Dipping nozzle, casting mold, and continuous casting method of steel

By optimizing the discharge area ratio of the impregnation nozzle and using electromagnetic devices to adjust the flow and magnetic field of the molten steel, the problems of inclusion adhesion and melting losses caused by uneven molten steel are solved, and the stability and quality of continuous casting are improved.

CN119053395APending Publication Date: 2024-11-29JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030541.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2023-03-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the continuous casting of steel, the bottom of the impregnation nozzle is unevenly flowing, which affects operating stability and product quality.

Method used

By optimizing the opening area ratio and flow rate of the upper and lower discharge outlets of the immersion nozzle, combined with the use of electromagnetic stirring and brake devices, the magnetic field and gas flow rate are adjusted to control the flow of the steel and the fluctuation of the liquid surface to prevent inclusions from adhesion and melting.

Benefits of technology

The uniformity of liquid steel flow and operating stability are achieved, the refractory reaction of the nozzle and inclusions is reduced, the liquid level fluctuation is reduced, and the quality and efficiency of continuous casting are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053395A_ABST
    Figure CN119053395A_ABST
Patent Text Reader

Abstract

Provided is a technique for reducing the adhesion of inclusions in molten steel to a nozzle and the melting loss of the nozzle while appropriately controlling the flow of the molten steel in a mold. The immersion nozzle supplies molten steel from a molten steel storage container into a casting mold of a continuous casting machine for continuous casting during continuous casting of steel, and the end part of a nozzle main body of the immersion nozzle on the side immersed in the molten steel in the casting mold is closed. The nozzle body has a pair of discharge ports each having a central axis as an axis of symmetry in each of an upper segment and a lower segment of a portion immersed in molten steel, and the opening area of the discharge port in the lower segment is in a range of 1.0-1.6 times the opening area of the discharge port in the upper segment. Preferably, in the flow path inside the immersion nozzle, the ratio r / R of the inner diameter r from the upper end of the discharge port upper hole to the bottom of the lower end of the immersion nozzle to the inner diameter R from the upper end of the discharge port upper hole is in the range of 0.6 or more and less than 1.0; the discharge direction of the discharge port of the upper section and the discharge port of the lower section is arranged at an angle [theta] of 10 DEG or less in plan view.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an immersion nozzle for injecting molten steel into a casting mold during continuous casting of steel, a casting mold for a continuous casting machine using the immersion nozzle, and a continuous casting method for steel. Background Art

[0002] When continuous casting of steel is performed, the immersion nozzle is immersed in the molten steel in the mold to inject the molten steel. Regarding the flow of the molten steel in the mold, the discharge flow from the left and right paired discharge ports of the immersion nozzle collides with the inner wall of the short side of the mold, and is divided into an upward flow that rises along the inner wall of the mold and a downward flow that descends along the inner wall of the mold.

[0003] At this time, especially when the discharge flow rate is high, uneven flow velocity distribution may occur at the upper and lower parts of the discharge port. As a result, the flow balance of the upward and downward flows may be disturbed, resulting in a locally strong discharge flow, which may cause the flow to fluctuate greatly. Such fluctuations may cause defects such as poor formation of solidified shells, and the capture of bubbles and inclusions into the solidified shells.

[0004] In order to solve such a problem, it is considered to make continuous casting possible by slowing down the flow of molten steel in the mold and forming a uniform flow to prevent defects caused by bubbles and inclusions. According to this idea, for example, the following patent document proposes a four-hole immersion nozzle (four-hole nozzle) with molten steel discharge ports arranged in two sections in the upper and lower directions.

[0005] Patent Document 1 discloses a nozzle in which the discharge port area of ​​the upper stage is larger than the discharge port area of ​​the lower stage in order to reduce the maximum falling flow velocity as much as possible, and a continuous casting method using the nozzle.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: International Publication No. 2010 / 109887 Summary of the invention

[0009] Problems to be solved by the invention

[0010] In the technology described in Patent Document 1, although the falling flow rate is successfully reduced, the flow of molten steel to the upper and lower discharge ports is prone to unevenness due to the nature of gravity, resulting in a high pressure at the bottom of the nozzle. Therefore, there is a case where precipitation is generated at the bottom of the nozzle and reacts with inclusions present in the molten steel, and inclusions are attached to the inner tube of the immersion nozzle, causing melting loss of the inner tube. In addition, compared with a two-hole nozzle, the cross-sectional area of ​​each discharge port is smaller, so there is a problem that the adhesion and melting loss disturb the flow of molten steel and easily hinder the operation.

[0011] The present invention has been made to solve the above-mentioned problems, and its object is to provide a technology for reducing the adhesion of inclusions in the molten steel to the nozzle and the nozzle melting loss while appropriately controlling the flow of molten steel in the mold.

[0012] Means for solving problems

[0013] To solve the above problems, the inventors of the present application studied the pressure distribution in the nozzle in order to optimize the opening area ratio of the upper and lower discharge ports of the multi-hole immersion nozzle and the flow rate of each discharge port, and thus achieved the present invention.

[0014] The immersion nozzle provided by the present invention for solving the above-mentioned problems is an immersion nozzle for supplying molten steel from a storage container of molten steel to a mold of a continuous casting machine performing the continuous casting during continuous casting of steel, and is characterized in that the end of the nozzle body of the immersion nozzle on the side immersed in the molten steel in the mold is closed, and the upper section and the lower section of the portion of the nozzle body immersed in the molten steel have a pair of discharge ports each with the central axis as the axis of symmetry, and the opening area of ​​the discharge port of the lower section is in the range of not less than 1.0 times and not more than 1.6 times the opening area of ​​the discharge port of the upper section.

[0015] It should be noted that a more preferred solution for the immersion nozzle according to the present invention is as follows:

[0016] a. In the flow path inside the immersion nozzle, the ratio r / R of the inner diameter r from the upper end of the discharge port hole to the lower end of the immersion nozzle relative to the inner diameter R of the upper end of the discharge port hole is greater than 0.6 and less than 1.0;

[0017] b. The discharge direction of the discharge outlet of the upper section and the discharge outlet of the lower section is configured at an angle θ within 10° in a plan view;

[0018] etc.

[0019] The present invention also relates to a casting mold for a continuous casting machine having any of the above-mentioned immersion nozzles, characterized in that the casting mold is constructed so that the index K affecting the liquid level fluctuation represented by the following formula (1) is within the range of 0.09 to 0.14.

[0020] K 2 = (L 2 +W 2 / 4) / TP 2 (1)

[0021] Wherein, L is the distance from the meniscus to the upper end of the discharge port upper hole of the immersion nozzle [m],

[0022] W is the distance between the short sides of the mold at the meniscus position [m],

[0023] TP is the mass of molten steel passing through per unit time [t / min].

[0024] It should be noted that a more preferred solution for the casting mold involved in the present invention is to include: an electromagnetic stirring device having a DC coil and an AC coil, the electromagnetic stirring device being arranged outside the long side of the casting mold above the discharge outlet of the immersion nozzle, and being capable of applying a magnetic field obtained by superimposing an AC magnetic field on a DC magnetic field to the molten steel in the casting mold; and an electromagnetic braking device having a DC coil, the electromagnetic braking device being arranged outside the long side of the casting mold below the discharge outlet of the immersion nozzle, and being capable of applying a DC magnetic field to the molten steel in the casting mold.

[0025] In addition, the continuous casting method of steel according to the present invention is characterized in that, when continuously casting steel using any of the above-mentioned immersion nozzles, the liquid level fluctuation index K represented by the above-mentioned formula (1) is adjusted to be in the range of 0.09 to 0.14.

[0026] It should be noted that the more preferred solution for the continuous casting method of steel according to the present invention is as follows:

[0027] c. Comparing the magnetic field obtained by superimposing an alternating magnetic field with a magnetic flux density of 0.03 to 0.1 T on a direct magnetic field with a magnetic flux density of 0.1 to 0.8 T to the molten steel in the mold above the discharge outlet of the immersion nozzle immersed in the molten steel in the mold, and comparing the direct magnetic field with a magnetic flux density of 0.1 to 0.8 T to the molten steel in the mold below the discharge outlet;

[0028] d. Ar gas flow rate Q Ar The ratio Q of [NL / min] to the mass of molten steel passing through TP [t / min] Ar / TP is adjusted so that Ar flows in from the upper nozzle;

[0029] etc.

[0030] Effects of the Invention

[0031] According to the immersion nozzle and continuous casting machine of the present invention, by increasing the area of ​​the lower discharge port relative to the area of ​​the upper discharge port of the porous immersion nozzle, it is possible to continuously cast steel without the flow being retained at the bottom of the nozzle to form a high pressure portion and without forming a negative pressure near the discharge port. Therefore, it is possible to prevent adhesion and nozzle melting loss caused by the reaction between the nozzle refractory and the inclusions, and it is expected to reduce the risk of hindering the operation. The immersion nozzle of the present invention is suitable for use in a continuous casting method for steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] [ Figure 1] is a longitudinal cross-sectional view of an immersion nozzle involved in one embodiment of the present invention.

[0033] [ Figure 2 ] is a diagram showing the positional relationship between upper and lower discharge ports in a cross-sectional view of an immersion nozzle according to another embodiment of the present invention.

[0034] [ Figure 3 ] is a graph showing the relationship between the maximum pressure inside the immersion nozzle and the ratio of the cross-sectional area of ​​the upper discharge outlet to the cross-sectional area of ​​the lower discharge outlet.

[0035] [ Figure 4 ] is a graph showing the relationship between the minimum pressure near the discharge port and the ratio of the cross-sectional area of ​​the upper discharge port to the cross-sectional area of ​​the lower discharge port.

[0036] [ Figure 5 ] is a graph showing the relationship between the normalized maximum pressure inside the immersion nozzle and the ratio r / R of the inner diameter of the immersion nozzle.

[0037] [ Figure 6 ] is an explanatory diagram of the positional relationship of the discharge port of the submerged nozzle that affects the floating of Ar bubbles in the mold for the continuous casting machine involved in another embodiment of the present invention. DETAILED DESCRIPTION

[0038] The following is a detailed description of the embodiments of the present invention. It should be noted that each figure is a schematic diagram, which is sometimes different from the actual structure. In addition, the following embodiments illustrate the device and method for concretizing the technical concept of the present invention, and do not limit the structure to the following embodiments. That is, the technical concept of the present invention can be subjected to various changes within the technical scope recorded in the claims.

[0039] [Immersion nozzle]

[0040] Figure 1 This is a longitudinal cross-sectional view showing the front end shape of a multi-hole immersion nozzle according to an embodiment of the present invention. During continuous casting of steel, such an immersion nozzle is immersed in molten steel in a casting mold to inject molten steel. In this embodiment, the nozzle has two pairs of upper and lower discharge ports, a total of four discharge ports, with the central axis 4 as the axis of symmetry, i.e., a so-called four-hole immersion nozzle.

[0041] In the present embodiment, the cross-sectional area of ​​the lower discharge port 2 is set to be 1.0 times or more and 1.6 times or less the cross-sectional area of ​​the upper discharge port 1. The reason is as follows.

[0042] Generally, with regard to a multi-hole immersion nozzle having discharge ports at upper and lower stages, attention is paid to how to obtain a discharge flow rate attenuation effect to reduce defects in cast pieces.

[0043] However, the inventors of the present application have found that the flow of molten steel tends to be biased toward the lower section due to the influence of gravity. As a result, it has been found that the pressure at the bottom 3 of the inner tube of the immersion nozzle becomes high, a stagnant portion is easily formed, and negative pressure is easily formed near the discharge port. As a result of both, it has been found that the reaction between the inclusions in the molten steel and the refractory of the immersion nozzle is induced, causing the inclusions to adhere to the immersion nozzle and the melting loss of the nozzle refractory, making it difficult to perform stable operation.

[0044] First, regarding the immersion nozzle having the upper discharge port 1 and the lower discharge port 2, by making the opening area of ​​the lower discharge port 2 larger than the opening area of ​​the upper discharge port 1, the flow between the upper and lower discharge ports is rectified, and the stagnation area (stagnant part) formed at the bottom 3 of the immersion nozzle is reduced. Regarding the stagnation area, the size of the stagnation part changes the balance of the discharge port areas of the upper and lower stages and the inner diameter of the nozzle body around the discharge port, which are factors that determine the flow of the molten steel, and these factors also affect the "continuity" of the flow field of the molten steel, so it is difficult to predict the influence of each factor separately.

[0045] Therefore, in order to control the formation of stagnation caused by local high pressure and negative pressure parts by balancing the sizes of the upper and lower discharge ports, numerical calculations were used to evaluate the effect of the ratio of the upper and lower discharge port areas on the stagnation part.

[0046] In addition, it is believed that by making a part of the molten steel flow collide with the refractory between the upper and lower discharge outlets, the stagnation portion at the bottom of the nozzle can be controlled even if a part of the molten steel flow is forcibly guided to the upper discharge outlet. By performing numerical calculations, the influence of the change in the inner diameter of the nozzle body around the discharge outlet on the stagnation portion was studied.

[0047] like Figure 2 As shown, the configuration positions of the upper and lower discharge ports 1 and 2 are set to an angle difference θ (°) in the nozzle circumferential direction, preferably with a maximum offset of 10°. The lower discharge port 2 is preferably arranged relative to the short side of the mold in a manner that makes the discharge direction of the molten steel parallel to the long side of the mold, and the upper discharge port 1 is offset in the circumferential direction. This is because, even if it is assumed that aluminum oxide or the like is attached to the nozzle, by making the flow from the upper discharge port 1 collide with the long side of the mold, it is expected that the influence of the molten steel flow directly colliding with the liquid surface can be suppressed. Thus, the influence on the liquid level height can be suppressed at a low level. On the other hand, when the offset angle is too large, the molten steel flow collides with the long side of the mold, thereby deflecting the molten steel flow, and sometimes the liquid level fluctuation may increase due to the upward flow. The angle difference θ is more preferably greater than 1° and less than 10°, and further preferably greater than 3° and less than 10°.

[0048] <Analysis 1>

[0049] First, the immersion nozzle was set to a straight shape with an inner diameter R of 150 mm, and the 4-hole immersion nozzles No. 1 to 5 with upper and lower outlets having openings of the shapes shown in Table 1 were used for numerical calculation. The general thermal fluid analysis solution STAR-CCM+ was used for the analysis, and the steady-state total pressure distribution was calculated and evaluated under the conditions of setting the pressure near the outlet side of the outlet to 0 and the maximum flow rate in the nozzle to 3.0 m / s. In Table 1, "vertical" indicates the vertical direction and "horizontal" indicates the horizontal direction.

[0050] [Table 1]

[0051]

[0052] The analysis results in Table 1 show the relationship between the maximum pressure inside the immersion nozzle and the ratio SL / SU of the cross-sectional area of ​​the upper discharge port 1 to the cross-sectional area of ​​the lower discharge port 2. Figure 3 In the figure, the cross-sectional area of ​​the upper discharge port 1 is SU, and the cross-sectional area of ​​the lower discharge port 2 is SL. Figure 3 As shown in FIG. 1 , as SL / SU increases, that is, as the cross-sectional area of ​​the lower discharge port 2 increases relative to the cross-sectional area of ​​the upper discharge port 1, the maximum pressure tends to decrease, and it is considered that the stagnation caused by high pressure can be eliminated. In particular, when SL / SU is 1.0 or more, a greater pressure reduction effect can be obtained.

[0053] In addition, in the analysis results of Table 1, the relationship between the minimum pressure near the discharge port and the ratio SL / SU of the cross-sectional area of ​​the upper discharge port 1 to the cross-sectional area of ​​the lower discharge port 2 is shown in Figure 4 In the figure. Figure 4 As shown in the figure, as SL / SU increases, the minimum pressure near the discharge port decreases, and in particular, when it is greater than 1.6, it becomes a negative pressure. Inclusions in the molten steel tend to gather at the negative pressure part, and it is considered that this also causes the inclusions in the molten steel to react with the refractory of the immersion nozzle, causing the attachment of the inclusions to the immersion nozzle and the melting loss of the nozzle refractory, just like the stagnation part. Therefore, SL / SU is set to 1.6 or less.

[0054] Analysis 2

[0055] Next, for the immersion nozzle with SL / SU of 1.0, the relationship between the ratio r / R of the inner diameter r from the upper end of the discharge port upper hole to the bottom of the lower end of the immersion nozzle in the flow path inside the nozzle and the maximum pressure is analyzed. The analysis results are shown in Table 2. The maximum pressure in the nozzle when r / R is 1.0 is normalized to 1.0. The relationship between the normalized maximum pressure and the inner diameter ratio r / R is shown in Figure 5 .

[0056] [Table 2]

[0057]

[0058] According to Table 2 and Figure 5 The results show that there is an optimal range for the inner diameter ratio r / R. When the inner diameter ratio is about 0.7, the normalized maximum pressure becomes the minimum, and whether it is smaller or larger than this, the normalized maximum pressure becomes larger. In particular, when r / R is 0.5, the normalized maximum pressure is greater than 1.0. The reason is believed to be: since the proportion of the part where the molten steel flows and the refractory between the upper and lower discharge ports is increased, a new high-pressure part and a dangerous area formed by the stagnant part are formed. Therefore, the inner diameter ratio r / R is preferably greater than 0.6 and less than 1.0. The normalized maximum pressure can be suppressed to less than 1.0. Preferably, r / R is less than 0.9.

[0059] Furthermore, when continuously casting steel, in the case of using an immersion nozzle, an inert gas such as Ar gas can be passed through the upper nozzle and mixed into the molten steel for casting. Thus, the molten steel is subjected to the buoyancy effect of bubbles and the formation of a high pressure portion generated at the bottom 3 of the immersion nozzle can be alleviated.

[0060] However, if the amount of inert gas mixed is too much, the buoyancy of the flow from the immersion nozzle to the meniscus in the mold for casting steel becomes larger, causing large liquid level fluctuations, thus hindering the operation. Therefore, there is a range of appropriate gas injection amount.

[0061] [Mold]

[0062] In the continuous casting method using the above-mentioned immersion nozzle, Ar gas or the like is blown into the nozzle to suppress nozzle clogging caused by adhesion of alumina or the like into the nozzle. In particular, bubbles flowing out from the upper discharge port 1 together with the molten steel may sometimes float and cause the molten steel surface to fluctuate. Figure 6 This is an enlarged conceptual view of a cross section of a casting mold 20 for a continuous casting machine. Figure 6 In the figure, the trajectory of the bubble rising is indicated by the arrow with the mark Ar. In addition, the rising position of the bubble and the diagonal length from the upper discharge port 1 to the short side meniscus position of the mold are √(L 2 +W 2 / 4) and the mass TP of molten steel passing through per unit time. According to the research of the inventors of the present application, it was found that by making the index K affecting the liquid level fluctuation represented by the following formula (1) in the range of 0.09 to 0.14, the liquid level fluctuation can be significantly suppressed. In order to satisfy the relationship of the following formula (1), it is preferred to perform the following controls: change control of the distance between the short sides 8 of the mold, control of the casting speed that affects the mass of molten steel passing through, i.e., the casting sheet drawing speed, control of the immersion depth of the immersion nozzle 10, and so on. As for the distance between the short sides 8 of the mold, since it is fixed due to the required width of the casting sheet, it is preferred to adjust the immersion depth of the immersion nozzle 10 or the casting speed.

[0063] K 2 =(L 2 +W 2 / 4) / TP 2 (1)

[0064] Wherein, L is the distance [m] from the meniscus 5 to the upper end of the discharge port upper hole of the immersion nozzle,

[0065] W is the distance between the short sides 8 of the mold at the location of the meniscus 5 [m],

[0066] TP is the mass of molten steel passing through per unit time [t / min].

[0067] Example

[0068] (Example 1)

[0069] The present invention is constructed as described above. The feasibility and effects of the present invention will be further described below through embodiments.

[0070] When the present nozzle is used for casting by a vertical bending continuous casting machine, the nozzle composition and casting method described in Table 3 are used. As an indicator of the operational stability in Table 3, an eddy current sensor is provided directly above the liquid surface at the center of the thickness from the short side to the center of the width close to 1 / 4 of the distance W (casting width) between the short sides of the mold. The eddy current sensor is used to measure the time-dependent change in the liquid level. At this time, the magnitude of the liquid level fluctuation of treatment No.A1 is set to 100, and the magnitude of the liquid level fluctuation of each treatment is indexed. The average value of the first half and the second half of the casting is used as an index representing the operational stability for evaluation. It should be noted that the discharge outlets of the upper and lower sections are both open in the direction opposite to the short side, and the center of the discharge flow is parallel to the long side of the mold.

[0071] [Table 3]

[0072]

[0073] The results in Table 3 show that the inventive examples all obtained better results than the comparative examples. Ar When the inner diameter ratio r / R is the same, the treatments No. A2 and A4 with the inner diameter ratio r / R set to the appropriate range have better results than the treatments No. A1 and A3 with the inner diameter ratio r / R of 1.0. When the inner diameter ratio r / R is the same, the Ar gas amount blown from the upper nozzle is increased by Q. Ar No. A3 and A4, in which / TP was set in an appropriate range, showed better results than treatment No. A1 and A2, respectively. Among them, treatment No. A4 showed the lowest average liquid level fluctuation index, indicating high operational stability.

[0074] (Example 2)

[0075] Table 4 shows the liquid level fluctuation index when the treatment is performed under the conditions of treatment No. A1 of Example 1 using an immersion nozzle in which the upper discharge port of the immersion nozzle is inclined only at an angle θ in the nozzle circumferential direction relative to the short side of the mold. In treatments No. C2 to C4 in which the angle θ is 3 to 10°, improvement in liquid level fluctuation can be observed compared to treatment No. A1. In treatment No. C5, liquid level fluctuation increases slightly. The reason is believed to be that since the discharge port is excessively inclined toward the long side, the influence of the reverse flow that collides with the long side and reaches the liquid surface becomes greater.

[0076] [Table 4]

[0077]

[0078] (Example 3)

[0079] The liquid level fluctuation index when the treatment was performed under the conditions of Treatment No. A4 of Example 1 using an immersion nozzle in which the upper discharge port of the immersion nozzle was inclined only 7° in the nozzle circumferential direction relative to the short side of the mold is shown in Table 5. In Treatment No. D1, improvement in liquid level fluctuation was observed compared to Treatment No. A4.

[0080] [Table 5]

[0081]

[0082] (Example 4)

[0083] The liquid level fluctuation index when the continuous casting machine of Example 1 was used and the opening area ratio SL / SU of the upper and lower discharge ports was different was used, and various changes were made to the K value of the above formula (1) to treat the liquid level fluctuation index. It should be noted that the inner diameter ratio r / R of the submerged nozzle was 1.00, and the amount of Ar gas injected from the upper nozzle was Q Ar / TP is set to 1.50. When the K value is in the range of 0.09 to 0.14, the improvement of the liquid level fluctuation is significant. On the other hand, when the K value is too small, the liquid level fluctuation is not effectively suppressed due to the influence of the excessive mass of the molten steel passing through, the too narrow casting width, or the too shallow immersion depth of the nozzle. In addition, when the K value is too large, the liquid level fluctuation is not effectively suppressed due to the influence of the excessive mass of the molten steel passing through, the too wide casting width, or the too deep immersion depth of the nozzle. The inventors of the present application believe that maintaining an appropriate deceleration distance for the discharge molten steel flow from the immersion nozzle is effective in suppressing the liquid level fluctuation.

[0084] [Table 6]

[0085] (Example 5)

[0086] In the casting mold of the continuous casting machine of Example 1, Figure 6 The upper section shown in the figure is provided with an electromagnetic stirring device, and the lower section is provided with an electromagnetic braking device. For the electromagnetic stirring device of the upper section, an AC magnetic field is superimposed on a DC magnetic field. For the electromagnetic braking device of the lower section, a DC magnetic field is applied. It should be noted that the inner diameter ratio r / R of the immersion nozzle is 1.00, and the amount of Ar gas blown from the upper nozzle is Q Ar / TP is set to 1.50. Treatment No. F01 is equivalent to Treatment No. E11 of Example 4. Various treatment conditions and liquid level fluctuation indexes are summarized in Table 7. In Treatment Nos. F02 to F10, the liquid level fluctuation index is reduced by applying a magnetic field compared to the case where no magnetic field is applied. On the other hand, in Treatment No. F02, the DC magnetic field in the lower section is too weak, the DC magnetic field in the upper section is too strong, and the AC magnetic field in the upper section is too weak, which is better than the case where no magnetic field is applied, but the liquid level fluctuation is promoted. In addition, in Treatment No. F10, the DC magnetic field in the lower section is too weak, the DC magnetic field in the upper section is too strong, and the AC magnetic field in the upper section is too strong. Although it is good compared to the case where no magnetic field is applied, it promotes liquid level fluctuation. In addition, in Treatment No. F11, although a magnetic field is applied, the discharge port area ratio SL / SU of the upper and lower sections is outside the scope of the present invention, so the liquid level fluctuation index deteriorates. Therefore, it is preferred to apply a DC magnetic field with a magnetic flux density of 0.1 to 0.8 T in the electromagnetic braking device at the lower stage. It is preferred to apply a magnetic field obtained by superimposing an AC magnetic field with a magnetic flux density of 0.03 to 0.1 T on a DC magnetic field with a magnetic flux density of 0.1 to 0.8 T in the electromagnetic stirring device at the upper stage. It can be seen that the liquid level fluctuation can be further improved by appropriately combining magnetic field stirring and magnetic field braking.

[0087] [Table 7]

[0088]

[0089] In this specification, "L" as a unit of volume means 10 -3 m 3 , "t" as a unit of mass refers to metric tons = 10 3 kg, and the symbol "N" for the volume of a gas represents the volume at the standard state, i.e., temperature 0°C and pressure 101325Pa.

[0090] Description of Reference Numerals

[0091] 1 Upper section outlet

[0092] 2 Lower section outlet

[0093] 3 Bottom

[0094] 4 Center axis

[0095] 5. Liquid level (meniscus)

[0096] 6 Electromagnetic stirring device

[0097] 7 Electromagnetic brake device

[0098] 8 Short side of the mold

[0099] 10 Dipping nozzle

[0100] 20 (for continuous casting machine) casting mold

[0101] RInner diameter from the top of the discharge port hole

[0102] rInner diameter from the top of the discharge port to the bottom of the immersion nozzle

[0103] W The distance between the short sides of the mold at the meniscus position

[0104] L is the distance from the meniscus to the upper end of the discharge hole of the immersion nozzle.

Claims

1. An immersion nozzle for supplying molten steel from a storage container of molten steel to a casting mold of a continuous casting machine for continuous casting during continuous casting of steel, wherein: The end of the nozzle body of the immersion nozzle on the side immersed in the molten steel in the mold is closed, and the upper and lower sections of the nozzle body immersed in the molten steel have a pair of discharge ports each with the central axis as the axis of symmetry. The opening area of ​​the discharge port of the lower stage portion is in a range of not less than 1.0 times and not more than 1.6 times the opening area of ​​the discharge port of the upper stage portion.

2. The immersion nozzle according to claim 1, wherein: In the flow path inside the submerged nozzle, the ratio r / R of the inner diameter r from the upper end of the discharge port upper hole to the lower end bottom of the submerged nozzle to the inner diameter R to the upper end of the discharge port upper hole is within a range of 0.6 or more and less than 1.

0.

3. The immersion nozzle according to claim 1 or 2, wherein: The discharge directions of the discharge outlet of the upper stage portion and the discharge outlet of the lower stage portion are arranged at an angle θ within 10° in a plan view.

4. A casting mold for a continuous casting machine having the submerged nozzle according to any one of claims 1 to 3, wherein: The casting mold is constructed so that the index K affecting the liquid level fluctuation represented by the following formula (1) is within the range of 0.09 to 0.

14. K 2 =(L 2 +W 2 / 4) / TP 2 (1) Wherein, L is the distance from the meniscus to the upper end of the discharge port upper hole of the immersion nozzle [m], W is the distance between the short sides of the mold at the meniscus position [m], TP is the mass of molten steel passing through per unit time [t / min].

5. The casting mold according to claim 4, comprising: an electromagnetic stirring device having a DC coil and an AC coil, the electromagnetic stirring device being arranged outside the long side of the mold above the discharge port of the immersion nozzle and capable of applying a magnetic field obtained by superimposing an AC magnetic field on a DC magnetic field to the molten steel in the mold; and An electromagnetic brake device having a DC coil is provided outside the long side of the mold below the discharge port of the immersion nozzle and can apply a DC magnetic field to the molten steel in the mold.

6. A method for continuous casting of steel, wherein: When continuously casting steel using the submerged nozzle according to any one of claims 1 to 3, the liquid level fluctuation index K represented by the following formula (1) is adjusted to be within the range of 0.09 to 0.

14. K 2 =(L 2 +W 2 / 4) / TP 2 (1) Where L is the distance from the meniscus to the upper end of the discharge port hole [m], W is the distance between the short sides of the mold at the meniscus position [m], TP is the mass of molten steel passing through per unit time [t / min].

7. The method for continuous casting of steel according to claim 6, wherein: The molten steel in the mold above the discharge outlet of the immersion nozzle immersed in the molten steel in the mold is subjected to a magnetic field obtained by superimposing an AC magnetic field with a magnetic flux density of 0.03 to 0.1 T on a DC magnetic field with a magnetic flux density of 0.1 to 0.8 T. The molten steel in the mold below the discharge outlet is subjected to a DC magnetic field with a magnetic flux density of 0.1 to 0.8 T.

8. The method for continuous casting of steel according to claim 6 or 7, wherein: The Ar gas flow rate Q Ar The ratio Q of [NL / min] to the mass of molten steel passing through TP [t / min] Ar The Ar was allowed to flow from the upper nozzle by adjusting / TP to be 2.0 or more and 5.0 or less.