Paper-based silicon carbon negative electrode as well as preparation method and application thereof
By using paper-based silicon carbon negative electrodes in lithium batteries and using plant fibers and conductive agents to construct a three-dimensional electrode conductive support framework, the structural problems caused by volume expansion of silicon carbon negative electrode materials in lithium batteries are solved, and the battery life is extended and the battery life is improved. Safety performance, suitable for large-scale production.
Patent Information
- Application Number
- CN202411150484.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
The huge volume expansion effect of silicon carbon anode material during the charging and discharging process of lithium batteries leads to structural rupture, powdering and inactivation, affecting the cycle life and performance stability of the battery, and the active substance falls off from the metal current collector, resulting in battery failure.
The paper-based silicon carbon negative electrode is used to prepare electrode slurry by fusing plant fibers as support frameworks with negative electrode active particles, conductive agents and binders. The self-supported three-dimensional porous structure electrode is prepared by using papermaking technology to avoid cracks in traditional coatings. and shedding problems, and are combined by carbon nanotubes and comb-shaped polymer dispersant to improve the conductive pathway and dispersion effect.
It realizes the self-support function of the electrode, extends the cycle life, avoids the fall of active substances and coating cracks, improves the safety performance and production cost of the battery, and is also suitable for large-scale continuous production.
Smart Images

Figure CN119050303A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery materials, and more specifically to a paper-based silicon-carbon negative electrode and a preparation method and application thereof. Background Art
[0002] With the deepening of lithium-ion battery research and development technology, traditional graphite negative electrode materials can no longer meet the needs of high-energy-density lithium-ion batteries, and new silicon-carbon negative electrode materials based on silicon have become a research and development hotspot. Silicon-carbon negative electrode materials have many advantages. For example, the theoretical capacity of silicon-carbon negative electrode is as high as 3580mAh / g, far exceeding the 372mAh / g of traditional graphite negative electrode. Silicon negative electrode materials can achieve faster lithium ion insertion and extraction, thus having the potential for fast charging. Silicon-based negative electrode materials have lower lithium insertion and extraction potentials. Compared with graphite negative electrodes, they can avoid surface lithium precipitation during charging and reduce the formation of lithium dendrites, thereby improving the safety performance of batteries. With the continuous advancement of technology, silicon-carbon negative electrode materials are expected to play a more important role in future battery technology.
[0003] The huge volume expansion effect of silicon negative electrode materials during the charging and discharging process of lithium batteries has also brought difficulties to its commercial application in the field of lithium batteries. The volume expansion of silicon will not only cause the structure of silicon-carbon negative electrode materials to crack, pulverize and deactivate, thus affecting the cycle life and performance stability of the battery, but may also cause the active material to fall off the metal current collector, causing the battery to fail.
[0004] Therefore, how to develop a paper-based silicon-carbon negative electrode and its preparation method and application that avoids cracks and shedding of traditional electrode coatings and increases the cycle life of the electrode is an urgent problem that technical personnel in this field need to solve. Summary of the invention
[0005] In view of this, the present invention provides a paper-based silicon-carbon negative electrode and a preparation method and application thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A paper-based silicon-carbon negative electrode comprises the following raw materials in parts by weight:
[0008] 70-90 parts of silicon-carbon material, 2-5 parts of conductive agent, 1-3 parts of dispersant, 120-360 parts of deionized water, 10-30 parts of graphite, 1-5 parts of binder, and 10-20 parts of dehydrated pulp.
[0009] Beneficial effects of the present invention:
[0010] The present invention uses flexible plant fibers as the supporting skeleton of the electrode sheet. The plant fibers are fused with negative electrode active particles, conductive agents, and binders to prepare electrode slurry, and then prepared into an integrated self-supporting silicon-carbon negative electrode through a papermaking process. The silicon-carbon negative electrode prepared by the method of the present invention has the flexibility and mechanical strength of paper, and is loaded with negative electrode active materials, and can be directly used as an electrode sheet.
[0011] Compared with the prior art, the present invention has the following advantages:
[0012] 1. The present invention constructs a three-dimensional electrode conductive support skeleton through plant fibers and conductive carbon materials. The prepared paper-based silicon-carbon negative electrode has a self-supporting function, and can omit the metal current collector and be directly used as an electrode.
[0013] 2. The paper-based silicon-carbon negative electrode prepared by the method of the present invention has a three-dimensional porous structure of paper in terms of microstructure. This structure can not only provide a favorable channel for the transmission of ions and electrons, but also provide a buffer space for the volume expansion of the silicon-based negative electrode material during the charging and discharging process, greatly extending the cycle life of the silicon-carbon negative electrode sheet, and will not cause problems such as the shedding of active materials of the traditional coated current collector electrode and cracks in the electrode coating.
[0014] 3. The raw materials used in the electrode preparation method of the present invention are widely available, with low production costs, and can be used to achieve continuous large-scale production with the help of papermaking technology.
[0015] Furthermore, the silicon-carbon material is a composite material of silicon and porous carbon prepared by CVD vapor deposition method.
[0016] Furthermore, the silicon content in the above silicon-carbon material is 10-60wt%, the remainder is porous carbon, and the particle size is 5-15μm.
[0017] Preferably, the silicon content in the silicon-carbon material is 40-55 wt %, and the remainder is porous carbon.
[0018] Furthermore, the conductive agent includes a first conductive agent and a second conductive agent, the mass ratio of the first conductive agent to the second conductive agent is (5-7):(3-5), the first conductive agent is one or more of Superp, acetylene black or Ketjen black, and the second conductive agent is a carbon nanotube material.
[0019] The beneficial effect of adopting the above further technical solution is: by compounding carbon nanotubes with conventional conductive agents and utilizing the high aspect ratio structure of carbon nanotubes, when a large volume change occurs after the silicon-carbon material is charged and discharged for a cycle, the conductive path between the materials can still be maintained.
[0020] Furthermore, the above-mentioned dispersant includes a comb-like polymer dispersant and sodium dodecylbenzene sulfonate, and the mass ratio of the comb-like polymer dispersant to the sodium dodecylbenzene sulfonate is (6-9):(1-4).
[0021] The beneficial effect of adopting the above further technical solution is: by compounding the comb-like polymer dispersant and sodium dodecylbenzene sulfonate, the comb-tooth structure of the comb-like polymer dispersant can produce steric hindrance between micro-nano inorganic particles, prevent the agglomeration of micro-nano particles, and have a good dispersing effect on micro-nanostructured silicon-carbon materials.
[0022] Furthermore, the comb-like polymer dispersant is the comb-like polymer super dispersant WANALYST DS360.
[0023] Furthermore, the graphite is natural graphite or artificial graphite, and the particle size is 10-20 μm.
[0024] Furthermore, the binder is a polyacrylic acid aqueous solution with a mass fraction of 5-10%.
[0025] Furthermore, the dewatered pulp is one of softwood or hardwood dewatered bleached pulp, the pulp fiber length is 1-4 mm, and the beating degree is 40-60° RS.
[0026] The beneficial effects of adopting the above further technical solution are as follows: the pulp fibers can be fibrillated by high beating degree, the hydroxyl binding sites on the fiber filaments can be increased, and the pulp fibers can be more tightly bonded after papermaking.
[0027] The present invention also provides a method for preparing a paper-based silicon-carbon negative electrode, comprising the following steps:
[0028] (1) Weighing the raw materials according to the above-mentioned paper-based silicon-carbon negative electrode, dividing the deionized water into a first part of deionized water and a second part of deionized water, the mass ratio of the first part of deionized water to the second part of deionized water is (100-300):(20-60);
[0029] (2) mixing and stirring the silicon-carbon material, the conductive agent, the dispersant and the first portion of deionized water to obtain a prefabricated slurry 1;
[0030] (3) mixing and stirring graphite, a binder and prefabricated slurry 1 to obtain prefabricated slurry 2;
[0031] (4) mixing the dewatered pulp with a second portion of deionized water and dispersing at high speed to obtain a pulp slurry;
[0032] (5) mixing the prefabricated slurry 2 and the paper pulp slurry to obtain a composite slurry;
[0033] (6) Filter the composite slurry to remove the filtrate, and perform hot pressing and drying on the filtered product, and roll pressing to obtain the above-mentioned paper-based silicon-carbon negative electrode.
[0034] Beneficial effects of the invention: The preparation method of the invention is simple, easy to operate, and suitable for wide production and application.
[0035] Furthermore, in step (2), the mixture is first stirred at a low speed of 500-1000 r / min for 3-5 min, and then stirred at a high speed of 2000-2500 r / min for 10-15 min.
[0036] Furthermore, in step (3), the stirring speed is 1500 r / min and the stirring time is 15 min.
[0037] Furthermore, in step (4), the dispersion speed is 1000-1500 r / min, and the dispersion time is 3-5 min.
[0038] Furthermore, in step (5), the stirring speed is 500-800 r / min and the stirring time is 5 min.
[0039] Furthermore, in step (6), the filter membrane used in the above filtration is made of PP or PA material, and the pore size of the filter membrane is 0.5-2 μm.
[0040] Furthermore, in step (6), the filtration time is within 2 minutes.
[0041] Furthermore, in step (6), the temperature of the hot pressing drying is 90-100° C., the time is 5-10 min, and the pressure is 500-800 kPa.
[0042] Furthermore, in step (6), the rolling speed is 0.54 m / min, and the rolling pressure is 25-30 t.
[0043] The present invention also provides an application of the paper-based silicon-carbon negative electrode or the paper-based silicon-carbon negative electrode prepared by the above method in a lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a physical picture of the composite slurry of the present invention.
[0045] Figure 2 This is a physical picture of the paper-based silicon-carbon negative electrode of the present invention.
[0046] Figure 3 This is a three-dimensional porous structure diagram of the paper-based silicon-carbon negative electrode of the present invention. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] Example 1
[0049] The method for preparing a paper-based silicon-carbon negative electrode comprises the following steps:
[0050] (1) Weigh 70 g of silicon-carbon material, 2 g of conductive agent, 1 g of dispersant, 120 g of deionized water, 30 g of graphite, 1 g of binder, and 10 g of dehydrated pulp, and divide the deionized water into a first part of 100 g of deionized water and a second part of 20 g of deionized water;
[0051] The silicon content in the silicon-carbon material is 50wt%, the remainder is porous carbon, and the particle size is 5-15μm;
[0052] The conductive agent includes a first conductive agent and a second conductive agent, the mass ratio of the first conductive agent to the second conductive agent is 5:3, the first conductive agent is Superp, and the second conductive agent is a carbon nanotube material;
[0053] The dispersant includes a comb-like polymer dispersant and sodium dodecylbenzene sulfonate, and the mass ratio of the comb-like polymer dispersant to the sodium dodecylbenzene sulfonate is 6:1;
[0054] The comb-like polymer dispersant is the comb-like polymer superdispersant WANALYST DS360;
[0055] The graphite is natural graphite with a particle size of 10-20 μm;
[0056] The binder is a polyacrylic acid aqueous solution with a mass fraction of 5%;
[0057] Dewatered pulp is a type of softwood dewatered bleached pulp, with a pulp fiber length of 1-4 mm and a beating degree of 40°RS;
[0058] (2) mixing the silicon-carbon material, the conductive agent, the dispersant and the first portion of deionized water with a planetary mixer, first stirring at a low speed of 500 r / min for 3 min, then stirring at a high speed of 2000 r / min for 10 min, to obtain a prefabricated slurry 1;
[0059] (3) mixing graphite, binder and prefabricated slurry 1 with a planetary mixer at a stirring speed of 1500 r / min for 15 min to obtain prefabricated slurry 2;
[0060] (4) mixing the dehydrated pulp and the second portion of deionized water and dispersing them in a high-speed disperser at a dispersing speed of 1000 r / min for a dispersing time of 5 min to obtain a pulp slurry;
[0061] (5) Prefabricated slurry 2 and paper pulp slurry are mixed and stirred by a planetary mixer at a stirring speed of 500 r / min for 5 min to obtain a composite slurry;
[0062] (6) The composite slurry is filtered under negative pressure in a vacuum filter with a vacuum degree of 10 -5 Pa, the filtration time is 1 min, the filtrate is removed, the filter membrane used for filtration is made of PP material, the filter membrane pore size is 0.5 μm, and the filtered product is hot-pressed and dried at a temperature of 90°C, a time of 5 min, a pressure of 800 kPa, a rolling speed of 0.54 m / min, and a rolling pressure of 30 t to obtain a paper-based silicon-carbon negative electrode.
[0063] Example 2
[0064] The method for preparing a paper-based silicon-carbon negative electrode comprises the following steps:
[0065] (1) Weigh 80 g of silicon-carbon material, 3 g of conductive agent, 2 g of dispersant, 240 g of deionized water, 20 g of graphite, 3 g of binder, and 15 g of dehydrated pulp, and divide the deionized water into a first part of 200 g of deionized water and a second part of 40 g of deionized water;
[0066] The silicon content in the silicon-carbon material is 50wt%, the remainder is porous carbon, and the particle size is 5-15μm;
[0067] The conductive agent is a first conductive agent and a second conductive agent, the mass ratio of the first conductive agent to the second conductive agent is 6:4, the first conductive agent is acetylene black, and the second conductive agent is a carbon nanotube material
[0068] The dispersant includes a comb-like polymer dispersant and sodium dodecylbenzene sulfonate, and the mass ratio of the comb-like polymer dispersant to the sodium dodecylbenzene sulfonate is 7:3;
[0069] The comb-like polymer dispersant is the comb-like polymer superdispersant WANALYST DS360;
[0070] The graphite is artificial graphite with a particle size of 10-20 μm;
[0071] The binder is a polyacrylic acid aqueous solution with a mass fraction of 7%;
[0072] The dewatered pulp is dewatered bleached hardwood pulp, with a pulp fiber length of 1-4 mm and a beating degree of 50°RS;
[0073] (2) mixing the silicon-carbon material, the conductive agent, the dispersant and the first portion of deionized water with a planetary mixer, first stirring at a low speed of 800 r / min for 4 min, then stirring at a high speed of 2300 r / min for 13 min, to obtain a prefabricated slurry 1;
[0074] (3) mixing graphite, binder and prefabricated slurry 1 with a planetary mixer at a stirring speed of 1500 r / min for 15 min to obtain prefabricated slurry 2;
[0075] (4) mixing the dehydrated pulp and the second portion of deionized water and dispersing them in a high-speed disperser at a dispersing speed of 1200 r / min for a dispersing time of 4 min to obtain a pulp slurry;
[0076] (5) Prefabricated slurry 2 and paper pulp slurry were mixed by a planetary mixer at a stirring speed of 700 r / min for a stirring time of 5 min to obtain a composite slurry;
[0077] (6) The composite slurry is filtered under negative pressure in a vacuum filter with a vacuum degree of 10 -5 Pa, the filtration time is 1.5min, the filtrate is removed, the filter membrane used for filtration is made of PA material, the filter membrane pore size is 1μm, and the filtered product is hot-pressed and dried at a temperature of 95°C, a time of 7min, a pressure of 600kPa, a rolling speed of 0.54m / min, and a rolling pressure of 25t to obtain a paper-based silicon-carbon negative electrode.
[0078] Example 3
[0079] The method for preparing a paper-based silicon-carbon negative electrode comprises the following steps:
[0080] (1) Weigh 90 g of silicon-carbon material, 5 g of conductive agent, 3 g of dispersant, 360 g of deionized water, 10 g of graphite, 5 g of binder, and 20 g of dehydrated pulp, and divide the deionized water into a first part of 300 g of deionized water and a second part of 60 g of deionized water;
[0081] The silicon content in the silicon-carbon material is 55wt%, the remainder is porous carbon, and the particle size is 5-15μm;
[0082] The conductive agent includes a first conductive agent and a second conductive agent, the mass ratio of the first conductive agent to the second conductive agent is 7:5, the first conductive agent is Ketjen black, and the second conductive agent is a carbon nanotube material;
[0083] The dispersant includes a comb-shaped polymer dispersant and sodium dodecylbenzene sulfonate, and the mass ratio of the comb-shaped polymer dispersant to the sodium dodecylbenzene sulfonate is 9:4;
[0084] The comb-like polymer dispersant is the comb-like polymer superdispersant WANALYST DS360;
[0085] The graphite is natural graphite with a particle size of 10-20 μm;
[0086] The binder is a polyacrylic acid aqueous solution with a mass fraction of 10%;
[0087] The dewatered pulp is dewatered bleached hardwood pulp, with a pulp fiber length of 1-4 mm and a beating degree of 60°RS;
[0088] (2) mixing the silicon-carbon material, the conductive agent, the dispersant and the first portion of deionized water with a planetary mixer, first stirring at a low speed of 1000 r / min for 5 min, then stirring at a high speed of 2500 r / min for 15 min, to obtain a prefabricated slurry 1;
[0089] (3) mixing graphite, binder and prefabricated slurry 1 with a planetary mixer at a stirring speed of 1500 r / min for 15 min to obtain prefabricated slurry 2;
[0090] (4) mixing the dehydrated pulp and the second portion of deionized water and dispersing them in a high-speed disperser at a dispersing speed of 1500 r / min for a dispersing time of 3 min to obtain a pulp slurry;
[0091] (5) Prefabricated slurry 2 and paper pulp slurry are mixed by a planetary mixer at a stirring speed of 800 r / min for a stirring time of 5 min to obtain a composite slurry;
[0092] (6) The composite slurry is filtered under negative pressure in a vacuum filter with a vacuum degree of 10 -5 Pa, the filtration time is 2min, the filtrate is removed, the filter membrane used for filtration is made of PP material, the filter membrane pore size is 2μm, and the filtered product is hot-pressed and dried at a temperature of 100°C, a time of 10min, a pressure of 500kPa, a rolling speed of 0.54m / min, and a rolling pressure of 20t to obtain a paper-based silicon-carbon negative electrode.
[0093] A silicon-carbon material with a silicon content of 50 wt % was used as an active material, and a slurry was prepared according to the scheme of Example 1 and coated on a copper foil current collector with a coating thickness of 200 μm to prepare a current collector coated electrode.
[0094] The current collector coated electrode prepared as above and the paper-based electrode prepared in the manner of Examples 1-3 were prepared into button-type standard half-cells under the same conditions, and charge and discharge cycle tests were carried out at a current density of 100 mAh / g and a voltage of 0.005-1.5 V. The test results are shown in Table 1.
[0095] Table 1 Performance comparison results
[0096]
[0097]
[0098] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A paper-based silicon-carbon negative electrode, characterized in that: The invention comprises the following raw materials in parts by weight: 70-90 parts of silicon-carbon material, 2-5 parts of conductive agent, 1-3 parts of dispersant, 120-360 parts of deionized water, 10-30 parts of graphite, 1-5 parts of binder, and 10-20 parts of dehydrated pulp.
2. A paper-based silicon-carbon negative electrode according to claim 1, characterized in that: The silicon content in the silicon-carbon material is 10-60wt% and the particle size is 5-15μm.
3. The paper-based silicon-carbon negative electrode according to claim 1, characterized in that: The conductive agent includes a first conductive agent and a second conductive agent, the mass ratio of the first conductive agent to the second conductive agent is (5-7):(3-5), the first conductive agent is one or more of Superp, acetylene black or Ketjen black, and the second conductive agent is a carbon nanotube material.
4. The paper-based silicon-carbon negative electrode according to claim 1, characterized in that: The dispersant comprises a comb-like polymer dispersant and sodium dodecylbenzene sulfonate, and the mass ratio of the comb-like polymer dispersant to the sodium dodecylbenzene sulfonate is (6-9):(1-4).
5. The paper-based silicon-carbon negative electrode according to claim 1, characterized in that: The graphite is natural graphite or artificial graphite, and the particle size is 10-20 μm.
6. The paper-based silicon-carbon negative electrode according to claim 1, characterized in that: The binder is a polyacrylic acid aqueous solution with a mass fraction of 5-10%.
7. The paper-based silicon-carbon negative electrode according to claim 1, characterized in that: The dewatered pulp is one of softwood or hardwood dewatered bleached pulps, the pulp fiber length is 1-4 mm, and the beating degree is 40-60° RS.
8. A method for preparing a paper-based silicon-carbon negative electrode, characterized in that: The following steps are involved: (1) Weighing the raw materials according to the paper-based silicon-carbon negative electrode according to any one of claims 1 to 7, dividing the deionized water into a first part of deionized water and a second part of deionized water, the mass ratio of the first part of deionized water to the second part of deionized water being (100-300):(20-60); (2) mixing and stirring the silicon-carbon material, the conductive agent, the dispersant and the first portion of deionized water to obtain a prefabricated slurry 1; (3) mixing and stirring graphite, a binder and prefabricated slurry 1 to obtain prefabricated slurry 2; (4) mixing the dewatered pulp with a second portion of deionized water and dispersing at high speed to obtain a pulp slurry; (5) mixing the prefabricated slurry 2 and the paper pulp slurry to obtain a composite slurry; (6) Filter the composite slurry to remove the filtrate, and perform hot pressing and drying on the filtered product, and roll pressing to obtain the paper-based silicon-carbon negative electrode.
9. The paper-based silicon-carbon negative electrode according to claim 1, characterized in that: In step (2), the mixture is first stirred at a low speed of 500-1000 r / min for 3-5 min, and then stirred at a high speed of 2000-2500 r / min for 10-15 min.
10. Use of the paper-based silicon-carbon negative electrode according to any one of claims 1 to 7 or the paper-based silicon-carbon negative electrode prepared by the method according to claim 8 or 9 in a lithium-ion battery.
Citation Information
Cited By
Flexible negative electrode paper for solid-state battery as well as preparation method and application of flexible negative electrode paper
CN119786543A
Flexible negative electrode paper for solid-state batteries and preparation method and application thereof