A spin-optimized layered oxide cathode material, its preparation method, and a sodium-ion battery.
By introducing specific metal elements into the cathode material of sodium-ion batteries and regulating the spin electronic state and MO orbital hybridization of Fe, the problems of energy density and cycle stability of sodium-ion batteries have been solved, and the preparation and application of high-performance sodium-ion batteries have been realized.
Patent Information
- Application Number
- CN202411176933.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing sodium-ion battery cathode materials have low energy density and poor cycle stability. Existing doping techniques are difficult to control effectively, and coating techniques increase costs and have limited effectiveness.
Introducing specific metal elements with strong electron-donating capabilities, such as Ni, Mn, Cu, Ti, Ca, Mg, Zn, and Al, into layered cathode materials can improve the energy density and structural stability of the material by controlling the spin electronic state distribution of Fe and optimizing the MO orbital hybridization.
This improved the energy density and cycle stability of the material, reduced production costs, facilitated large-scale production, and enabled the application of high-performance sodium-ion batteries.
Smart Images

Figure CN119050345B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a spin-optimized layered oxide cathode material, its preparation method, and a sodium-ion battery, belonging to the field of sodium-ion battery technology. Background Technology
[0002] Sodium-ion batteries, with their low cost, high safety, and wide temperature range, play a crucial role in building the energy internet and promoting the green and low-carbon transformation of energy, making them a key development target in the green energy storage market. However, their relatively low energy density is a bottleneck restricting the industrialization of sodium-ion batteries. Therefore, researching and developing a mature sodium-ion battery support system that overcomes this bottleneck is of significant strategic importance. Cathode materials, as a key factor determining battery performance and cost, are the core of this support system's research.
[0003] In recent years, layered cathode materials for sodium-ion batteries (Na) have been developing rapidly. x TMO2 (TM = Ti, V, Cr, Mn, Fe, Co, Ni, etc.) has attracted much attention due to its high theoretical specific capacity, high operating voltage, and ease of large-scale production and preparation. Meanwhile, the activation and stabilization mechanism of anionic oxygen under high voltage has become a well-known optimal method for constructing high-capacity layered cathode materials. Existing technologies mainly employ multi-element doping and the construction of various types of coating layers to regulate and optimize the internal structure and interfaces of layered cathode materials. However, existing doping techniques struggle to achieve the control of matrix structural elements by doping elements; furthermore, existing coating layer techniques cannot achieve targeted design and optimization of the material's internal structure, limiting their effectiveness in improving energy density. Furthermore, the additional coating technology increases the application cost of the material, thus exhibiting certain limitations. Summary of the Invention
[0004] In view of this, the purpose of this invention is to provide a spin-optimized layered oxide cathode material, a preparation method, and a sodium-ion battery. By introducing specific dopants with strong electron-donating capabilities into the layered cathode material, the spin electronic state distribution of Fe is controlled, thereby solving the problems of poor cycle stability and limited energy density of layered cathode materials. Specifically, metal dopants can enhance oxygen octahedral coordination and reduce Fed. 5 Spin degree promotes electron-ion transport rate and improves the rate performance of materials; spin optimization promotes MO orbital hybridization in materials and improves the structural stability of materials during sodium insertion and extraction processes; at the same time, by regulating the electron distribution of Fe 3d, more active Fe is excited to participate in charge compensation, effectively improving the energy density of materials.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows.
[0006] A spin-optimized layered oxide cathode material, the chemical formula of which is Nax M a N b Fe c O2, wherein M is one or more of Ni, Mn, Cu, Ti, Ca, Mg, Zn, and Al, and N is one or more of Ir, Mo, Ru, Y, Nb, and Zr, wherein 0.2 < x < 1; 0 < a ≤ 0.65; 0 < b ≤ 0.1; 0.3 ≤ c ≤ 0.6, and the values of x, a, b, and c satisfy the valence equilibrium of the chemical formula; the material has a layered structure, and N is doped into the layered structure, forming MO inside the material. lat O lat -N structure.
[0007] Preferably, the material belongs to the hexagonal or rhombohedral crystal system, with a space group of [missing information].
[0008] Preferably, the bond energy of NO in the material is 700–1000 kJ / mol. -1 .
[0009] Preferably, 0.6 < x < 1; 0.3 < a ≤ 0.65; 0.05 ≤ b ≤ 0.1; 0.3 ≤ c ≤ 0.6.
[0010] Preferably, the M element is one or more of Ni, Mn, Mg and Al, and the N element is one or more of Mo, Ru and Nb.
[0011] Preferably, the particle size of the material is 1–5 μm.
[0012] A method for preparing a spin-optimized layered oxide cathode material according to the present invention includes the following steps:
[0013] The M source, N source, iron source and 5% to 10% excess sodium source were weighed according to the stoichiometric ratio, mixed, ball-milled, pressed into sheets, calcined at 600 to 1000°C for 10 to 36 hours, and cooled after calcination to obtain a spin-optimized layered oxide cathode material.
[0014] Preferably, the M source is one or more of an oxide, carbonate, hydroxide, and acetate of element M; and the N source is one or more of an oxide, carbonate, hydroxide, and acetate of element N.
[0015] Preferably, the ball milling is carried out in an inert gas atmosphere, with a milling speed of 400–1000 rpm and a milling time of 3–10 h. More preferably, the milling speed is 400–600 rpm and the milling time is 3–6 h.
[0016] Preferably, when compressing into sheets, the pressure is 5-20 MPa and the time is 5-10 min.
[0017] Preferably, during calcination, the atmosphere is air, oxygen, or nitrogen, the temperature is 800–1000°C, and the time is 10–24 hours. More preferably, during calcination, the atmosphere is air.
[0018] Preferably, the heating rate during calcination is 1–10 °C / min, and the cooling rate after calcination is 5–50 °C / min. More preferably, the heating rate during calcination is 2–5 °C / min, and the cooling rate after calcination is 5–20 °C / min.
[0019] A sodium-ion battery, wherein the positive electrode of the battery is a spin-optimized layered oxide positive electrode material as described in this invention.
[0020] Beneficial effects
[0021] This invention provides a spin-optimized layered oxide cathode material. By introducing specific metal elements into the Fe-based layered cathode material, the local charge structure and spin electronic states of Fe (electron distribution in Fe 3d) are controlled. This excites more Fe to participate in redox reactions and charge compensation, thereby increasing the material's energy density. Simultaneously, it optimizes the Fe-O octahedral coordination structure, enhances MO bond bonding within the layered material, and regulates the electrostatic forces between Na-Fe-O bonds, thereby improving interlayer structural stability and cycle life.
[0022] This invention provides a method for preparing spin-optimized layered oxide cathode materials. The preparation process is simple and controllable, the reaction conditions are mild, the cost is low, and it is easy to achieve large-scale industrial production.
[0023] This invention provides a sodium-ion battery. The positive electrode of the battery uses the spin-optimized layered oxide positive electrode material described in this invention, which has excellent energy density and cycle stability, and has good application prospects in practical applications. Attached Figure Description
[0024] Figure 1 This is an X-ray powder diffraction test pattern of Embodiment 1 of the present invention.
[0025] Figure 2 This is a scanning electron microscope (SEM) image of the powder prepared in Example 1 of this invention.
[0026] Figure 3 This is an X-ray powder diffraction test pattern of Embodiment 2 of the present invention.
[0027] Figure 4 This is a scanning electron microscope (SEM) image of the powder prepared in Example 2 of this invention. Detailed Implementation
[0028] The present invention will be further described in detail below with reference to specific embodiments.
[0029] In the following examples and comparative examples, the obtained positive electrode material was mixed with carbon black and polyvinylidene fluoride binder at a mass ratio of 7:2:1 to form a slurry, which was then coated onto an aluminum foil current collector. The slurry was dried in a vacuum drying oven at 80°C for 24 hours, cut into sheets, and used as the working electrode. In a glove box under an argon atmosphere, using a sodium sheet as the counter electrode, the positive electrode shell, negative electrode shell, glass fiber separator, sodium sheet, and electrolyte were assembled into a CR2025 type button cell according to the correct operating procedures. After the assembled battery was allowed to stand for 24 hours, constant current charge-discharge tests and rate performance tests were performed in the Blue Electric testing system, with a voltage range of 2.0-4.5V.
[0030] Example 1
[0031] Step (1): Weigh 10.5 mmol sodium carbonate, 2 mmol nickel oxide, 4 mmol manganese trioxide, 4 mmol ferric oxide, and 1 mmol niobium oxide and mix them in a ball mill jar; transfer the ball mill jar to a glove box to purge the inert atmosphere; set the ball mill speed to 600 rpm and the ball milling time to 180 min to obtain the mixed material. Nickel oxide and manganese trioxide are used as M sources, and niobium oxide is used as N source.
[0032] Step (2): The above mixed material was pressed at 15 MPa for 5 min, and after being pressed into sheets, it was placed in a muffle furnace for calcination; the calcination temperature was 800℃, the calcination time was 10 h, the heating rate was 5℃ / min, and the cooling rate was 5℃ / min; a spin-optimized layered oxide cathode material, O3-NaNi, was obtained by grinding. 0.1 Mn 0.4 Fe 0.4 Nb 0.1 O2.
[0033] Figure 1 The figure shows the XRD test results of the cathode material. From the figure, it can be seen that the prepared material belongs to... The space group exhibits good crystallinity.
[0034] Figure 2 The SEM test results of the cathode material show that the morphology of the prepared material is a sheet-like structure with a particle size of 1 μm.
[0035] Example 2
[0036] Unlike Example 1, in this example, the ratio of nickel, manganese, iron, and niobium added in step 1 is adjusted to 1:5:3:1, while the conditions of all other steps remain unchanged, resulting in a spin-optimized layered oxide cathode material, O3-NaNi. 0.1 Mn 0.5 Fe 0.3 Nb 0.1 O2.
[0037] Figure 3 The XRD test results of the cathode material indicate that the material obtained in Example 2 belongs to... The space group exhibits good crystallinity.
[0038] Figure 4 The SEM test results of the cathode material show that the morphology of the prepared material is a sheet-like structure with a particle size of 1 μm.
[0039] Example 3
[0040] Unlike Example 1, in this example, the ratio of nickel, manganese, iron and niobium added in step 1 is adjusted to 1:3:5:1, while the conditions of the other steps remain unchanged.
[0041] Example 4
[0042] Unlike Example 1, in this example, the ratio of nickel, manganese, iron and niobium added in step 1 is adjusted to 1:3:6:1, while the conditions of the other steps remain unchanged.
[0043] Example 5
[0044] Unlike Example 1, in this example, the N-source niobium oxide in step 1 is adjusted to N-source zirconium oxide with similar properties, and the ratio of nickel, manganese, iron and zirconium is adjusted to 1:4:4:1, while the conditions of the other steps remain unchanged.
[0045] Example 6
[0046] Unlike Example 5, in this example, the ratio of nickel, manganese, iron and zirconium added in step 1 is adjusted to 1:5:3:1, while the conditions of the other steps remain unchanged.
[0047] Example 7
[0048] Unlike Example 5, in this example, the ratio of nickel, manganese, iron and zirconium added in step 1 is adjusted to 1:3:5:1, while the conditions of the other steps remain unchanged.
[0049] Example 8
[0050] Unlike Example 5, in this example, the ratio of nickel, manganese, iron and zirconium added in step 1 is adjusted to 1:3:6:1, while the conditions of the other steps remain unchanged.
[0051] Example 9
[0052] Unlike Example 1, in this example, the N-source niobium oxide in step 1 is adjusted to N-source molybdenum oxide with similar properties, and the ratio of nickel, manganese, iron and molybdenum is adjusted to 1:4:4:1, while the conditions of the other steps remain unchanged.
[0053] Example 10
[0054] Unlike Example 9, in this example, the ratio of nickel, manganese, iron and molybdenum added in step 1 is adjusted to 1:5:3:1, while the conditions of the other steps remain unchanged.
[0055] Example 11
[0056] Unlike Example 9, in this example, the ratio of nickel, manganese, iron and molybdenum added in step 1 is adjusted to 1:3:5:1, while the conditions of the other steps remain unchanged.
[0057] Example 12
[0058] Unlike Example 9, in this example, the ratio of nickel, manganese, iron and molybdenum added in step 1 is adjusted to 1:3:6:1, while the conditions of the other steps remain unchanged.
[0059] Example 13
[0060] Unlike Example 1, in this example, the N-source niobium oxide in step 1 is adjusted to N-source yttrium oxide with similar properties, and the ratio of nickel, manganese, iron and yttrium is adjusted to 1:4:4:1, while the conditions of the other steps remain unchanged.
[0061] Example 14
[0062] Unlike Example 13, in this example, the ratio of nickel, manganese, iron and yttrium in step 1 is adjusted to 1:5:3:1, while the conditions of the other steps remain unchanged.
[0063] Example 15
[0064] Unlike Example 13, in this example, the ratio of nickel, manganese, iron and yttrium in step 1 is adjusted to 1:3:5:1, while the conditions of the other steps remain unchanged.
[0065] Example 16
[0066] Unlike Example 13, in this example, the ratio of nickel, manganese, iron and yttrium in step 1 is adjusted to 1:3:6:1, while the conditions of the other steps remain unchanged.
[0067] Comparative Example 1
[0068] Unlike Example 1, only the M source is added, and the N source for niobium oxide is not added. The ratio of nickel, manganese and iron is adjusted to 1:5:4. The rest is the same as in Example 1.
[0069] Comparative Example 2
[0070] Unlike Example 1, the ratio of nickel, manganese, iron and niobium added in step 1 of this comparative example is adjusted to 1:1:7:1, and the rest is the same as in Example 1.
[0071] Comparative Example 3
[0072] Unlike Example 1, the ratio of nickel, manganese, iron and niobium added in step 1 of this comparative example is adjusted to 1:4.9:4:0.1, and the rest is the same as in Example 1.
[0073] Performance testing:
[0074] Sodium-ion batteries assembled with the spin-optimized Fe-based substrate cathode materials obtained in Examples 1-16 and the comparative examples were subjected to high-voltage cycling performance tests. The charge / discharge cutoff voltage range was 2.0-4.5V. The discharge capacity in the first cycle and the capacity retention rate after 50 cycles were tested. The test results are shown in Table 1.
[0075] Table 1
[0076]
[0077]
[0078] Theoretical calculations and analyses were performed on Examples 1-4 and Comparative Example 1: From the local charge density distribution (ELF), it can be seen that the local charge density of the surrounding oxygen is enhanced after Nb doping, i.e., E... F The nearby O 2p band significantly contributes to the stability of the structure and the modulation of the spin state of neighboring Fe. Density of states (DOS) calculations show that Nb doping results in stronger metal-oxygen (Nb-O) orbital hybridization. Synchrotron radiation analysis of Fe reveals a significant shift in the characteristic peaks of Fe after Nb doping, indicating that Nb doping enables the modulation of Fe spin electronic states. This allows for spin optimization of the local structure of layered cathode materials, improving reversible capacity and cycle stability. Furthermore, the influence on Fe spin increases with increasing Nb doping ratio.
[0079] Theoretical calculations and analyses of Examples 9-12, Examples 13-16, and Comparative Example 1 show that after doping with different types of strong electron-donating elements, the local charge density around oxygen in the material increases. At the same time, the density of states of Fe changes significantly, and characteristic peaks of different spin states appear. Electrochemical data analysis also shows that the redox reaction of Fe changes during the charge and discharge process after doping. That is, the regulation of the spin electronic state structure of Fe affects the actual electrochemical behavior, thereby affecting the energy density of the material. Moreover, the performance of the material after regulation is related to the doping ratio.
[0080] In summary, the invention includes, but is not limited to, the above embodiments. Any equivalent substitutions or partial improvements made under the spirit and principles of this invention shall be considered to be within the protection scope of this invention.
Claims
1. A spin-optimized layered oxide cathode material, characterized in that: The chemical formula of the material is Na. x M a N b Fe c O2, wherein M is one or more of Ni, Mn, Cu, Ti, Ca, Mg, Zn, and Al, and N is one or more of Ir, Mo, Ru, Y, Nb, and Zr, wherein 0.2 < x < 1; 0 < a ≤ 0.65; 0 < b ≤ 0.1; 0.3 ≤ c ≤ 0.6, and the values of x, a, b, and c satisfy the valence equilibrium of the chemical formula; the material has a layered structure, and N is doped into the layered structure, forming MO inside the material. lat O lat -N structure; By introducing specific metal elements into Fe-based substrate cathode materials, the local charge structure and spin electronic state of Fe can be controlled. After element doping, an enhanced local charge density appears around oxygen, and the density of states of Fe changes significantly, with characteristic peaks of the spin state appearing. The material is prepared by the following method, the steps of which include: mixing M source, N source, iron source and 5%~10% excess sodium source weighed according to stoichiometric ratio, ball milling in an inert gas atmosphere, pressing into sheets, calcining at 600~1000℃ for 10~36h, cooling after calcination, to obtain a spin-optimized layered oxide cathode material.
2. The spin-optimized layered oxide cathode material as described in claim 1, characterized in that: The material belongs to the hexagonal or rhombohedral crystal system, with space group [missing information]. P 63 mmc / R m.
3. The spin-optimized layered oxide cathode material as described in claim 1, characterized in that: The bonding energy of NO in the material is 700~1000 KJ•mol. -1 .
4. The spin-optimized layered oxide cathode material as described in claim 1, characterized in that: 0.6<x<1; 0.3 < a ≤ 0.65; 0.05 ≤ b ≤ 0.1; 0.3 ≤ c ≤ 0.
6.
5. The spin-optimized layered oxide cathode material as described in claim 1, characterized in that: The element M is one or more of Ni, Mn, Mg and Al, and the element N is one or more of Mo, Ru and Nb.
6. A spin-optimized layered oxide cathode material as described in any one of claims 1 to 5, characterized in that: The particle size of the material is 1~5μm.
7. A method for preparing a spin-optimized layered oxide cathode material as described in any one of claims 1 to 6, characterized in that: The method steps include: The M source, N source, iron source and 5%~10% excess sodium source were weighed according to the stoichiometric ratio, mixed, ball-milled in an inert gas atmosphere, pressed into sheets, calcined at 600~1000℃ for 10~36h, and cooled after calcination to obtain a spin-optimized layered oxide cathode material.
8. The method for preparing a spin-optimized layered oxide cathode material as described in claim 7, characterized in that: The M source is one or more of the oxides, carbonates, hydroxides, and acetates of element M; the N source is one or more of the oxides, carbonates, hydroxides, and acetates of element N; During ball milling, the ball milling speed is 400~1000 rpm; the ball milling time is 3~10 hours. When compressing into tablets, the pressure is 5~20MPa and the time is 5~10min; During calcination, the atmosphere is air, oxygen, or nitrogen, the temperature is 800~1000℃, and the time is 10~24h; The heating rate during calcination is 1~10℃ / min, and the cooling rate after calcination is 5~50℃ / min.
9. The method for preparing a spin-optimized layered oxide cathode material as described in claim 8, characterized in that: The ball milling speed is 400~600 rpm; the ball milling time is 3~6 hours; During calcination, the atmosphere is air; The heating rate during calcination is 2~5℃ / min, and the cooling rate after calcination is 5~20℃ / min.
10. A sodium-ion battery, characterized in that: The positive electrode of the battery is a spin-optimized layered oxide positive electrode material according to any one of claims 1 to 6.
Citation Information
Patent Citations
Layered oxide positive electrode doped with elements on sodium layer and application of layered oxide positive electrode and sodium ion battery
CN118315579A