Preparation method and application of hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane
By using the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film as the zinc negative electrode interface protective layer in aqueous zinc ion batteries, the problem of zinc ion transport and deposition inhomogeneity is solved, and the cycle life and electrochemistry of the battery are significantly improved. performance.
Patent Information
- Application Number
- CN202411166083.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing nanoscale thickness zinc negative electrode artificial interface protective layer cannot effectively ensure the rapidity of zinc ion transport kinetics and the uniformity of zinc ion deposition, affecting the cycle life of aqueous zinc ion batteries.
The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is used as the interface protective layer of the zinc negative electrode. By using surfactant as a soft template at the air-water interface, LaF3 is induced to connect to a dense and uniform nano film to form a crystalline structure. and CF-LaF3 membranes of continuous zinc transport channels promote zinc ion transport and deposition.
It significantly improves the transmission kinetics and deposition uniformity of zinc ions, extends the cycle life of the battery, and inhibits the corrosion of zinc negative electrode and active water, improving electrochemical performance.
Smart Images

Figure CN119050362A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal zinc negative electrodes of aqueous zinc ion batteries. Background Art
[0002] Aqueous zinc-ion batteries have become a research hotspot for more and more scientific researchers due to their high safety and low cost. However, the slow zinc ion transmission dynamics and uneven electric field distribution on the zinc negative electrode surface will lead to uncontrolled dendrite growth, which seriously affects the cycle life of aqueous zinc-ion batteries. In order to effectively inhibit the dendrite growth problem from the source, the existing technology mostly constructs an artificial interface protective layer of the zinc negative electrode on the zinc surface, but the thickness of the existing zinc negative electrode artificial interface protective layer is usually at the micron level, which will lengthen the transmission path of zinc ions and affect the volume energy density of the battery. Even if a protective layer with nanometer thickness is prepared, it cannot effectively guarantee fast zinc ion transmission dynamics and uniform zinc ion deposition. Summary of the invention
[0003] The present invention aims to solve the problem that the existing protective layer with nanometer thickness cannot effectively guarantee the rapid zinc ion transmission dynamics and uniform zinc ion deposition, and further provide a preparation method and application of a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film.
[0004] A method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is carried out according to the following steps:
[0005] 1. Add perfluorotetradecanoic acid to a mixed solution of chloroform and methanol, stir and dissolve to obtain a perfluorotetradecanoic acid solution; add lanthanum nitrate powder to secondary water, stir and dissolve to obtain a lanthanum nitrate aqueous solution; add sodium fluoride powder to secondary water, stir and dissolve to obtain a sodium fluoride aqueous solution;
[0006] 2. Under the condition of a droplet acceleration rate of 2 μL / s to 5 μL / s, a perfluorotetradecanoic acid solution is added dropwise to the surface of the lanthanum nitrate aqueous solution, and then under the condition of an injection rate of 1 mL / s to 2 mL / s, a sodium fluoride aqueous solution is injected into the bottom of the solution and allowed to stand at room temperature to obtain a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film at the air-water interface;
[0007] The molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to perfluorotetradecanoic acid in the perfluorotetradecanoic acid solution is 1:(0.0001-0.0002); the molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to sodium fluoride in the sodium fluoride aqueous solution is 1:(3-4).
[0008] Application of hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane, which is used as the interfacial protective layer of zinc negative electrode in aqueous zinc ion batteries.
[0009] The beneficial effects of the present invention are:
[0010] The present invention uses a surfactant as a soft template to induce LaF3 to connect into a dense and uniform nanofilm at the air-water interface, and provides an organic-inorganic composite material and a hydrophobic zinc ion conductor membrane CF-LaF3 that can be prepared on a large area for zinc negative electrode protection of aqueous zinc ion batteries. It should be emphasized that the template agent perfluorotetradecanoic acid used in the present invention induces lanthanum fluoride to form a continuous nanofilm, which has a crystalline structure and a continuous zinc transfer channel. Its composition structure is perfluorotetradecanoic acid on the surface and lanthanum fluoride at the bottom. The surface perfluorotetradecanoic acid active agent monolayer is exposed, which has hydrophobicity and promotes Zn(H2O)6 2+ After desolvation, the lanthanum fluoride at the bottom has a uniform zinc ion transport channel, which accelerates zinc ion transport and induces uniform zinc ion deposition. The two components synergistically enhance the zinc ion transport kinetics.
[0011] The present invention transfers the CF-LaF3 nanofilm to the surface of the zinc foil. Due to the zinc-philic transmission channel inside the CF-LaF3 nanofilm, CF-LaF3 as a zinc negative electrode protective layer can significantly improve the Zn 2+ Transfer dynamics. In addition, the hydrophobic properties of the CF-LaF3 nanofilm surface accelerate the desolvation process of interfacial zinc ions, and further prevent the direct contact between the zinc negative electrode and active water, inhibiting the corrosion of the zinc surface by the electrolyte. Due to the dense uniformity of the CF-LaF3 nanofilm and the special zinc transmission path, the overall electrochemical performance of the CF-LaF3 / Zn electrode is significantly improved. The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of zinc foil with a thickness of 150μm to 250μm to obtain CF-LaF3 / Zn. CF-LaF3 / Zn is used as the positive and negative electrodes to assemble a CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery. At a current density of 5mA / cm 2 and area capacity of 1 mAh / cm 2 The symmetrical battery can be stably cycled for more than 4000h under the condition of 100% hygroscopic conditions. The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of a thin zinc foil with a thickness of 30μm to obtain CF-LaF3 / Zn. CF-LaF3 / Zn is used as the positive and negative electrodes to assemble the CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery. At a current density of 2mA / cm 2 And the area capacity is 10mAh / cm 2Under the condition that the zinc utilization rate is 67%, the symmetrical battery can stably cycle for more than 240 hours; the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of zinc foil with a thickness of 150μm to 250μm to obtain CF-LaF3 / Zn, and the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of titanium foil with a thickness of 5μm to 15μm to obtain CF-LaF3 / Ti. CF-LaF3 / Ti is used as the positive electrode and CF-LaF3 / Zn is used as the negative electrode to assemble the CF-LaF3 / Zn||CF-LaF3 / Ti half-cell. At a current density of 5mA / cm 2 And the area capacity is 1mAh / cm 2 The half-cell can be stably cycled for more than 6000 times, with a cumulative cycle area capacity of 6000mAh / cm 2 In summary, the CF-LaF3 nanofilm prepared by the present invention has a good zinc negative electrode protection effect.
[0012] Instruction Manual
[0013] Figure 1 This is an optical microscope photo of the CF-LaF3 nanofilm prepared in Example 1 over a large area;
[0014] Figure 2 The transmission electron microscope of the CF-LaF3 nanofilm prepared in Example 1 and the corresponding element distribution map;
[0015] Figure 3 This is an atomic force microscope image of the CF-LaF3 nanofilm prepared in Example 1;
[0016] Figure 4 The powder X-ray diffraction and transmission electron microscopy images of the CF-LaF3 nanofilm prepared in Example 1;
[0017] Figure 5 The three-dimensional spectrum of the time-of-flight secondary ion mass spectrometry of the zinc negative electrode with a CF-LaF3 protective layer prepared in Example 2;
[0018] Figure 6 XPS graphs of different depths of the zinc negative electrode with a CF-LaF3 protective layer prepared in Example 2, a is the F1s spectrum, b is the La3d spectrum, and c is the Zn2p spectrum;
[0019] Figure 7 Static contact angle test of the zinc negative electrode with CF-LaF3 protective layer prepared in Example 2 and bare zinc;
[0020] Figure 8 The SEM images of the zinc negative electrode with CF-LaF3 protective layer and bare zinc prepared in Example 2 after being immersed in 2 mol / L zinc sulfate aqueous solution for 6 days;
[0021] Fig. 9 This is a DFT theoretical calculation simulation diagram of the CF-LaF3 nanofilm prepared in Example 1;
[0022] Fig.10 The CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery (zinc foil thickness of 200 μm) assembled in Example 2 was charged at a current density of 5 mA / cm 2 and area capacity of 1 mAh / cm 2 The long cycle diagram below;
[0023] Fig.11 For comparison, the Zn||Zn symmetric battery (zinc foil thickness 200 μm) assembled in experiment 1 was charged at a current density of 5 mA / cm 2 and area capacity of 1 mAh / cm 2 The cycle diagram below;
[0024] Fig.12 At a current density of 2 mA / cm 2 and area capacity of 10 mAh / cm 2 Below is the cycle performance diagram of the deep charge and discharge zinc utilization rate of 67% of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery (zinc foil thickness is 30 μm) assembled in Example 2;
[0025] Fig.13 At a current density of 2 mA / cm 2 and area capacity of 10 mAh / cm 2 Below is the cycle performance diagram of the Zn||Zn symmetric battery (zinc foil thickness is 30μm) assembled in comparative experiment 1 with a deep charge and discharge zinc utilization rate of 67%;
[0026] Fig.14 The CF-LaF3 / Zn||CF-LaF3 / Ti half-cell assembled in Example 3 was tested at a current density of 5 mA / cm 2 And the area capacity is 1mAh / cm 2 The long cycle diagram below;
[0027] Fig.15 For comparison, the Zn||Ti half-cell assembled in Experiment 2 was tested at a current density of 5 mA / cm 2 And the area capacity is 1mAh / cm 2 The cycle diagram below;
[0028] Fig.16 Linear sweep voltammetry test diagram (LSV) of the CF-LaF3 / Zn||CF-LaF3 / Ti half-cell assembled in Example 3 and the Zn||Ti half-cell assembled in Comparative Experiment 2, a is hydrogen evolution, b is oxygen evolution;
[0029] Fig.17 The activation energy test results of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Example 2 and the Zn||Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Comparative Experiment 1;
[0030] Fig.18 Scanning morphology of the negative electrode of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Example 2 and the Zn||Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Comparative Experiment 1 after cycling;
[0031] Fig.19 In-situ optical microscope deposition images of the negative electrode after cycling of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Example 2 and the Zn∥Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Comparative Experiment 1. DETAILED DESCRIPTION
[0032] Specific implementation method 1: This implementation method is a method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film, which is carried out according to the following steps:
[0033] 1. Add perfluorotetradecanoic acid to a mixed solution of chloroform and methanol, stir and dissolve to obtain a perfluorotetradecanoic acid solution; add lanthanum nitrate powder to secondary water, stir and dissolve to obtain a lanthanum nitrate aqueous solution; add sodium fluoride powder to secondary water, stir and dissolve to obtain a sodium fluoride aqueous solution;
[0034] 2. Under the condition of a droplet acceleration rate of 2 μL / s to 5 μL / s, a perfluorotetradecanoic acid solution is added dropwise to the surface of the lanthanum nitrate aqueous solution, and then under the condition of an injection rate of 1 mL / s to 2 mL / s, a sodium fluoride aqueous solution is injected into the bottom of the solution and allowed to stand at room temperature to obtain a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film at the air-water interface;
[0035] The molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to perfluorotetradecanoic acid in the perfluorotetradecanoic acid solution is 1:(0.0001-0.0002); the molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to sodium fluoride in the sodium fluoride aqueous solution is 1:(3-4).
[0036] The beneficial effects of this embodiment are:
[0037] This embodiment uses a surfactant as a soft template to induce LaF3 to connect into a dense and uniform nanofilm at the air-water interface, providing an organic-inorganic composite material and a hydrophobic zinc ion conductor membrane CF-LaF3 that can be prepared on a large area for zinc negative electrode protection of aqueous zinc ion batteries. It should be emphasized that the template agent perfluorotetradecanoic acid used in this embodiment induces lanthanum fluoride to form a continuous nanofilm, which has a crystalline structure and a continuous zinc transfer channel. Its composition structure is perfluorotetradecanoic acid on the surface and lanthanum fluoride at the bottom. The surface perfluorotetradecanoic acid active agent monolayer is exposed, which is hydrophobic and promotes Zn(H2O)6 2+ After desolvation, the lanthanum fluoride at the bottom has a uniform zinc ion transport channel, which accelerates zinc ion transport and induces uniform zinc ion deposition. The two components synergistically enhance the zinc ion transport kinetics.
[0038] In this embodiment, the CF-LaF3 nanofilm is transferred to the surface of the zinc foil. Due to the zinc-philic transmission channel inside the CF-LaF3 nanofilm, CF-LaF3 as a zinc negative electrode protective layer can significantly increase the Zn 2+ Transfer dynamics. In addition, the hydrophobic properties of the CF-LaF3 nanofilm surface accelerate the desolvation process of interfacial zinc ions, and further prevent the direct contact between the zinc negative electrode and active water, inhibiting the corrosion of the zinc surface by the electrolyte. Due to the dense uniformity of the CF-LaF3 nanofilm and the special zinc transmission path, the overall electrochemical performance of the CF-LaF3 / Zn electrode is significantly improved. The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of zinc foil with a thickness of 150μm to 250μm to obtain CF-LaF3 / Zn. CF-LaF3 / Zn is used as the positive and negative electrodes to assemble a CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery. At a current density of 5mA / cm 2 and area capacity of 1 mAh / cm 2 The symmetrical battery can be stably cycled for more than 4000h under the condition of 100% hygroscopic conditions. The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of a thin zinc foil with a thickness of 30μm to obtain CF-LaF3 / Zn. CF-LaF3 / Zn is used as the positive and negative electrodes to assemble the CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery. At a current density of 2mA / cm 2 And the area capacity is 10mAh / cm 2Under the condition that the zinc utilization rate is 67%, the symmetrical battery can stably cycle for more than 240 hours; the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of zinc foil with a thickness of 150μm to 250μm to obtain CF-LaF3 / Zn, and the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to the surface of titanium foil with a thickness of 5μm to 15μm to obtain CF-LaF3 / Ti. CF-LaF3 / Ti is used as the positive electrode and CF-LaF3 / Zn is used as the negative electrode to assemble the CF-LaF3 / Zn||CF-LaF3 / Ti half-cell. At a current density of 5mA / cm 2 And the area capacity is 1mAh / cm 2 The half-cell can be stably cycled for more than 6000 times, with a cumulative cycle area capacity of 6000mAh / cm 2 In summary, the CF-LaF3 nanofilm prepared by the present invention has a good zinc negative electrode protection effect.
[0039] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that: the concentration of the perfluorotetradecanoic acid solution in step 1 is 1.5 mmol / mL to 2.5 mmol / mL; the volume ratio of chloroform to methanol in the mixed solution of chloroform and methanol in step 1 is (2 to 4): 1. The rest is the same as specific embodiment 1.
[0040] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the concentration of the lanthanum nitrate aqueous solution in step 1 is 150 mmol / mL to 250 mmol / mL. The rest is the same as specific embodiment 1 or 2.
[0041] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the concentration of the sodium fluoride aqueous solution in step 1 is 150 mmol / mL to 250 mmol / mL. The rest is the same as specific embodiments 1 to 3.
[0042] Specific implementation mode 5: This implementation mode is different from specific implementation modes 1 to 4 in that: in step 2, the mixture is left to stand at room temperature for 20 to 28 hours. The rest is the same as specific implementation modes 1 to 4.
[0043] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane described in step 2 is composed of surface perfluorotetradecanoic acid and bottom lanthanum fluoride. The rest is the same as specific embodiments 1 to 5.
[0044] Specific embodiment 7: This embodiment is different from the specific embodiments 1 to 6 in that: the bottom lanthanum fluoride has a uniform zinc ion transmission channel, which improves the Zn 2+Transport dynamics; the surface perfluorotetradecanoic acid is hydrophobic, promoting Zn(H2O)6 2+ Desolvation. Other aspects are the same as those of the first to sixth embodiments.
[0045] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the thickness of the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film in step 2 is 60nm to 80nm. The rest is the same as specific embodiments 1 to 7.
[0046] Specific implementation method 9: The application of the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane in this implementation method is characterized in that it is used as an interface protection layer of the zinc negative electrode in an aqueous zinc ion battery.
[0047] Specific embodiment ten: This embodiment differs from specific embodiment nine in that: a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is transferred to a zinc foil surface with a thickness of 150 μm to 250 μm to obtain CF-LaF3 / Zn, and CF-LaF3 / Zn is used as the positive and negative electrodes to assemble a CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery. At a current density of 5 mA / cm 2 and area capacity of 1 mAh / cm 2 Under this condition, the symmetrical battery can stably cycle for more than 4000h;
[0048] The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film was transferred to the surface of a thin zinc foil with a thickness of 30 μm to obtain CF-LaF3 / Zn. CF-LaF3 / Zn was used as the positive and negative electrodes to assemble the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery. At a current density of 2 mA / cm 2 And the area capacity is 10mAh / cm 2 Under this condition, when the zinc utilization rate is 67%, the symmetrical battery can stably cycle for more than 240 hours;
[0049] The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film was transferred to the surface of zinc foil with a thickness of 150μm to 250μm to obtain CF-LaF3 / Zn. The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film was transferred to the surface of titanium foil with a thickness of 5μm to 15μm to obtain CF-LaF3 / Ti. CF-LaF3 / Ti was used as the positive electrode and CF-LaF3 / Zn as the negative electrode to assemble the CF-LaF3 / Zn||CF-LaF3 / Ti half-cell. At a current density of 5mA / cm 2 And the area capacity is 1mAh / cm 2 The half-cell can be stably cycled for more than 6000 times, with a cumulative cycle area capacity of 6000mAh / cm 2The rest is the same as the ninth embodiment.
[0050] The following examples are used to verify the beneficial effects of the present invention:
[0051] Embodiment 1:
[0052] A method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film is carried out according to the following steps:
[0053] 1. Add perfluorotetradecanoic acid to a mixed solution of chloroform and methanol, stir and dissolve to obtain a perfluorotetradecanoic acid solution; add lanthanum nitrate powder to secondary water, stir and dissolve to obtain a lanthanum nitrate aqueous solution; add sodium fluoride powder to secondary water, stir and dissolve to obtain a sodium fluoride aqueous solution;
[0054] 2. Add lanthanum nitrate aqueous solution into a culture dish with a diameter of 6 cm, add perfluorotetradecanoic acid solution onto the surface of lanthanum nitrate aqueous solution at a drop rate of 5 μL / s, then inject sodium fluoride aqueous solution into the bottom of the solution at an injection rate of 2 mL / s and let stand at room temperature for 20 hours to obtain a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film, i.e., CF-LaF3 nanofilm, at the air-water interface;
[0055] The molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to perfluorotetradecanoic acid in the perfluorotetradecanoic acid solution is 1:0.00012; the molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to sodium fluoride in the sodium fluoride aqueous solution is 1:3.
[0056] The concentration of the perfluorotetradecanoic acid solution described in step 1 is 1.8 mmol / mL; the volume ratio of chloroform to methanol in the mixed solution of chloroform and methanol described in step 1 is 3:1.
[0057] The concentration of the lanthanum nitrate aqueous solution described in step 1 is 200 mmol / mL.
[0058] The concentration of the sodium fluoride aqueous solution described in step 1 is 200 mmol / mL.
[0059] The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane described in step 2 is composed of perfluorotetradecanoic acid on the surface and lanthanum fluoride on the bottom;
[0060] The bottom lanthanum fluoride has a uniform zinc ion transmission channel, which improves the Zn 2+ Transport dynamics; the surface perfluorotetradecanoic acid is hydrophobic, promoting Zn(H2O)6 2+ Desolvation.
[0061] The CF-LaF3 nanofilm described in step 2 has a diameter of 6 cm, a thickness of 70 nm and a uniform thickness, and a roughness of about 1 nm.
[0062] In the second embodiment, the aqueous zinc ion battery is a Zn||Zn symmetric battery:
[0063] 1. The surface of the zinc sheet was polished smooth using 800-mesh and 2000-mesh sandpapers respectively, and then the CF-LaF3 nanofilm prepared in Example 1 was transferred to the polished surface of the zinc sheet, and cut into small discs with an area of 0.785 square centimeters to obtain a zinc negative electrode with a CF-LaF3 protective layer and a zinc positive electrode with a CF-LaF3 protective layer;
[0064] 2. Assemble a button cell in the order of a negative electrode, a negative electrode shell, a spring, a gasket, a diaphragm, an electrolyte, a positive electrode and a positive electrode shell, wherein the positive electrode is a zinc positive electrode with a CF-LaF3 protective layer, the diaphragm is a glass fiber membrane, the electrolyte is a 2 mol / L zinc sulfate aqueous solution, and the negative electrode is a zinc negative electrode with a CF-LaF3 protective layer, to obtain a CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical cell;
[0065] The thickness of the zinc sheets are 200 μm and 30 μm respectively;
[0066] When a symmetrical battery is assembled using a 200 μm thick zinc sheet, the current density is 5 mA / cm 2 and area capacity of 1 mAh / cm 2 The CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery assembled in Example 2 was subjected to a constant current charge and discharge long cycle test.
[0067] When a symmetrical battery was assembled using a zinc sheet with a thickness of 30 μm, the 2 And the area capacity is 10mAh / cm 2 Under the conditions, the CF-LaF3||CF-LaF3 symmetrical battery assembled in Example 2 was subjected to a deep charge and discharge cycle test, and the DOD value was as high as 67%.
[0068] Embodiment 3, the aqueous zinc ion battery is a Zn||Ti half-cell:
[0069] 1. The CF-LaF3 nanofilm prepared in Example 1 was transferred to a titanium foil with a thickness of 10 μm to obtain a titanium positive electrode protected by the CF-LaF3 nanofilm; the surface of a zinc sheet with a thickness of 200 μm was polished smooth using sandpaper, and then the CF-LaF3 nanofilm prepared in Example 1 was transferred to the polished zinc sheet to obtain a zinc negative electrode protected by the CF-LaF3 nanofilm;
[0070] 2. Assemble button cells in the order of negative electrode, negative electrode shell, spring, gasket, diaphragm, electrolyte, positive electrode and positive electrode shell, wherein the negative electrode is a zinc negative electrode protected by a CF-LaF3 nanofilm, the diaphragm is a glass fiber membrane, the electrolyte is a 2 mol / L zinc sulfate aqueous solution, and the positive electrode is a titanium positive electrode protected by a CF-LaF3 nanofilm, and assemble a CF-LaF3 / Zn||CF-LaF3 / Ti half-cell;
[0071] At a current density of 5 mA / cm 2 And the area capacity is 1mAh / cm 2 The CF-LaF3 / Zn||CF-LaF3 / Ti half-cell assembled in Example 3 was subjected to a constant current charge and discharge long cycle test.
[0072] Comparative Experiment 1: The difference between this embodiment and the second embodiment is that the positive and negative electrodes are both polished ordinary zinc sheets. The rest is the same as the second embodiment.
[0073] Comparative Experiment 2: The difference between this embodiment and the third embodiment is that the positive electrode is a common titanium foil, and the negative electrode is a polished common zinc sheet. The rest is the same as the third embodiment.
[0074] CF-LaF3 nanofilm transfer process prepared by embodiment 1: a culture dish (6 cm in diameter) prepared with CF-LaF3 nanofilm is slowly placed in a large glass surface dish container with a diameter of 20 cm, secondary water is slowly injected along the edge of the 6 cm culture dish, and along with the continuous addition of secondary water, the CF-LaF3 nanofilm interface is slowly lifted and raised to the same height as the 6 cm culture dish. Then secondary water is injected into the 20 cm surface dish container until the water surface does not cover the 6 cm culture dish, at which time the CF-LaF3 nanofilm will slowly float out of the 6 cm culture dish and float on the interface of the 20 cm surface dish water, successfully transferring the nanofilm out, then a solid substrate (such as zinc sheet, titanium foil) is slowly extended into the bottom of the CF-LaF3 nanofilm floating on the water surface, slowly lifted upward and separated from the water surface, the CF-LaF3 nanofilm will be transferred to the solid substrate, and the bottom lanthanum fluoride contacts the solid substrate.
[0075] Figure 1 This is an optical microscope photo of the CF-LaF3 nanofilm prepared in Example 1 over a large area. As can be seen from the figure, the nanofilm has a uniform morphology over a large area.
[0076] Figure 2 The transmission electron microscope image of the CF-LaF3 nanofilm prepared in Example 1 and the corresponding element distribution diagram; it can be seen from the figure that the elements La, F and C are evenly distributed in the nanofilm.
[0077] Depend on Figure 2 and Figure 3 It can be seen that the CF-LaF3 nanofilm prepared in Example 1 forms a uniform and continuous zinc ion transmission channel.
[0078] Figure 3 This is an atomic force microscope image of the CF-LaF3 nanofilm prepared in Example 1; as can be seen from the image, the thickness of the nanofilm is 70nm.
[0079] Figure 4 Powder X-ray diffraction and transmission electron microscopy images of the CF-LaF3 nanofilm prepared in Example 1; it can be seen from the figure that the prepared CF-LaF3 nanofilm has a good correspondence with the hexagonal phase LaF3 of the standard card, and the clear lattice fringes in the transmission electron microscope also prove that the prepared film is polycrystalline.
[0080] Figure 5 This is a three-dimensional spectrum of the time-of-flight secondary ion mass spectrometry of the zinc negative electrode with a CF-LaF3 protective layer prepared in Example 2; as can be seen from the figure, the CF-LaF3 nanofilm on the surface of the zinc substrate shows a visualized organic-inorganic hybrid component, which is composed of perfluorotetradecanoic acid on the surface and lanthanum fluoride at the bottom.
[0081] Figure 6 The XPS graphs of different depths of the zinc negative electrode with CF-LaF3 protective layer prepared in Example 2, a is the F1s spectrum, b is the La3d spectrum, and c is the Zn2p spectrum; from the figure, we can first observe the appearance of the organic component CF bond (689.5eV) and the inorganic La-F bond (685.29eV), and the disappearance of the surface organic component CF and the enhancement of the inorganic La-F with the increase of time. At the same time, with the increase of etching time, the peaks of the zinc substrate (1044eV, 1021eV) become more and more obvious, and the above characterization proves the organic-inorganic hybrid composition of the CF-LaF3 nanofilm on the zinc substrate.
[0082] Figure 7 Static contact angle test of the zinc negative electrode with CF-LaF3 protective layer prepared in Example 2 and bare zinc; as can be seen from the figure, the contact angles of the zinc sheet protected by CF-LaF3 nanofilm and bare zinc with 2 mol / L zinc sulfate aqueous solution are 116° and 74°, respectively, indicating that the nanofilm surface is hydrophobic.
[0083] Figure 8The SEM images of the zinc negative electrode with CF-LaF3 protective layer prepared in Example 2 and bare zinc after being immersed in 2 mol / L zinc sulfate aqueous solution for 6 days respectively; it can be seen from the figure that due to the direct corrosion of the electrolyte, Zn4SO4(OH)6·5H2O(ZHS) byproducts are formed on the surface of bare zinc. In contrast, CF-LaF3 / Zn effectively inhibits the formation of ZHS byproducts, verifying the barrier effect of CF-LaF3 nanofilm on electrolyte.
[0084] Fig. 9 This is a DFT theoretical calculation simulation diagram of the CF-LaF3 nanomembrane prepared in Example 1; it simulates the diffusion path of zinc ions in the LaF3 open framework within the nanomembrane, among which the migration path of zinc ions from Zn1 to Zn9 is simulated, proving the orderly migration of zinc ions through the LaF3 pores.
[0085] Fig.10 The CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery (zinc foil thickness of 200 μm) assembled in Example 2 was charged at a current density of 5 mA / cm 2 and area capacity of 1 mAh / cm 2 The long cycle diagram below; it can be seen from the figure that the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery has a cycle life of up to 4000h, proving that the CF-LaF3 protective layer can effectively improve the performance of the symmetric battery.
[0086] Fig.11 For comparison, the Zn||Zn symmetric battery (zinc foil thickness 200 μm) assembled in experiment 1 was charged at a current density of 5 mA / cm 2 and area capacity of 1 mAh / cm 2 The cycle diagram below; it can be seen from the figure that the Zn||Zn symmetric battery has a cycle life of only 550h.
[0087] Fig.12 At a current density of 2 mA / cm 2 and area capacity of 10 mAh / cm 2 Below is the cycle performance diagram of the deep charge and discharge zinc utilization rate of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery (zinc foil thickness is 30μm) assembled in Example 2; it can be seen from the figure that the CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery can still operate stably for 240h under relatively harsh conditions, proving the ability of CF-LaF3 nanofilm to effectively inhibit dendrites on the metallic zinc negative electrode.
[0088] Fig.13 At a current density of 2 mA / cm 2 and area capacity of 10 mAh / cm 2Below is the cycle performance diagram of the Zn||Zn symmetrical battery (zinc foil thickness is 30μm) assembled in comparative experiment 1 with a deep charge and discharge zinc utilization rate of 67%; it can be seen from the figure that the Zn||Zn symmetrical battery assembled with bare zinc is difficult to operate normally under harsh conditions.
[0089] Fig.14 The CF-LaF3 / Zn||CF-LaF3 / Ti half-cell assembled in Example 3 was tested at a current density of 5 mA / cm 2 And the area capacity is 1mAh / cm 2 The long cycle diagram under the above conditions; As can be seen from the figure, the CF-LaF3 / Zn||CF-LaF3 / Ti half-cell can run stably for more than 6000 cycles, with a cumulative capacity of more than 6000 mAh / cm 2 , proving that CF-LaF3 nanofilm can quickly conduct uniform zinc ion flux to be deposited on titanium foil, and effectively inhibit the dendrite growth on the zinc negative electrode side. At the same time, the hydrophobic protective layer can effectively inhibit the corrosion of the electrolyte to the electrode, thereby significantly improving the cycle life of the zinc ion battery.
[0090] Fig.15 For comparison, the Zn||Ti half-cell assembled in Experiment 2 was tested at a current density of 5 mA / cm 2 And the area capacity is 1mAh / cm 2 The cycle diagram below; it can be seen from the figure that due to the slow accumulation of zinc dendrites and the generation of insulating by-products, the Zn||Ti half-cell assembled with unprotected titanium foil and zinc foil can only cycle normally for 187 times.
[0091] Fig.16 The linear sweep voltammetry test diagram (LSV) of the CF-LaF3 / Zn||CF-LaF3 / Ti half-cell assembled in Example 3 and the Zn||Ti half-cell assembled in Comparative Experiment 2, a is hydrogen evolution, b is oxygen evolution; it can be seen from the figure that compared with the unprotected bare zinc battery system, the CF-LaF3 nanofilm protected zinc battery body has a wider electrochemical window, which widens the hydrogen evolution potential from -85mV to -100mV, and the oxygen evolution potential from 2.55V to 2.7V.
[0092] Fig.17 The activation energy test results of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Example 2 and the Zn||Zn symmetric battery (zinc foil thickness is 200 μm) assembled in Comparative Experiment 1; as shown in the figure, the activation energy obtained by fitting the impedance at different temperatures based on the Arrhenius equation is smaller than the activation energy of bare zinc (57 J / mol) in the desolvation of the CF-LaF3 / Zn interface (45 kJ / mol), indicating that the CF-LaF3 nanofilm accelerates the Zn(H2O)62+ The process of desolvation.
[0093] The CF-LaF3 / Zn||CF-LaF3 / Zn symmetrical battery (zinc foil thickness of 200 μm) assembled in Example 2 and the Zn||Zn symmetrical battery (zinc foil thickness of 200 μm) assembled in Comparative Experiment 1 were tested at a current density of 10 mA / cm 2 And the area capacity is 1mAh / cm 2 30 and 60 cycles respectively under the conditions of Fig.18 The negative electrode scanning morphology of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery (zinc foil thickness of 200μm) assembled in Example 2 and the Zn||Zn symmetric battery (zinc foil thickness of 200μm) assembled in Comparative Experiment 1 after cycling; the scanning image shows that compared with bare zinc, the electrode surface protected by the CF-LaF3 nanofilm is smooth and flat, and no by-products are generated. This shows that the nanofilm with uniformly distributed zinc ion transmission channels is conducive to Zn 2+ Uniform deposition of ions and effective suppression of the generation of by-products.
[0094] The CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery (zinc foil thickness of 200 μm) assembled in Example 2 and the Zn||Zn symmetric battery (zinc foil thickness of 200 μm) assembled in Comparative Experiment 1 were tested at a current density of 20 mA / cm 2 And the area capacity is 1mAh / cm 2 The conditions were cycled for 30min and 50min respectively; Fig.19 The negative electrode in-situ optical microscope deposition image of the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery (zinc foil thickness of 200μm) assembled in Example 2 and the Zn∥Zn symmetric battery (zinc foil thickness of 200μm) assembled in Comparative Experiment 1 after cycling; As can be seen from the figure, tiny protrusions appeared on the surface of the bare zinc electrode at 30 minutes, and the protrusions became significantly larger after 50 minutes, accompanied by the continuous precipitation of gas. In contrast, the CF-LaF3 / Zn electrode still maintained a uniform and dense zinc deposition morphology for up to 50 minutes, indicating that the CF-LaF3 nanofilm can induce uniform zinc deposition and effectively inhibit hydrogen evolution.
Claims
1. A method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film, characterized in that It is carried out in the following steps:
1. Add perfluorotetradecanoic acid to a mixed solution of chloroform and methanol, stir and dissolve to obtain a perfluorotetradecanoic acid solution; add lanthanum nitrate powder to secondary water, stir and dissolve to obtain a lanthanum nitrate aqueous solution; add sodium fluoride powder to secondary water, stir and dissolve to obtain a sodium fluoride aqueous solution; 2. Under the condition of a droplet acceleration rate of 2 μL / s to 5 μL / s, a perfluorotetradecanoic acid solution is added dropwise to the surface of the lanthanum nitrate aqueous solution, and then under the condition of an injection rate of 1 mL / s to 2 mL / s, a sodium fluoride aqueous solution is injected into the bottom of the solution and allowed to stand at room temperature to obtain a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film at the air-water interface; The molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to perfluorotetradecanoic acid in the perfluorotetradecanoic acid solution is 1:(0.0001-0.0002); the molar ratio of lanthanum nitrate in the lanthanum nitrate aqueous solution to sodium fluoride in the sodium fluoride aqueous solution is 1:(3-4).
2. The method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film according to claim 1, characterized in that The concentration of the perfluorotetradecanoic acid solution described in step 1 is 1.5 mmol / mL to 2.5 mmol / mL; the volume ratio of chloroform to methanol in the mixed solution of chloroform and methanol described in step 1 is (2 to 4):
1.
3. The method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film according to claim 1, characterized in that The concentration of the lanthanum nitrate aqueous solution described in step 1 is 150 mmol / mL to 250 mmol / mL.
4. The method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film according to claim 1, characterized in that The concentration of the sodium fluoride aqueous solution described in step 1 is 150 mmol / mL to 250 mmol / mL.
5. The method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film according to claim 1, characterized in that In step 2, let stand at room temperature for 20 to 28 hours.
6. The method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film according to claim 1, characterized in that The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane described in step 2 is composed of perfluorotetradecanoic acid on the surface and lanthanum fluoride on the bottom.
7. The method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film according to claim 6, characterized in that The bottom lanthanum fluoride has a uniform zinc ion transmission channel, which improves Zn 2+ Transport dynamics; the surface perfluorotetradecanoic acid is hydrophobic, promoting Zn(H2O)6 2+ Desolvation.
8. The method for preparing a hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film according to claim 1, characterized in that The thickness of the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film described in step 2 is 60nm to 80nm.
9. Use of the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane prepared as claimed in claim 1, characterized in that It is used as an interfacial protective layer for zinc anodes in aqueous zinc-ion batteries.
10. Use of the hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 membrane according to claim 9, characterized in that The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film was transferred to the surface of zinc foil with a thickness of 150μm to 250μm to obtain CF-LaF3 / Zn. CF-LaF3 / Zn was used as the positive and negative electrodes to assemble the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery. The current density was 5mA / cm 2 and area capacity of 1 mAh / cm 2 Under this condition, the symmetrical battery can stably cycle for more than 4000h; The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film was transferred to the surface of a thin zinc foil with a thickness of 30 μm to obtain CF-LaF3 / Zn. CF-LaF3 / Zn was used as the positive and negative electrodes to assemble the CF-LaF3 / Zn||CF-LaF3 / Zn symmetric battery. At a current density of 2 mA / cm 2 And the area capacity is 10mAh / cm 2 Under this condition, when the zinc utilization rate is 67%, the symmetrical battery can stably cycle for more than 240 hours; The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film was transferred to the surface of zinc foil with a thickness of 150μm to 250μm to obtain CF-LaF3 / Zn. The hydrophobic zinc ion conductor perfluorotetradecanoic acid-LaF3 film was transferred to the surface of titanium foil with a thickness of 5μm to 15μm to obtain CF-LaF3 / Ti. CF-LaF3 / Ti was used as the positive electrode and CF-LaF3 / Zn as the negative electrode to assemble the CF-LaF3 / Zn||CF-LaF3 / Ti half-cell. At a current density of 5mA / cm 2 And the area capacity is 1mAh / cm 2 The half-cell can be stably cycled for more than 6000 times, with a cumulative cycle area capacity of 6000mAh / cm 2 above.
Citation Information
Patent Citations
Nanostructural designs for electrode materials of fluoride ion batteries
CN112166512A
Preparation method and application of zinc phosphate film
CN115332472A
Preparation method and application of zinc-loving hydrophobic interface nano film
CN116936726A
Nanostructural designs for electrode materials of fluoride ion batteries
US20190372111A1
Cited By
Preparation method of reducing phosphate solid electrolyte interface layer and application of reducing phosphate solid electrolyte interface layer in aqueous zinc ion battery anode
CN120089744A
Preparation method of reducing phosphate solid electrolyte interface layer and application thereof in anode of aqueous zinc ion battery