Electrolyte additive, electrolyte and alkali metal ion battery

CN119050479APending Publication Date: 2024-11-29SHENZHEN INST OF ADVANCED TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411165654.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

尽管如此,无负极碱金属电池仍然面临着一系列挑战:(1)负极侧电化学沉积不均匀

Benefits of technology

[0032] The present invention uses a negative electrode current collector to replace the negative electrode in the traditional battery. The negative electrode current collector does not contain active substances. Therefore, the alkali metal battery in the present invention is a negative electrode-free alkali metal battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007806260000031
    Figure BDA0005007806260000031
  • Figure BDA0005007806260000051
    Figure BDA0005007806260000051
  • Figure BDA0005007806260000061
    Figure BDA0005007806260000061
Patent Text Reader

Abstract

The invention discloses an electrolyte additive, an electrolyte and an alkali metal ion battery, the electrolyte additive comprises Ca (BHx (OR) y) 2, x is an integer in the range of 0-3, y is an integer in the range of 1-4, x + y = 4, and R is selected from at least one of C1-10 alkyl groups and fluorine-substituted C1-10 alkyl groups. According to the electrolyte additive, a strong positive ion (Ca < 2 + >) electrostatic shielding layer is provided in the deposition process of alkali metal ions (sodium ions, potassium ions or lithium ions) to inhibit growth of dendrites, and regulation and control of an electrolyte solvation structure are achieved through a large-size boron-based anion group ((BHx (OR) y) <->); and furthermore, the fast and uniform deposition and stripping of alkali metal ions are realized through the synergy of the electrolyte additive and the electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of batteries, and in particular relates to an electrolyte additive, an electrolyte and an alkali metal ion battery. Background Art

[0002] Commercial lithium-ion batteries and sodium-ion batteries all use carbon-based negative electrode materials. For example, the most commonly used negative electrode for lithium-ion batteries is graphite, with a theoretical specific capacity of 372mAh / g and a lithium insertion potential of 0.01-0.2V; the most commonly used negative electrode for sodium-ion batteries is hard carbon, with a specific capacity of 350-400mAh / g and a sodium insertion potential of 0.1-0.3V. On the one hand, the theoretical specific capacity of carbon-based negative electrode materials determines that a certain mass proportion of negative electrode materials is required in the battery. The presence of negative electrode materials increases the overall weight of the battery and affects the energy density of the battery. On the other hand, the lithium / sodium insertion potential of carbon-based negative electrodes is low, and dendrites are easily formed at the negative electrode, causing battery short circuits, loss of active lithium and other problems, affecting the life of the battery. In response to this, negative electrode-free secondary battery technology that directly abandons negative electrode active materials is an effective solution. The negative electrode side of the negative electrode-free alkali metal battery only uses a current collector without active materials, and forms a real negative electrode in situ during the first charging process. This battery configuration not only improves the energy density of the battery, but also further reduces the complexity and cost of battery production, and the subsequent storage, transportation and operation are more convenient and safe. Despite this, negative electrode-free alkali metal batteries still face a series of challenges: (1) uneven electrochemical deposition on the negative electrode side. (2) unstable chemical interface on the negative electrode side. (3) irreversible loss of a large amount of alkaline source. This makes negative electrode-free alkali metal batteries usually exhibit low coulombic efficiency and short cycle life. Their performance has decayed significantly after less than 50 cycles, which seriously hinders their large-scale application. Summary of the invention

[0003] In order to overcome at least one technical problem existing in the above-mentioned prior art, one of the objectives of the present invention is to provide an electrolyte additive.

[0004] A second object of the present invention is to provide a method for preparing an electrolyte additive.

[0005] A third object of the present invention is to provide an electrolyte.

[0006] A fourth object of the present invention is to provide an alkali metal ion battery.

[0007] A fifth object of the present invention is to provide application of the above-mentioned electrolyte additive and / or electrolyte in the field of batteries.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] The first aspect of the present invention provides an electrolyte additive, comprising Ca(BHx (OR) y )2, wherein x is an integer from 0 to 3, y is an integer from 1 to 4, x+y=4, and R is selected from C 1~10 Alkyl, fluorine-substituted C 1~10 At least one of the alkyl groups.

[0010] When the electrolyte additive of the present invention is applied to an alkali metal ion battery, the cation Ca 2+ A cationic electrostatic shielding layer is formed on the surface of the negative electrode current collector to inhibit the growth of dendrites and reduce the risk of dendrites penetrating the diaphragm and causing battery short circuit. x (OR) y ) - Adjust the solvation structure of alkali metal ions (sodium ions, potassium ions or lithium ions), anion groups (BH x (OR) y ) - Entering into the solvation structure of alkali metal ions, the cation Ca 2+ The electric field strength of the anion group (BH x (OR) y ) - It enters the inner solvation structure of alkali metal ions, effectively regulates the solvation structure of alkali metal ions, and promotes the solvation and desolvation process of alkali metal ions. At the same time, because the inner solvation structure of alkali metal ions introduces anion groups (BH x (OR) y ) - , realizing the anionic group (BH x (OR) y ) - The decomposition of the SEI layer forms an SEI layer. The inorganic content in the SEI layer is significantly increased, which reduces the side reactions between the electrolyte and the negative electrode collector during the desolvation of the alkali metal ions, enables the alkali metal ions to be highly reversibly deposited and stripped, and improves the average coulombic efficiency, rate performance, cycle life, and energy density of the alkali metal ion battery.

[0011] In the present invention, x is an integer between 0 and 3, for example, x can be selected from 0, 1, 2, and 3; preferably, x is 0 or 1.

[0012] In the present invention, y is an integer of 1 to 4, for example, y can be selected from 1, 2, 3, and 4; preferably, y is 3 or 4.

[0013] Preferably, the C 1~10The alkyl groups include C 1~10 Straight chain alkyl or C 1~10 of branched chain alkyl.

[0014] Preferably, the fluorine-substituted C 1~10 The alkyl groups include fluorine-substituted C 1~10 Branched alkyl or fluorine-substituted C 1~10 of a straight chain alkyl group.

[0015] In the present invention, Ca(BH x (OR) y )2, compared with the unsubstituted alkyl group, the fluorine-substituted alkyl group adjusts the solvation structure of the alkali metal ion, resulting in an increase in the Na signal of the electrolyte in the Na spectrum shifting toward the strong field as the concentration of the electrolyte additive increases, and the CF signal in the F spectrum also gradually shifts toward the strong field as the concentration of the electrolyte additive increases, indicating that the anion group enters the solvation structure of the alkali metal ion. At the same time, because the anion group is introduced into the inner layer solvation structure of the alkali metal ion, the fluorine-substituted alkyl anion group is preferentially decomposed during the desolvation process to form a SEI layer with a high F content. After the introduction of the fluorine-substituted alkyl anion group, the inorganic content in the SEI layer is significantly increased, further reducing the side reactions between the electrolyte and the negative electrode current collector during the desolvation process of the alkali metal ions, allowing the alkali metal ions to be highly reversibly deposited and stripped, further improving the average coulombic efficiency, rate performance, cycle life, and energy density of the alkali metal ion battery.

[0016] Preferably, the R is selected from C 1~5 Alkyl, fluorine-substituted C 1~5 At least one of the alkyl groups.

[0017] Preferably, the Ca(BH x (OR) y )2 in (BH x (OR) y ) - Selected from:

[0018] The second aspect of the present invention provides a method for preparing the electrolyte additive according to the first aspect of the present invention, comprising the following steps:

[0019] Ca(BH4)2 and ROH are mixed and reacted to obtain,

[0020] R is as defined in the first aspect of the present invention.

[0021] Preferably, the mixing reaction temperature is 35-55°C.

[0022] The third aspect of the present invention provides an electrolyte comprising the electrolyte additive described in the first aspect of the present invention, an electrolyte salt and a solvent.

[0023] Preferably, the electrolyte salt includes a sodium salt, a lithium salt or a potassium salt.

[0024] Preferably, the lithium salt is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethylsulfonylimide) (LiTFSI), and lithium bis(fluorosulfonylimide) (LiFSI).

[0025] Preferably, the sodium salt is selected from at least one of sodium hexafluorophosphate (NaPF6), sodium perchlorate (NaClO4), sodium dioxalatoborate (NaBOB), sodium difluorooxalatoborate (NaDFOB), sodium tetrafluoroborate (NaBF4), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), and sodium bis(fluorosulfonyl)imide (NaFSI).

[0026] Preferably, the potassium salt is selected from at least one of potassium hexafluorophosphate (KPF6), potassium perchlorate (KClO4), potassium dioxalatoborate (KBOB), potassium difluorooxalatoborate (KDFOB), potassium tetrafluoroborate (KBF4), potassium bistrifluoromethylsulfonyl imide (KTFSI), and potassium bisfluorosulfonyl imide (KFSI).

[0027] Preferably, the concentration of the electrolyte additive is 0.01-1mol / L, for example, it can be selected from: 0.01mol / L, 0.02mol / L, 0.03mol / L, 0.04mol / L, 0.05mol / L, 0.06mol / L, 0.07mol / L, 0.08mol / L, 0.09mol / L, 0.1mol / L, 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L, 1mol / L; further preferably, the concentration of the electrolyte additive is 0.01-0.1mol / L.

[0028] Preferably, the concentration of the electrolyte salt is 0.5-5 mol / L, for example, it can be selected from: 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L , 2mol / L, 2.2mol / L, 2.4mol / L, 2.6mol / L, 2.8mol / L, 3mol / L, 3.2mol / L, 3.4mol / L, 3.6mol / L, 3.8mol / L, 4mol / L, 4.2mol / L, 4.4mol / L, 4.6mol / L, 4.8mol / L, 5mol / L; further preferably, the concentration of the electrolyte salt is 0.8-2mol / L.

[0029] Preferably, the solvent is selected from at least one of esters, sulfones, ethers, nitriles and ionic liquids.

[0030] Preferably, the solvent is selected from at least one of diethylene glycol dimethyl ether, propylene carbonate, ethylene carbonate, diethyl carbonate, and fluoroethylene carbonate.

[0031] The fourth aspect of the present invention provides an alkali metal ion battery, comprising a positive electrode, a separator and a negative electrode current collector; the separator is located between the positive electrode and the negative electrode current collector, and the separator contains the electrolyte described in the third aspect of the present invention.

[0032] The present invention adopts a negative electrode current collector to replace the negative electrode in a traditional battery. The negative electrode current collector does not contain active materials. Therefore, the alkali metal battery in the present invention is an alkali metal battery without a negative electrode.

[0033] Preferably, the positive electrode contains a positive electrode active material.

[0034] Preferably, the alkali metal ion battery further comprises a positive electrode current collector; the positive electrode active material is located between the positive electrode current collector and the separator.

[0035] Preferably, the alkali metal ion battery is an alkali metal ion battery without a negative electrode. In the alkali metal ion battery without a negative electrode in the present invention, during the charging process, the alkali metal ions (sodium ions, lithium ions or potassium ions) in the positive electrode migrate to the electrolyte, and the alkali metal ions in the electrolyte are deposited on the negative electrode current collector; during the discharge process, the alkali metal ions return to the positive electrode from the electrolyte, and at the same time, the alkali metal ions are stripped from the negative electrode and returned to the electrolyte, thereby realizing the entire charging and discharging process.

[0036] Preferably, the alkali metal ion battery comprises a sodium ion battery, a potassium ion battery or a lithium ion battery.

[0037] Preferably, the alkali metal battery comprises a negative electrode-free sodium ion battery, a negative electrode-free potassium ion battery or a negative electrode-free lithium ion battery.

[0038] The fifth aspect of the present invention provides the use of the electrolyte additive described in the first aspect of the present invention and / or the electrolyte described in the third aspect of the present invention in the field of batteries.

[0039] The beneficial effects of the present invention are as follows: the electrolyte additive in the present invention provides a strong cation (Ca) during the deposition process of alkali metal ions (sodium ions, potassium ions or lithium ions). 2+ ) electrostatic shielding layer inhibits the growth of dendrites and through the large-sized boron anion groups ((BH x (OR) y ) - ) to achieve the regulation of the electrolyte solvation structure, and then achieve the rapid and uniform deposition and stripping of alkali metal ions through the synergy of electrolyte additives and electrolyte.

[0040] The alkali metal ion battery of the present invention has excellent dendrite inhibition effect in a long cycle process, good cycle stability, high coulomb efficiency, long cycle life and high energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is the Ca(BH(pftb)3)2 sample in Example 1 11 NMR spectrum of B.

[0042] Figure 2 The different concentrations of Ca(BH(pftb)3)2 sodium ion electrolyte in Example 1 are 23 NMR spectrum of Na.

[0043] Figure 3 The different concentrations of Ca(BH(pftb)3)2 sodium ion electrolyte in Example 1 are 19 NMR spectrum of F.

[0044] Figure 4 This is the cyclic coulombic efficiency diagram of the sodium ion battery in Example 2.

[0045] Figure 5 This is the cyclic coulombic efficiency diagram of the sodium ion battery in Comparative Example 1.

[0046] Figure 6 It is a charge and discharge curve diagram of different cycles of the sodium ion battery in Example 2.

[0047] Figure 7It is a charge and discharge curve diagram of different cycles of the sodium ion battery in Comparative Example 1.

[0048] Figure 8 This is a physical picture of the negative electrode of the sodium ion battery in the charged state in Example 2.

[0049] Fig. 9 This is the XPS graph of the charged negative electrode sheet of the negative electrode-free sodium ion battery in Example 2 and Comparative Example 1 after cycling.

[0050] Fig.10 This is a SEM image of the charged negative electrode sheet of the negative electrode-free sodium ion battery in Example 2 and Comparative Example 1 after cycling. DETAILED DESCRIPTION

[0051] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.

[0052] The electrolyte additive used in the embodiment of the present invention is Ca(BH x (OR) y )2, where (BH x (OR) y ) - It is: tris(2-(trifluoromethyl)hexafluoropropoxy)borate (chemical formula: (BH(pftb)3) - ), tris(2,2,2-trifluoroethoxy)borate (chemical formula: (BH(tfe)3) - ), triethoxyborate (chemical formula: (BH(Et)3) - ), tris(bis(2-hexafluoropropoxy)(2,2,2-trifluoroethoxy)(2-trifluoropropoxy))borate (chemical formula: (BH(hfip)3) - ), tris(3,3,3-trifluoropropoxy)borate (chemical formula: (BH(tf1p)3) - ), tris(2-trifluoropropoxy)borate (chemical formula: (BH(tf2p)3) - ), tetrakis(2,2,2-trifluoroethoxy)borate (chemical formula: (B(tfe)4) - ), tetraethoxyborate (chemical formula: (B(Et)4) - ), bis(2-hexafluoropropoxy)(2,2,2-trifluoroethoxy)(2-trifluoropropoxy)borate (chemical formula: (B(hfip)4) -), tetrakis(3,3,3-trifluoropropoxy)borate (chemical formula: (B(tf1p)4) - ), or, tetrakis(2-trifluoropropoxy)borate (chemical formula: (B(tf2p)4) - ); the specific structural formula is as follows:

[0053]

[0054]

[0055] The preparation method of the electrolyte additive in the above structural formula 1 to structural formula 6 is as follows:

[0056] Ca(BH4)2+6R-OH——Ca(BH(OR)3)2+6H2↑

[0057] In a glove box, Ca(BH4)2 and ROH were weighed at a molar ratio of 1:6. First, Ca(BH4)2 was added to ethylene glycol dimethyl ether (DME) to prepare a solution with a concentration of 0.2 mol / L. Then ROH was added to the Ca(BH4)2 / DME solution, stirred at 40°C and 800 r / min for 12 hours, and vacuumed to obtain calcium salt additive powders in structural formulas 1 to 6. ROH is hexafluoroisopropanol, perfluorotert-butyl alcohol, ethanol, 2,2,2-trifluoroethanol, 3,3,3-trifluoro-1-propanol, and 1,1,1-trifluoro-2-propanol.

[0058] The preparation methods of the electrolyte additives in the above structural formulas VII to XI are as follows:

[0059] Ca(BH4)2+8R-OH——Ca(B(OR)4)2+8H2↑

[0060] In a glove box, Ca(BH4)2 and ROH were weighed at a molar ratio of 1:8. First, Ca(BH4)2 was added to DME to prepare a solution with a concentration of 0.2 mol / L. Then ROH was added to the Ca(BH4)2 / DME solution, stirred at 40°C and 800 r / min for 24 hours, and vacuumed to obtain calcium salt additive powders in structural formulas 7 to 11. ROH was hexafluoroisopropanol, perfluorotert-butyl alcohol, ethanol, 2,2,2-trifluoroethanol, 3,3,3-trifluoro-1-propanol, and 1,1,1-trifluoro-2-propanol, respectively.

[0061] The implementation of the present invention is further described in detail below with reference to specific embodiments and comparative examples:

[0062] Example 1

[0063] This example provides a negative electrode-free sodium ion battery electrolyte, comprising a Ca(BH(pftb)3)2 electrolyte additive.

[0064] The negative electrode-free sodium ion battery electrolyte in this example is prepared by a preparation method comprising the following steps:

[0065] Add 73.68g Ca(BH(pftb)3)2 and 167.954g NaPF6 to 1L diethylene glycol dimethyl ether (G2), stir and dissolve to obtain the negative electrode-free sodium ion battery electrolyte in this example, wherein the concentration of Ca(BH(pftb)3)2 is 0.05mol / L and the concentration of NaPF6 is 1mol / L.

[0066] The Ca(BH(pftb)3)2 sample used in this test was 11 The NMR diagram of B is as follows Figure 1 shown. Figure 1 The sample has the characteristic peak of B in the anionic group and no other impurity peaks, indicating that the purity of the prepared Ca(BH(pftb)3)2 sample is very high.

[0067] According to the method in this example, different concentrations of Ca(BH(pftb)3)2 sodium ion battery electrolytes were prepared. Specifically, the concentrations of Ca(BH(pftb)3)2 were 0 mol / L, 0.01 mol / L, 0.05 mol / L, and 0.1 mol / L. Then, the NMR graphs of the prepared electrolytes were tested. Figure 2 and Figure 3 As shown. Figure 2 and Figure 3 It can be seen that the Na signal of the electrolyte in the Na spectrum shifts toward the strong field more and more with the increase of the electrolyte additive concentration, and the CF signal in the F spectrum also shifts toward the strong field more and more with the increase of the electrolyte additive concentration, which explains (BH(pftb)3) - Entering into the solvation structure of the sodium ion further indicates that the anionic group ((BH x (OR) y ) - ) has a significant effect on the solvation structure of alkali metal ions.

[0068] Example 2

[0069] This example provides a negative electrode-free sodium ion battery, using the negative electrode-free sodium ion battery electrolyte in Example 1 as the electrolyte.

[0070] The negative electrode-free sodium ion battery in this example is prepared by a preparation method comprising the following steps:

[0071] (1) Preparation of negative electrode current collector for battery: Prepare aluminum foil of required size as negative electrode current collector.

[0072] (2) Preparation of battery positive electrode: 9gNa 2.5 Fe 1.75 (SO4)3, 0.5g conductive carbon black, and 0.5g polyvinylidene fluoride were added to 14mL nitrogen methyl pyrrolidone solution and fully ground to obtain a uniform slurry; then the slurry was evenly coated on the surface of aluminum foil and vacuum dried. The dried electrode sheet was cut into a 10mm diameter disc, compacted and used as a positive electrode for later use.

[0073] (3) Preparation of diaphragm: Cut the glass fiber film into discs with a diameter of 16 mm and use them as diaphragms.

[0074] (4) Battery assembly: In an inert gas-protected glove box, the prepared negative electrode current collector, separator, and positive electrode plate are tightly stacked in sequence, and the negative electrode-free sodium ion battery electrolyte prepared in Example 1 is added dropwise to completely soak the separator. Then, the stacked part is encapsulated in a button battery casing to complete the assembly of the negative electrode-free sodium ion battery.

[0075] Embodiment 3-6

[0076] The only difference between the negative electrode-free sodium ion battery in Example 3-6 and Example 2 is that the concentration of the Ca(BH(pftb)3)2 electrolyte additive in the electrolyte used is different. Specifically, the concentrations of the Ca(BH(pftb)3)2 electrolyte additive in Examples 3-6 are 0.01 mol / L, 0.1 mol / L, 0.3 mol / L and 1 mol / L, respectively.

[0077] Examples 7-10

[0078] The only difference between the negative electrode-free sodium ion battery in Examples 7-10 and Example 2 is that the concentration of NaPF6 in the electrolyte used is different. Specifically, the concentration of NaPF6 in Examples 7-10 is 0.5 mol / L, 0.8 mol / L, 2 mol / L and 5 mol / L, respectively.

[0079] Examples 11-14

[0080] The difference between the negative electrode-free sodium ion batteries in Examples 11-14 and Example 2 is only that the diethylene glycol dimethyl ether in Example 2 is replaced by propylene carbonate + ethylene carbonate (500 mL + 500 mL, Example 11), propylene carbonate + diethyl carbonate (500 mL + 500 mL, Example 12), propylene carbonate + ethylene carbonate + diethyl carbonate (400 mL + 300 mL + 300 mL, Example 13), propylene carbonate + fluoroethylene carbonate (950 mL + 50 mL, Example 14).

[0081] Examples 15-24

[0082] The only difference between the negative electrode-free sodium ion batteries in Examples 15-24 and Example 2 is that the electrolyte used replaces the Ca(BH(pftb)3)2 electrolyte additive in Example 2 with: Ca(B(tfe)4)2 (Example 15), Ca(BH(tfe)3)2 (Example 16), Ca(B(Et)4)2 (Example 17), Ca(BH(Et)3)2 (Example 18), Ca(B(hfip)4)2 (Example 19), Ca(BH(hfip)3)2 (Example 20), Ca(B(tf1p)4)2 (Example 21), Ca(BH(tf1p)3)2 (Example 22), Ca(B(tf2p)4)2 (Example 23), Ca(BH(tf2p)3)2 (Example 24).

[0083] Examples 25-30

[0084] The only difference between the negative electrode-free sodium ion batteries in Examples 25-30 and Example 2 is that the electrolyte used is NaPF6 in Example 2 replaced by NaClO4 (Example 25), NaBOB (Example 26), NaDFOB (Example 27), NaBF4 (Example 28), NaTFSI (Example 29), and NaFSI (Example 30).

[0085] Embodiment 31

[0086] The negative electrode-free lithium-ion battery electrolyte in this example contains Ca(BH(pftb)3)2 electrolyte additive.

[0087] The negative electrode-free lithium-ion battery electrolyte in this example is prepared by a preparation method comprising the following steps:

[0088] Add 73.68g Ca(BH(pftb)3)2 and 151.905g LiPF6 to 1L diethylene glycol dimethyl ether (G2), stir and dissolve to obtain the negative electrode-free lithium-ion battery electrolyte in this example; wherein the concentration of Ca(BH(pftb)3)2 is 0.05mol / L and the concentration of LiPF6 is 1mol / L.

[0089] Embodiment 32

[0090] The only difference between the negative electrode-free lithium ion battery in this example and Example 2 is that the positive electrode active material used in this example is lithium iron phosphate, and the electrolyte used is the negative electrode-free lithium ion battery electrolyte prepared in Example 31.

[0091] Examples 33-36

[0092] The only difference between the negative electrode-free lithium-ion batteries in Examples 33-36 and Example 32 is that the concentrations of the Ca(BH(pftb)3)2 electrolyte additive in the electrolyte used are different. Specifically, the concentrations of the Ca(BH(pftb)3)2 electrolyte additive in Examples 33-36 are 0.01 mol / L, 0.1 mol / L, 0.3 mol / L and 1 mol / L, respectively.

[0093] Examples 37-40

[0094] The only difference between the negative electrode-free lithium-ion batteries in Examples 37-40 and Example 32 is that the concentration of LiPF6 in the electrolyte used is different. Specifically, the concentration of LiPF6 in Examples 37-40 is 0.5 mol / L, 0.8 mol / L, 2 mol / L and 5 mol / L, respectively.

[0095] Examples 41-44

[0096] The only difference between the negative electrode-free lithium-ion batteries in Examples 41-44 and Example 32 is that the electrolyte used is changed from diethylene glycol dimethyl ether in Example 32 to: propylene carbonate + ethylene carbonate (500mL + 500mL, Example 41), propylene carbonate + diethyl carbonate (500mL + 500mL, Example 42), propylene carbonate + ethylene carbonate + diethyl carbonate (400mL + 300mL + 300mL, Example 43), propylene carbonate + fluoroethylene carbonate (950mL + 50mL, Example 44).

[0097] Examples 45-54

[0098] The only difference between the negative electrode-free lithium ion batteries in Examples 45-54 and Example 32 is that the electrolyte used replaces the Ca(BH(pftb)3)2 electrolyte additive in Example 32 with: Ca(B(tfe)4)2 (Example 45), Ca(BH(tfe)3)2 (Example 46), Ca(B(Et)4)2 (Example 47), Ca(BH(Et)3)2 (Example 48), Ca(B(hfip)4)2 (Example 49), Ca(BH(hfip)3)2 (Example 50), Ca(B(tf1p)4)2 (Example 51), Ca(BH(tf1p)3)2 (Example 52), Ca(B(tf2p)4)2 (Example 53), Ca(BH(tf2p)3)2 (Example 54).

[0099] Examples 55-60

[0100] The only difference between the negative electrode-free lithium-ion batteries in Examples 55-60 and Example 32 is that the electrolyte used is LiPF6 in Example 32 replaced by LiClO4 (Example 55), LiBOB (Example 56), LiDFOB (Example 57), LiBF4 (Example 58), LiTFSI (Example 59), and LiFSI (Example 60).

[0101] Comparative Example 1

[0102] The only difference between the negative electrode-free sodium ion battery in this example and Example 2 is that the electrolyte used in this example does not contain Ca(BH(pftb)3)2 electrolyte additive.

[0103] Comparative Example 2

[0104] The only difference between the negative electrode-free lithium-ion battery in this example and Example 32 is that the electrolyte used in this example does not contain Ca(BH(pftb)3)2 electrolyte additive.

[0105] Comparative Example 3

[0106] The sodium ion battery in this example is different from that in Example 2 only in that a negative electrode is provided in this example, and the negative electrode is sodium metal (diameter 15.6 mm, thickness 0.5 mm).

[0107] Comparative Example 4

[0108] The lithium-ion battery in this example is different from that in Example 32 only in that this example is provided with a negative electrode, which is lithium metal (diameter 15.6 mm, thickness 0.5 mm).

[0109] Comparative Example 5

[0110] The sodium ion battery in this example is different from that in Example 2 only in that: a negative electrode is provided in this example, and the negative electrode is a hard carbon negative electrode. The preparation method of the hard carbon negative electrode is as follows: 9g hard carbon, 0.5g conductive carbon black, and 0.5g polyvinylidene fluoride are added to 14mL nitrogen methyl pyrrolidone solution, and fully ground to obtain a uniform slurry; then the slurry is evenly coated on the surface of aluminum foil and vacuum dried. The dried electrode sheet is cut into a disc with a diameter of 16mm, and after compaction, it is used as a negative electrode for standby use.

[0111] Comparative Example 6

[0112] The lithium-ion battery in this example is different from that in Example 32 only in that: a negative electrode is provided in this example, and the negative electrode is a graphite negative electrode. The preparation method of the graphite negative electrode is as follows: 9g of graphite, 0.5g of conductive carbon black, and 0.5g of polyvinylidene fluoride are added to 14mL of nitrogen methyl pyrrolidone solution, and fully ground to obtain a uniform slurry; then the slurry is evenly coated on the surface of aluminum foil and vacuum dried. The dried electrode sheet is cut into a disc with a diameter of 16mm, and after compaction, it is used as a negative electrode for standby use.

[0113] Performance Testing

[0114] After the batteries of Examples 2-30, Examples 32-60 and Comparative Examples 1-6 were formed at a constant temperature of 25°C for 24 hours, constant current charge and discharge tests were performed, with a rate of 5C and a test environment temperature of 25°C. The specific test results are shown in Table 1. The cycle life is the number of cycles when the capacity decay is less than 80% of the initial capacity, the average coulomb efficiency refers to the average value of the coulomb efficiency from the first cycle to the cycle life cycle, and the energy density is the battery discharge energy divided by the mass of the positive and negative active materials.

[0115] Table 1 Constant current charge and discharge test results

[0116]

[0117]

[0118]

[0119]

[0120] It can be seen from Table 1 that the energy density, cycle life and average coulombic efficiency of the negative electrode-free sodium ion batteries in Examples 2-30 and the negative electrode-free lithium ion batteries in Examples 32-60 of the present invention are significantly better than those in Comparative Examples 1-6; and compared with other examples, the performance of the negative electrode-free batteries obtained in Examples 2 and 32 is superior.

[0121] After the batteries of Example 2 and Comparative Example 1 were formed at a constant temperature of 25°C for 24 hours, constant current charge and discharge tests were performed at a rate of 5C and a test environment temperature of 25°C. The measured cyclic coulomb efficiency test graphs are shown as follows: Figure 4 and Figure 5 As shown in the figure, the charge and discharge curves of different cycles are respectively as follows: Figure 6 and Figure 7 As shown. Figure 4 and Figure 5 It can be seen that the coulombic efficiency of the negative electrode-free sodium ion battery in Example 2 is very high, the cycle life is long, and it is very stable during the 500-cycle cycle. The average coulombic efficiency of 500 cycles is 99.98%, and the energy density is 338Wh / kg; while the sodium ion battery in Comparative Example 1 does not contain the Ca(BH(pftb)3)2 electrolyte additive, and its coulombic efficiency is low, the cycle life is short, the average coulombic efficiency of 30 cycles is 86.94%, and the energy density is 201Wh / kg, which is significantly inferior to Example 2. Figure 6 and Figure 7It can be seen that the sodium ion battery in Example 2 has excellent charge and discharge stability and slow capacity decay, while the sodium ion battery in Comparative Example 1 does not contain the Ca(BH(pftb)3)2 electrolyte additive, and its battery charge and discharge stability is very poor, and its capacity decays very quickly.

[0122] After charging, the negative electrode-free sodium ion battery in Example 2 was disassembled in a protective atmosphere glove box, and the negative electrode was taken out. The actual picture of the charged negative electrode is as follows: Figure 8 As shown. Figure 8 It can be seen that the Ca(BH(pftb)3)2 electrolyte additive effectively promotes the uniform deposition of sodium on the surface of the current collector, and the surface of the deposited sodium is smooth, thus forming a uniformly deposited negative electrode.

[0123] The XPS graphs of the negative electrode sheets of the negative electrode-free sodium ion batteries in Example 2 and Comparative Example 1 after cycling and charging are respectively tested. The specific test results are as follows: Fig. 9 As shown, Fig. 9 (a) and Fig. 9 (b) are XPS images of the negative electrode sheets in Comparative Example 1 and Example 2; Fig. 9 It can be seen that the inorganic content in the negative electrode SEI of the sodium ion battery containing Ca(BH(pftb)3)2 in Example 2 is significantly increased.

[0124] The SEM images of the negative electrode sheets of the negative electrode-free sodium ion batteries in Example 2 and Comparative Example 1 after cycling and charging are respectively tested. The specific test results are as follows: Fig.10 As shown, Fig.10 (a) and Fig.10 (b) are SEM images of the negative electrode sheets in Comparative Example 1 and Example 2, respectively; Fig.10 It can be observed that the surface of the negative electrode in Comparative Example 1 shows obvious grooves and unevenness, while the surface of the negative electrode in Example 2 is denser and more uniform, indicating that the sodium ion battery negative electrode containing Ca(BH(pftb)3)2 in Example 2 has fewer dendrites, that is, Ca(BH(pftb)3)2 has a good inhibitory effect on dendrites.

[0125] In summary, in the present invention, the cation Ca 2+ A cationic electrostatic shielding layer is formed on the surface of the negative electrode current collector to inhibit the growth of dendrites and reduce the risk of dendrites penetrating the diaphragm and causing battery short circuit. x (OR) y ) - ) adjusts the solvation structure of lithium ions or sodium ions. From the NMR diagram, it can be seen that the Na signal of the electrolyte in the Na spectrum shifts toward the strong field more and more with the increase of the concentration of the electrolyte additive, and the CF signal in the F spectrum also shifts toward the strong field more and more with the increase of the concentration of the electrolyte additive, which shows that the anion group enters the solvation structure of the sodium ion, Ca2+ The electric field strength is much higher than that of lithium ions / sodium ions, which takes away a large number of solvent molecules in the lithium ion / sodium ion solvation structure, effectively reducing the occupancy of solvent molecules in the inner layer solvation structure of lithium ions / sodium ions, and further synergistically realizes the entry of anion groups into the inner layer solvation structure of lithium ions / sodium ions, efficiently realizes the regulation of the solvation structure of lithium ions / sodium ions, and promotes the solvation and desolvation process of lithium ions / sodium ions. At the same time, because the inner layer solvation structure of lithium ions / sodium ions introduces anion groups, the preferential decomposition of high-fluorinated anion groups in the desolvation process is realized, forming a SEI layer with a high F content. The XPS spectrum of the battery pole piece after cycling can show that the highly fluorinated anion groups ((BH x (OR) y ) - ) is introduced, the inorganic content in the SEI layer is significantly improved, which reduces the side reaction between the electrolyte and the negative electrode current collector during the desolvation of lithium ions / sodium ions, enables highly reversible deposition and stripping of lithium ions / sodium ions, and improves the average coulombic efficiency, rate performance, cycle life and energy density of lithium / sodium ion batteries.

[0126] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. An electrolyte additive, Features: Including Ca(BH x (OR) y ) 2 , wherein x is an integer from 0 to 3, y is an integer from 1 to 4, x+y=4, and R is selected from C 1~10 Alkyl, fluorine-substituted C 1~10 At least one of the alkyl groups.

2. The electrolyte additive according to claim 1, Features: The x is 0 or 1; the y is 3 or 4.

3. The electrolyte additive according to claim 1, Features: The R is selected from C 1~5 Alkyl, fluorine-substituted C 1~5 At least one of the alkyl groups.

4. The electrolyte additive according to claim 3, Features: The Ca(BH x (OR) y ) 2 (BH x (OR) y ) - Selected from:

5. A method for preparing the electrolyte additive according to any one of claims 1 to 4, Features: The following steps are involved: Ca(BH 4 ) 2 It is prepared by mixing with ROH to react.

6. An electrolyte, Features: The electrolyte comprises the electrolyte additive according to any one of claims 1 to 4, an electrolyte salt and a solvent.

7. The electrolyte according to claim 6, Features: The electrolyte salt includes a sodium salt, a lithium salt or a potassium salt.

8. The electrolyte according to claim 7, Features: The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonylimide), and lithium bis(fluorosulfonylimide); Or, the sodium salt is at least one selected from sodium hexafluorophosphate, sodium perchlorate, sodium dioxalatoborate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bis(trifluoromethylsulfonyl)imide, and sodium bis(fluorosulfonyl)imide; Or, the potassium salt is selected from at least one of potassium hexafluorophosphate, potassium perchlorate, potassium dioxalatoborate, potassium difluorooxalatoborate, potassium tetrafluoroborate, potassium bistrifluoromethylsulfonyl imide, and potassium bisfluorosulfonyl imide.

9. The electrolyte according to claim 6, Features: The concentration of the electrolyte additive is 0.01-1 mol / L; And / or, the concentration of the electrolyte salt is 0.5-5 mol / L.

10. The electrolyte according to claim 6, Features: The solvent is selected from at least one of esters, sulfones, ethers, nitriles and ionic liquids.

11. An alkali metal ion battery, comprising a positive electrode, a separator and a negative electrode current collector; the separator is located between the positive electrode and the negative electrode current collector, Features: The separator contains the electrolyte according to any one of claims 6 to 10.

12. The alkali metal ion battery according to claim 11, Features: The alkali metal ion battery is an alkali metal ion battery without a negative electrode.

13. The alkali metal ion battery according to claim 11, Features: The alkali metal ion battery includes a sodium ion battery, a potassium ion battery or a lithium ion battery.

14. Use of the electrolyte additive according to any one of claims 1 to 4 and / or the electrolyte according to any one of claims 6 to 10 in the field of batteries.