Example 1, except that the maximum carbonization temperature of the phenolic resin was 900°C, and a porous nano-silicon-carbon composite material coated with a carbon layer was obtained, which was recorded as Si@PF@CTP-900°C.
[0100] Example 4
[0101] Compared with Example 1, the difference is that it only includes steps (1) and (2) to prepare nano-silicon carbon with a porous structure, which is denoted as Si@PF.
[0102] Comparative Example 1
[0103] Commercially purchased nano silicon carbon was directly used for testing and comparison.
[0104] like Figure 3 As shown, the SEM image of the nano-silicon carbon Si@PF prepared in Example 4 shows that it has a porous structure and a uniform particle size distribution of about 0.01 to 5 μm.
[0105] Figure 4 The morphology and structure of the porous nano-silicon-carbon composite material (Si@PF@CTP-500℃) coated with a carbon layer are shown, and the existence of pores can be clearly seen inside the material.
[0106] like Figure 5 As shown, obvious Si peaks and C peaks can be observed from the XRD pattern of the porous nano-silicon-carbon composite material coated with a carbon layer.
[0107] From the charge and discharge curves of Example 1, Example 2, Example 3, Comparative Example 1, and Comparative Example 2 ( Figure 6 ) and cycle test curve ( Figure 7 ) It can be seen that the porous nano-silicon-carbon composite electrode coated with carbon layer by carbonized coal tar has better first coulombic efficiency and cycle coulomb than the porous nano-silicon-carbon electrode without carbon coating. The porous nano-silicon-carbon composite material coated with carbon layer at 700℃ phenolic resin carbonization temperature (Si@PF@CTP-700℃) has the best cycle performance and the highest specific capacity, and the corresponding nano-silicon dispersion structure, coating carbonization degree and thickness have the best performance.
[0108] The specific electrochemical performance data of the test are shown in Table 1.
[0109] Table 1
[0110]
[0111] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a porous nano-silicon-carbon composite material coated with a carbon layer, characterized in that: The following steps are involved: S1, dispersing nano silicon and phenolic resin in ethanol respectively to obtain nano silicon slurry and phenolic resin solution, mixing and stirring to form a mixed slurry; S2, spray drying the mixed slurry to disperse the nano silicon particles in the phenolic resin to obtain a mixed powder; S3, subjecting the mixed powder to a first carbonization treatment in an inert atmosphere to obtain nano-silicon carbon with a porous structure; S4, adding coal tar into the solvent and stirring, then adding the porous nano silicon carbon and stirring to dissolve, ball milling and mixing, and then performing a second carbonization treatment to obtain the porous nano silicon carbon composite material coated with the carbon layer.
2. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 1, characterized in that: In step S1, the particle size of the nano-silicon is 10 to 200 nm; the mass ratio of the nano-silicon to the phenolic resin is (1:3) to (3:1).
3. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 1, characterized in that: In step S2, the process conditions of spray drying are: the inlet temperature of spray drying is 100-200°C, the outlet temperature is 50-150°C, and the spray drying time is 0.5-5h.
4. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 1, characterized in that: In step S3, the step of subjecting the mixed powder to a first carbonization treatment in an inert atmosphere specifically comprises: placing the mixed powder in a tubular furnace into which an inert gas is introduced, and heating the mixture by: Raise the temperature from room temperature to the first temperature at a rate of 1 to 5°C / min, and keep warm for 0.5 to 2 hours; Raise the temperature from the first temperature to the second temperature at a rate of 1 to 5°C / min and keep warm for 0.5 to 2 hours; Raise the temperature from the second temperature to the third temperature at a rate of 1 to 5°C / min, and keep warm for 0.5 to 2 hours; Raise the temperature from the third temperature to the first carbonization temperature at a rate of 3-10°C / min, and keep the temperature for 0.5-2h; The first temperature is 80-120° C., the second temperature is 100-140° C., the third temperature is 120-180° C., and the third temperature is greater than the second temperature and greater than the first temperature.
5. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 4, characterized in that: The first carbonization temperature is 500-900°C.
6. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 1, characterized in that: In step S4, the ratio of the mass of the coal tar pitch to the sum of the mass of the nano-silicon and the phenolic resin is 1:(30-150); and / or, the solvent is ethanol or toluene.
7. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 1, characterized in that: In step S4, the parameter conditions of the ball milling mixing are: The ball-to-material mass ratio is (1:2) to (2:1); The forward speed rate is 300-700rpm, and the forward rotation time is 15-60min; The reversal rate is 300-700 rpm, and the reversal time is 15-60 min.
8. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 1, characterized in that: In step S4, the heating method of the second carbonization treatment is: Heating from room temperature to a fourth temperature at a heating rate of 5 to 30°C / min; The temperature is raised from the fourth temperature to the second carbonization temperature at a heating rate of 5 to 30°C / min and kept at this temperature for 6 hours; Wherein, the fourth temperature is 400-600°C.
9. The method for preparing the porous nano-silicon-carbon composite material coated with a carbon layer according to claim 8, characterized in that: The second carbonization temperature is 800-1000°C.
10. A porous nano-silicon-carbon composite material coated with a carbon layer, characterized in that: The porous nano silicon-carbon composite material coated with a carbon layer is prepared by the method for preparing the porous nano silicon-carbon composite material coated with a carbon layer according to claims 1 to 9; the particle size of the porous nano silicon-carbon composite material coated with a carbon layer is 0.1 to 10 μm.
Citation Information
Patent Citations
Preparation method of graphite silicon substrate composite cathode material
CN104916831A
Three-dimensional spherical silicon-carbon composite negative electrode material and preparation method therefor
CN107230781A
Nanometer silicon-graphite coated composite silicon carbon negative electrode material and preparation process thereof
CN117996038A
Method for fabricating graphite silicon-based composite negative-electrode material
WO2017008494A1
Cited By
Silicon-carbon negative electrode material based on spheroid phenolic resin and preparation method of silicon-carbon negative electrode material
CN121394373A
A silicon-carbon anode material based on spherical phenolic resin and its preparation method