Shapeable and flexible haptic materials and structures
By using a composition of piezoelectric polymer and binder in an HMI electronic device to form a flexible piezoelectric transducer, the problem of lack of haptic feedback in the prior art is solved, the manufacturing process is simplified and the size of the device is reduced and weight.
Patent Information
- Application Number
- CN202380035443.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art lacks an effective haptic feedback mechanism when manufacturing human-machine interface (HMI) electronic circuits, resulting in uncertainty in user operations, and existing haptic feedback methods increase the complexity, weight and size of the device.
Using a composition containing a piezoelectric polymer and a binder, a flexible piezoelectric transducer is formed by printing technology for providing tactile feedback, simplifying the manufacturing process, and reducing the size and weight of the electronic device.
This achieves effective haptic feedback in HMI electronic devices, simplifies manufacturing processes, reduces costs, and avoids the drawbacks of using additional rigid devices.
Smart Images

Figure CN119054440A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composition, a method of making the composition, a method of making an in-mold electronic (IME) component, an in-mold electronic (IME) component, a capacitive touch switch, a resistive touch switch, a method of forming a tactile component, and a tactile component. Background Art
[0002] In printed electronics, most human-machine interface (HMI) electronic circuits, structures and surfaces are usually produced by screen printing conductive inks and dielectric inks on thin flexible substrates. Many of these circuits / structures involve resistive touch switches or capacitive touch switches. The problem with some of these touch switches is the lack of human "feel" for the user. In many applications, users usually prefer to have a sensory response or some other feedback to the user's actions, while in other cases, some feedback is usually required to ensure that the correct action has been performed. For example, in an in-mold electronic device such as that used on a car dashboard, the user should be able to receive non-visual feedback while turning a knob in a dark compartment. Devices based on membrane contact switches usually provide passive feedback (a finger presses a metal dome, making an audible click), which relies on the touch feel of a human finger, just as a physical knob relies on touch and linear or rotational movement sensed by a human hand. For a capacitive touch switch, passive feedback can be introduced into the design of the physical shape of the touch position (protrusion or depression) to ensure that the user has touched the correct position. However, in order to ensure that the switch has performed its function when activated, such as turning something on or off, another form of confirmation is required. This feedback can be in the form of an auditory signal or a low-intensity vibration that can be easily sensed by a person's finger (a so-called "tactile feedback mechanism"). The audio signal can be generated using a speaker built using one of the existing technologies (such as an induction coil or a piezoelectric transducer), while the low-intensity vibration can be generated, for example, by an electric motor. Both of these technologies involve the use of additional independent rigid devices, thereby increasing complexity, weight and size.
[0003] There is a need to produce haptic components through similar printing techniques that will be used to make the entire device fully functional, including the haptic feedback mechanism, without compromising any other properties. Summary of the invention
[0004] The present invention is intended to address at least some of the problems associated with the prior art or to provide a commercially acceptable alternative.
[0005] In a first aspect, the present invention provides a composition comprising:
[0006] Piezoelectric polymers, and
[0007] Binder.
[0008] Each aspect or embodiment as defined herein may be combined with any other aspect or embodiment unless clearly indicated to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature indicated as being preferred or advantageous.
[0009] The inventors have surprisingly found that the composition can be used to form a tactile component during a printing method for forming an electronic device. Since the composition can be printed, the formation of the tactile component can be performed using similar printing techniques used to manufacture other components of the device (such as a resistive touch switch or a capacitive touch switch). This can simplify the manufacture of the electronic device, thereby reducing costs. In addition, the size and weight of the electronic device can also be reduced.
[0010] The composition comprises a piezoelectric polymer. As used herein, the term "piezoelectric" may encompass materials in which electric charges accumulate in response to an applied mechanical stress or generate mechanical forces in response to an applied electric field. Without being bound by theory, it is believed that this property is caused by an electric dipole moment formed in certain crystal structures. In piezoelectric materials, these dipoles can be oriented or aligned by a process called poling, in which a high voltage is applied across the material, and the material can be heated to facilitate dipole alignment. After polarization, ferroelectric materials will also exhibit piezoelectric behavior. In the present invention, the piezoelectric properties of the polymer mean that the composition can be used to form a piezoelectric transducer, which can form a part of a tactile component (such as a vibrating component or an audio component in an HMI device). Such a piezoelectric transducer can be activated in response to being touched by a user of the HMI device.
[0011] Inorganic ceramic piezoelectric materials are known, such as lead zirconate. Inorganic crystalline piezoelectric materials exhibit a greater piezoelectric response than other piezoelectric materials - for example, by producing more charge for the same amount of applied mechanical stress - and maintain their piezoelectric properties at higher temperatures than other piezoelectric materials. However, they are rigid and bulky, and require high temperature processing to obtain effective performance. For example, to form a piezoelectric transducer from lead zirconate, lead zirconate powder is combined with additives such as an inert binder and fired at high temperatures (typically in excess of 750°C) to form a solid shape. In contrast, by having a piezoelectric material in the form of a polymer, the composition of the present invention can be processed at sufficiently low temperatures to avoid damaging typical electronic device substrates. In addition, the composition can have rheological properties suitable for printing, and can result in the formation of flexible piezoelectric transducers.
[0012] The piezoelectric polymer is usually included in the composition in the form of a powder.
[0013] The composition may be printable. For example, the composition is preferably capable of screen printing, stencil printing, gravure printing, offset printing and / or roll-to-roll printing, more preferably screen printing. Such techniques are commonly used when printing electronic components.
[0014] The composition comprises a binder. Typically, the piezoelectric polymer is dispersed in the binder. The piezoelectric polymer can be blended with the binder. The binder can be used to hold the composition together ("bonding") and can help provide a composition with a desired rheological property.
[0015] The composition is preferably used in the manufacture of in-mold electronic (IME) components. IME components are typically manufactured by printing electronic circuits onto a flexible substrate and then thermoforming the substrate into a desired shape within a mold. The use of a piezoelectric material in polymer form makes the composition of the present invention flexible enough to retain its form during thermoforming.
[0016] The composition is preferably in the form of an ink. The ink may be suitable for use in printing techniques and / or other dispensing techniques employed in typical methods of manufacturing electronic devices. The ink is preferably a conductive ink or a dielectric ink. Conductive inks and dielectric inks capable of forming tactile components may be particularly useful in the manufacture of HMI electronic devices.
[0017] The composition is preferably in the form of a paste. The paste can be suitably applied to the substrate using typical dispensing techniques employed in methods of manufacturing electronic devices. The paste is preferably a conductive paste or a dielectric paste. Conductive pastes and dielectric pastes capable of forming tactile components can be particularly useful in the manufacture of HMI electronic devices.
[0018] The piezoelectric polymer preferably comprises polyvinylidene fluoride (PVDF). PVDF has the following chemical formula:
[0019]
[0020] PVDF can exhibit particularly advantageous piezoelectric properties and can exhibit an advantageous degree of flexibility. PVDF can also be processed at sufficiently low temperatures to avoid damaging typical substrates used in HMI devices. Without being bound by theory, it is believed that in PVDF, the high electronegativity of the hydrogen-fluorine bonds is responsible for the formation of piezoelectricity.
[0021] Piezoelectric polymers preferably include copolymers of PVDF, more preferably polyvinylidene fluoride-trifluoroethylene copolymers (PVDF-TrFe). Although the unit structure of the copolymer may be less polar than the unit structure of pure PVDF, the copolymer may exhibit higher crystallinity. Compared with pure PVDF, this may result in a greater piezoelectric response. Typically, PVDF crystallizes into a non-polar α phase. Advantageously, by copolymerizing with trifluoroethylene, the fluorine atoms in trifluoroethylene suppress the molecular structure of the polymer, and therefore PVDF-TrFe may be directly crystallized in the ferroelectric β phase. The mass ratio of PVDF to the comonomer may be in the range of 30:70 to 70:30 or 45:55 to 55:45 or 60:40 to 70:30.
[0022] Based on the total weight of the composition, the composition preferably comprises: 5 wt % to 95 wt % of piezoelectric polymer, preferably 15 wt % to 70 wt % of piezoelectric polymer, more preferably 20 wt % to 60 wt % of piezoelectric polymer; and 5 wt % to 95 wt % of binder, preferably 30 wt % to 85 wt % of binder, more preferably 40 wt % to 80 wt % of binder. This can result in a particularly advantageous combination of high piezoelectric response and suitable rheological properties.
[0023] The binder preferably comprises: a thermoplastic resin containing hydroxyl groups, a crosslinking agent, and a solvent. As used herein, the term "thermoplastic resin" can encompass a plastic polymer material that becomes flexible or moldable at a specific elevated temperature and solidifies upon cooling. The use of a thermoplastic resin can ensure that the composition is appropriately flexible during thermoforming, but is solid in the final electronic device. The crosslinking agent can react with the hydroxyl groups at an elevated temperature in order to "cure" the composition. The solvent can be used to dissolve the thermoplastic resin, the crosslinking agent, and any other components of the binder.
[0024] The thermoplastic resin preferably has a glass transition temperature below 100° C. and / or a softening point below 100° C. This can make the composition particularly capable of being thermoformed.
[0025] The thermoplastic resin preferably comprises one or more of polyurethane resin, polyester resin, polyacrylate resin, polyvinyl ester resin, phenoxy resin and ketone resin. Such resins are particularly suitable for the present invention and react with a crosslinking agent under the dry conditions of a typical IME manufacturing process to provide the desired degree of crosslinking.
[0026] Based on the total weight of the thermoplastic resin, the thermoplastic resin preferably comprises: 20 wt % to 60 wt % polyurethane resin, preferably 35 wt % to 47 wt % polyurethane resin, 5 wt % to 30 wt % polyester resin, preferably 13 wt % to 19 wt % polyester resin, and 20 wt % to 60 wt % phenoxy resin, preferably 34 wt % to 51 wt % phenoxy resin. Such ratios of components can provide the composition with particularly advantageous rheological, curing and / or adhesion properties.
[0027] Preferably, the thermoplastic resin:
[0028] Contains homopolymers and copolymers and / or terpolymers; and / or
[0029] having a glass transition temperature of less than 100°C; and / or
[0030] having a weight average molecular weight of 1000 g / mol to 100000 g / mol; and / or
[0031] has a softening point of less than 100°C; and / or
[0032] It has a hydroxyl content (OH number) greater than 20 mgKOH / g.
[0033] This can render the composition particularly capable of thermoforming.High hydroxyl values can lead to advantageously high levels of crosslinking upon curing.
[0034] The crosslinking agent preferably comprises one or more of melamine resin, amino resin, polyamine resin, isocyanate and polyisocyanate, more preferably melamine formaldehyde, even more preferably hexamethoxymethyl melamine. Such substances can react advantageously with the hydroxyl groups of the thermoplastic resin, thereby resulting in an advantageously high degree of crosslinking.
[0035] The crosslinking agent preferably also comprises isocyanate and / or polyisocyanate and / or blocked polyisocyanate. This can increase the level of crosslinking.
[0036] The solvent preferably comprises one or more of an alcohol, a glycol, a glycol ether, a glycol ester, an ester, a ketone, and a hydrocarbon. Such materials may be particularly suitable for dissolving components of the binder and may provide the composition with desired rheological properties.
[0037] Based on the total weight of the solvent, the solvent preferably comprises: up to 95 wt. % of glycol ether acetate, preferably up to 85 wt. % of glycol ether acetate, and / or up to 95 wt. % of glycol ether, preferably up to 85 wt. % of glycol ether, and / or up to 15 wt. % of ester, preferably up to 5 wt. % of ester, and / or up to 40 wt. % of ketone, preferably up to 32 wt. % of ketone, and / or up to 80 wt. % of alcohol, preferably up to 70 wt. % of alcohol and / or up to 30 wt. % of hydrocarbon, preferably up to 22 wt. % of hydrocarbon. Such ratios can make the solvent particularly suitable for dissolving the components of the binder and can provide the composition with desired rheological properties.
[0038] The binder preferably comprises, based on the total weight of the binder: 10 wt % to 40 wt % of a thermoplastic resin, preferably 11 wt % to 30.4 wt % of a thermoplastic resin; 0.5 wt % to 12 wt % of a crosslinking agent, preferably 1.5 wt % to 7.7 wt % of a crosslinking agent; and 40 wt % to 85 wt % of a solvent, preferably 46.7 wt % to 78.8 wt % of a solvent.
[0039] The binder preferably further comprises a thermosetting resin, more preferably one or both of an acrylic resin and an epoxy resin; and a curing catalyst for curing the thermosetting resin, preferably for heat-curing the thermosetting resin and / or for UV-curing the thermosetting resin. The presence of the thermosetting resin and the curing catalyst can be used to form a three-dimensional thermosetting network. This may be beneficial when the dry composition needs to have a stronger "thermosetting" property.
[0040] The binder preferably further comprises one or more functional additives, which are preferably selected from one or more of surfactants, rheology modifiers, dispersants, defoamers, anti-adhesive agents, slip additives, anti-sagging agents, leveling agents, surfactants, surface tension reducers, tackifiers, anti-skinning agents, matting agents, colorants, dyes, pigments and wetting agents.
[0041] Based on the total weight of the binder, the binder preferably comprises: 0.5 wt % to 12 wt % of a crosslinking agent, preferably 1.5 wt % to 7.7 wt % of a crosslinking agent; 10 wt % to 40 wt % of the thermoplastic resin, preferably 11 wt % to 30.4 wt % of the thermoplastic resin; and 40 wt % to 85 wt % of a solvent, preferably 46.7 wt % to 78.8 wt % of a solvent, optionally: 0.1 wt % to 30 wt % of a thermosetting resin and 0.1 wt % to 3 wt % of a curing catalyst for curing the thermosetting resin, preferably 1 wt % to 10 wt % of a thermosetting resin and 0.1 wt % to 1 wt % of a curing catalyst for curing the thermosetting resin; and / or 0.1 wt % to 20 wt % of a functional additive, preferably 1.7 wt % to 17 wt % of a functional additive.
[0042] In another aspect, the present invention provides a method of making a composition as described herein, the method comprising:
[0043] Provide solvent,
[0044] providing a thermoplastic resin having a hydroxyl group,
[0045] dissolving the thermoplastic resin in the solvent at a temperature of 50° C. to 100° C., preferably 70° C. to 100° C.,
[0046] The solution was cooled to room temperature.
[0047] To the cooled solution, a piezoelectric polymer, a cross-linking agent and optionally a functional additive, a thermosetting resin, a curing catalyst for curing the thermosetting resin, one or more of conductive particles and non-conductive particles are added.
[0048] The advantages and preferred features of the first aspect also apply to this aspect.
[0049] Dissolving the thermoplastic resin in the solvent at an elevated temperature can facilitate dissolution of the thermoplastic resin.
[0050] In another aspect, the present invention provides a method of manufacturing an in-mold electronic (IME) component, the method comprising:
[0051] preparing a blank; and
[0052] thermoforming the blank,
[0053] Wherein preparing the blank comprises forming one or more structures on a thermoformable substrate, each structure being formed by a method comprising the steps of:
[0054] disposing the composition described herein on a thermoformable substrate, and
[0055] The composition is dried at a temperature of 20°C to 150°C for 0.5 to 60 minutes.
[0056] The advantages and preferred features of the first aspect also apply to this aspect.
[0057] As used herein, the term "thermoforming" may encompass a manufacturing process in which a plastic sheet is heated to a pliable forming temperature, formed into a specific shape in a mold, and trimmed to create a usable product. The sheet is typically heated in an oven to a sufficiently high temperature to allow it to be stretched into or onto a mold and cooled to its final shape. A simplified version of this is vacuum forming. Pressure may be applied during thermoforming. Thermoforming may include high pressure thermoforming.
[0058] Drying the composition may include evaporating the solvent from the composition. Typically a majority of the solvent is removed from the composition, more typically substantially all of the solvent is removed from the composition.
[0059] The one or more structures preferably comprise a multilayer stack.
[0060] The composition is preferably subjected to an electric field. This can align most of the dipoles in the polymer chain, thereby making the polymer piezoelectric. The composition can be subjected to an electric field before being arranged on the substrate, after being arranged on the substrate but before thermoforming, or after thermoforming. The composition is preferably subjected to an electric field at an elevated temperature. This can promote the alignment of the dipoles.
[0061] The method preferably also includes disposing one or more conductive inks or dielectric inks on the thermoformable substrate before disposing the composition described herein on the thermoformable substrate. In this case, disposing the composition described herein on the thermoformable substrate includes disposing the composition on one or more conductive inks or dielectric inks, which are disposed on the thermoformable substrate. The method may preferably also include, then, disposing one or more conductive inks or dielectric inks on the composition. Thus, the blank may include a thermoformable substrate having a layer of the composition sandwiched between one or more layers of conductive inks and / or dielectric inks. This may result in the integration of a tactile component with a capacitive touch switch or a resistive touch switch.
[0062] The one or more structures preferably comprise a tactile structure, more preferably an audio speaker or a mechanical vibration device.
[0063] The disposing composition preferably comprises a printing composition, more preferably a screen printing, stencil printing, gravure printing, offset printing and / or roll-to-roll printing composition, even more preferably a screen printing composition.
[0064] The substrate preferably comprises one or more of polyethylene terephthalate (PET), polycarbonate (PC), paper, polymethyl methacrylate) (PMMA), polyethylene naphthalate (PEN), polyimide (PI) and thermoplastic polyurethane (TPU). The composition as described herein can be compatible with such materials and form strong adhesion with such materials. Such materials also exhibit favorable thermoforming properties.
[0065] Thermoforming is preferably carried out at a temperature of 140°C to 210°C. Such conditions can result in particularly advantageous thermoforming, but without causing damage to the substrate and / or degradation of the components of the composition. Such temperatures are particularly suitable for thermoforming, and the compositions described herein can be stable at such temperatures. Thermoforming can include vacuum thermoforming. In a preferred embodiment, vacuum thermoforming is carried out at a pressure of 0.25MPa to 0.4MPa. In another preferred embodiment, high pressure thermoforming is carried out at a pressure in the range of 6MPa to 12MPa.
[0066] Preferably, the method further comprises applying a resin layer to the substrate using injection molding after thermoforming, preferably wherein the resin comprises one or more of polycarbonate (PC), polyethylene terephthalate (PET), acrylonitrile butadiene styrene (ABS), polypropylene (PP), polyester, poly(methyl methacrylate) (PMMA), low density polyethylene (LDPE), high density polyethylene (HDPE), polystyrene (PS) and thermoplastic polyurethane (TPU). Other similar resins may also be used. Such resin layers may provide advantageous mechanical and / or aesthetic properties to the final IME component.
[0067] Injection molding is preferably performed at a temperature of 170° C. to 330° C. Such temperatures are particularly suitable for injection molding, and the compositions described herein may be stable at such temperatures.
[0068] Preparing the blank preferably further comprises forming one or more conductive layers and / or dielectric layers on the substrate and / or structure.
[0069] The in-mold electronics (IME) component preferably includes a capacitive touch switch, a resistive touch switch, or a capacitive touch sensor.
[0070] In-mold electronics (IME) components preferably include one or more of displays, lights / luminaires, sensors, indicator lights, and haptic / tactile feedback devices.
[0071] In another aspect, the present invention provides an in-mold electronic (IME) component manufactured according to the method described herein.
[0072] The advantages and preferred features of the first aspect also apply to this aspect.
[0073] In another aspect, the present invention provides an in-mold electronic (IME) component comprising the composition described herein.
[0074] The advantages and preferred features of the first aspect also apply to this aspect.
[0075] In another aspect, the present invention provides an in-mold electronic (IME) component comprising a piezoelectric polymer.
[0076] The advantages and preferred features of the first aspect also apply to this aspect.
[0077] The in-mold electronic (IME) components of the last three aspects preferably include haptic components.
[0078] In another aspect, the present invention provides a capacitive touch switch or a resistive touch switch including the in-mold electronics (IME) component described herein.
[0079] The advantages and preferred features of the first aspect also apply to this aspect.
[0080] The haptic is preferably sandwiched between two electrodes, more preferably wherein one of the electrodes comprises a touch pad.
[0081] The haptic is preferably dielectric.
[0082] The capacitive touch preferably also includes a dielectric layer between the tactile component and each electrode.
[0083] In another aspect, the present invention provides a method of forming a haptic, the method comprising:
[0084] providing a substrate;
[0085] disposing a composition as described herein onto a substrate; and
[0086] The composition is dried at a temperature of 20°C to 150°C for 0.5 to 60 minutes.
[0087] The advantages and preferred features of the first aspect also apply to this aspect.
[0088] In another aspect, the present invention provides a haptic formed using a method described herein or comprising a composition described herein.
[0089] The advantages and preferred features of the first aspect also apply to this aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0090] The present invention will now be further described with reference to the following drawings, in which:
[0091] Figure 1 a. Figure 1 b and Figure 1 c is a photograph of a touch pad formed using the composition of the present invention.
[0092] Figure 2 Shows that when you press repeatedly with your finger Figure 1 A touch of the pad displays the electrical response on the oscilloscope screen.
[0093] Figure 3 An oscilloscope screenshot showing force sensing signals from a polymer-based haptic integrated with a capacitive touch switch.
[0094] Figure 4 The force signal detected from the printed touch sensor is shown. DETAILED DESCRIPTION
[0095] The present invention will now be further described with reference to the following examples.
[0096] Example
[0097] A dual-electrode touch pad was prepared according to the following method. A flexible polycarbonate film was first provided. A conductive silver ink was printed on the film to form a bottom electrode. A composition according to the invention in the form of an ink was then printed on the bottom electrode to form a tactile layer, and a conductive silver ink was printed on the tactile layer to form a top electrode. The ink was then cured in a hood at a temperature below 120° C. The resulting touch pad was placed in a Figure 1 Shown in a.
[0098] Two further two-electrode touch pads were prepared using a similar process. However, after curing, the touch pads were thermoformed at a temperature of 150°C to 180°C. Figure 1 b and Figure 1 The resulting thermoformed touchpad is shown in c.
[0099] Figure 1 The touch pads of a were connected to an oscilloscope to monitor the electrical signals generated during the experiment. During the initial experiment, the center pad was repeatedly pressed with a finger to observe whether any electrical signals were generated. To avoid grounding through the human body, electrical insulating tape was taped on top of the top electrode.
[0100] Figure 2 The electrical response displayed on the oscilloscope screen when the touch pad is repeatedly pressed with a finger is shown. No filtering circuit is used between the touch pad and the oscilloscope. Therefore, multiple peaks are observed for each touch, showing the natural response and naturally damped vibration as expected. The touch pad formed into a 3D shape ( Figure 1 b and Figure 1 c) also shows similarity to the flat sample ( Figure 1a). Extreme forming (where samples are stretched beyond the limits of the materials used to make them) can lead to performance degradation or failure. For example, failure of a conductive ink may be a loss of conductivity, whereas failure of a dielectric or tactile layer may be an increase in leakage current (loss of isolation).
[0101] Figure 3 A typical electrical response from an active tactile layer beneath a capacitive touch pad made in accordance with the present invention is shown. In this case, a known weight was placed on the touch pad. The response was recorded as the weight was quickly lifted. As expected, variations in the response time were observed because the weight was manually lifted. Similar responses were observed when the weight was placed on the sample. The manual nature of the experiment means that the stimulus rate / time applied varies, and therefore the observed response time varies. The polarity of the electrical signal is not important here, as it depends on the order of the probe terminals.
[0102] Figure 4 Shows Figure 1 a shows the total energy response of the tactile member / sensor versus the applied force. The total energy response is calculated as Figure 3 The fully integrated area under the response curve shown in . This integration is used to remove the variations caused by manual experimentation. Each data point is the average of a large number of measurements. Experiments with different samples produce similar responses. The response signal increases as the applied force increases. This shows that the structure can be used as a force sensor. Alternatively, a touch sensor switch can be used to turn on a voltage to physically expand or contract the active tactile layer. An AC voltage signal can be used to vibrate the stack at a preset frequency and send a sensing signal back to an object touching the pad.
[0103] The above detailed description has been provided by way of explanation and illustration and is not intended to limit the scope of the appended claims. Many variations of the preferred embodiments of the invention shown herein will be apparent to those of ordinary skill in the art and are still within the scope of the appended claims and their equivalents.
Claims
1. A composition comprising: Piezoelectric polymers, and Binder.
2. The composition of claim 1, wherein the composition is used to make in-mold electronic (IME) parts.
3. A composition according to claim 1 or claim 2, in the form of an ink, preferably wherein the ink is a conductive ink or a dielectric ink.
4. A composition according to claim 1 or claim 2, in the form of a paste, preferably wherein the paste is a conductive paste or a dielectric paste.
5. A composition according to any preceding claim, wherein the piezoelectric polymer comprises polyvinylidene fluoride (PVDF).
6. The composition of claim 5, wherein the piezoelectric polymer comprises polyvinylidene fluoride-trifluoroethylene copolymer (PVDF-TrFe).
7. A composition according to any preceding claim, comprising, based on the total weight of the composition: 5 wt % to 95 wt % piezoelectric polymer, preferably 15 wt % to 70 wt % piezoelectric polymer, more preferably 20 wt % to 60 wt % piezoelectric polymer; and 5 to 95 wt% binder, preferably 30 to 85 wt% binder, more preferably 40 to 80 wt% binder.
8. A composition according to any preceding claim, wherein the binder comprises: A thermoplastic resin containing a hydroxyl group, Crosslinking agent, and Solvent.
9. The composition according to claim 8, wherein the thermoplastic resin has a glass transition temperature of less than 100°C and / or a softening point of less than 100°C.
10. The composition according to claim 8 or claim 9, wherein the thermoplastic resin comprises one or more of a polyurethane resin, a polyester resin, a polyacrylate resin, a polyvinyl ester resin, a phenoxy resin and a ketone resin.
11. The composition of claim 10, wherein the thermoplastic resin comprises, based on the total weight of the thermoplastic resin: 20 to 60 wt% of polyurethane resin, preferably 35 to 47 wt% of polyurethane resin, 5 to 30 wt% of polyester resin, preferably 13 to 19 wt% of polyester resin, and 20 to 60 wt% of phenoxy resin, preferably 34 to 51 wt% of phenoxy resin.
12. The composition according to any one of claims 8 to 11, wherein the thermoplastic resin: Contains homopolymers and copolymers and / or terpolymers; and / or having a glass transition temperature of less than 100°C; and / or having a weight average molecular weight of 1000 g / mol to 100000 g / mol; and / or has a softening point of less than 100°C; and / or It has a hydroxyl content (OH number) greater than 20 mgKOH / g.
13. The composition according to any one of claims 8 to 12, wherein the crosslinking agent comprises one or more of a melamine resin, an amino resin, a polyamine resin, an isocyanate, and a polyisocyanate.
14. The composition of any one of claims 8 to 13, wherein the crosslinking agent comprises melamine formaldehyde.
15. The composition of claim 14, wherein the melamine formaldehyde comprises hexamethoxymethylmelamine.
16. The composition according to claim 14 or claim 15, wherein the crosslinking agent further comprises isocyanate and / or polyisocyanate and / or blocked polyisocyanate.
17. The composition of any one of claims 8 to 16, wherein the solvent comprises one or more of an alcohol, a glycol, a glycol ether, a glycol ester, an ester, a ketone, and a hydrocarbon.
18. The composition of claim 17, wherein the solvent comprises, based on the total weight of the solvent: Up to 95% by weight of glycol ether acetate, preferably up to 85% by weight of glycol ether acetate, and / or Up to 95% by weight of glycol ethers, preferably up to 85% by weight of glycol ethers, and / or Up to 15% by weight of esters, preferably up to 5% by weight of esters, and / or up to 40 wt. % ketones, preferably up to 32 wt. % ketones, and / or up to 80% by weight of alcohol, preferably up to 70% by weight of alcohol, and / or Up to 30 wt% hydrocarbons, preferably up to 22 wt% hydrocarbons.
19. The composition according to any one of claims 8 to 18, wherein the binder comprises, based on the total weight of the binder: 10 to 40 wt% of said thermoplastic resin, preferably 11 to 30.4 wt% of said thermoplastic resin; 0.5 to 12 wt% of the crosslinking agent, preferably 1.5 to 7.7 wt% of the crosslinking agent; and 40 to 85 wt% solvent, preferably 46.7 to 78.8 wt% solvent.
20. The composition according to any one of claims 8 to 19, wherein the binder further comprises a thermosetting resin, preferably one or both of an acrylic resin and an epoxy resin; and A curing catalyst, the curing catalyst is used for curing the thermosetting resin, preferably for thermally curing the thermosetting resin and / or for UV curing the thermosetting resin.
21. A composition according to any preceding claim, wherein the binder further comprises one or more functional additives, preferably selected from one or more of surfactants, rheology modifiers, dispersants, defoamers, anti-adhesive agents, slip additives, anti-sagging agents, leveling agents, surfactants, surface tension reducers, tackifiers, anti-skinning agents, matting agents, colorants, dyes, pigments and wetting agents.
22. A composition according to any preceding claim, wherein the binder comprises, based on the total weight of the binder: 0.5 wt % to 12 wt % of the crosslinking agent, preferably 1.5 wt % to 7.7 wt % of the crosslinking agent; 10 to 40 wt% of said thermoplastic resin, preferably 11 to 30.4 wt% of said thermoplastic resin; and 40% to 85% by weight of solvent, preferably 46.7% to 78.8% by weight of solvent, optionally: 0.1 wt % to 30 wt % of a thermosetting resin and 0.1 wt % to 3 wt % of a curing catalyst for curing the thermosetting resin, preferably 1 wt % to 10 wt % of a thermosetting resin and 0.1 wt % to 1 wt % of a curing catalyst for curing the thermosetting resin; and / or 0.1 wt% to 20 wt% of functional additives, preferably 1.7 wt% to 17 wt% of functional additives.
23. A method of making a composition according to any one of claims 8 to 22, the method include: Provide solvent, providing a thermoplastic resin having a hydroxyl group, dissolving the thermoplastic resin in the solvent at a temperature of 50° C. to 100° C., preferably 70° C. to 100° C., The solution was cooled to room temperature. To the cooled solution, a piezoelectric polymer, a cross-linking agent and optionally a functional additive, a thermosetting resin, a curing catalyst for curing the thermosetting resin, one or more of conductive particles and non-conductive particles are added.
24. A method of manufacturing an in-mold electronic (IME) component, the method include: preparing a blank; as well as thermoforming the blank, Wherein preparing the blank comprises forming one or more structures on a thermoformable substrate, each structure being formed by a method comprising the steps of: providing a composition according to any one of claims 1 to 22 on a thermoformable substrate, and The composition is dried at a temperature of 20°C to 150°C for 0.5 to 60 minutes.
25. A method according to claim 24, wherein the one or more structures comprise a tactile structure, preferably an audio speaker or a mechanical vibration device.
26. A method according to claim 24 or claim 25, wherein providing the composition comprises printing the composition, preferably screen printing the composition.
27. The method of any one of claims 24 to 26, wherein the substrate comprises one or more of polyethylene terephthalate (PET), polycarbonate (PC), paper, poly(methyl methacrylate) (PMMA), polyethylene naphthalate (PEN), polyimide (PI), and thermoplastic polyurethane (TPU).
28. The method according to any one of claims 24 to 27, wherein the thermoforming is carried out at a temperature of 140 to 210°C and / or at a pressure of 0.25 to 0.4 MPa and / or at a pressure in the range of 6 to 12 MPa.
29. The method according to any one of claims 24 to 28, further comprising applying a resin layer to the substrate using injection molding after thermoforming, preferably wherein the resin comprises one or more of polycarbonate (PC), polyethylene terephthalate (PET), acrylonitrile butadiene styrene (ABS), polypropylene (PP), polyester, poly(methyl methacrylate) (PMMA), low density polyethylene (LDPE), high density polyethylene (HDPE), polystyrene (PS) and thermoplastic polyurethane (TPU).
30. The method of claim 29, wherein the injection molding is performed at a temperature of 170°C to 330°C.
31. The method of any one of claims 24 to 30, wherein preparing the blank further comprises forming one or more conductive and / or dielectric layers on the substrate and / or structure.
32. The method of any one of claims 24 to 31, wherein the in-mold electronics (IME) component comprises a capacitive touch switch, a resistive touch switch, or a capacitive touch sensor.
33. A method according to any one of claims 24 to 32, wherein the in-mold electronics (IME) component comprises one or more of a display, a lamp / light fixture, a sensor, an indicator light and a haptic / tactile feedback device.
34. An in-mold electronic (IME) component manufactured according to the method of any one of claims 24 to 33.
35. An in-mold electronic (IME) component comprising the composition of any one of claims 1 to 22.
36. An in-mold electronic (IME) component comprising a piezoelectric polymer.
37. An In-Mold Electronics (IME) component according to any one of claims 33 to 35, wherein the component comprises a haptic component.
38. A capacitive touch switch or a resistive touch switch, comprising an in-mold electronics (IME) component according to any one of claims 24 to 37.
39. A capacitive touch switch or a resistive touch switch according to claim 38, wherein the tactile component is sandwiched between two electrodes, preferably one of the electrodes comprises a touch pad.
40. The capacitive touch switch of claim 39, wherein the tactile component is dielectric.
41. The capacitive touch switch of claim 39, further comprising a dielectric layer between the tactile component and each electrode.
42. A method of forming a haptic component, the method include: providing a substrate; disposing the composition according to any one of claims 1 to 22 on the substrate; as well as The composition is dried at a temperature of 20°C to 150°C for 0.5 to 60 minutes.
43. A haptic formed using the method of claim 42 or comprising the composition of any one of claims 1 to 22.