Catalyst for preparing ethylene and propylene through catalytic cracking as well as preparation and application of catalyst
By combining silica, potassium and metal oxides with ZSM-5 molecular sieve in the catalyst, a bimetal modified catalyst is formed, which solves the problem of low selectivity and yield of ethylene propylene in n-butane cracking of existing catalysts. , achieving efficient catalytic effects and low-cost industrial applications.
Patent Information
- Application Number
- CN202310635246.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The selectivity and yield of ethylene propylene in the catalytic cracking of n-butane are low, and the preparation process is complex and the cost is high, making it difficult to meet the needs of industrial applications.
Using catalysts including silica, potassium, molecular sieve and metals or oxides attached to the molecular sieve, the activity and selectivity of the catalyst are improved by specific preparation methods, including mixing metal oxides with ZSM-5 molecular sieve and SiO2, and adding them. Potassium tartrate is roasted to form a bimetal modified molecular sieve catalyst.
It significantly improves the conversion rate of n-butane and the yield of ethylene propylene, reduces the harshness of the reaction, improves the stability and wear resistance of the catalyst, is low in cost, and is suitable for industrial applications.
Smart Images

Figure BDA0004260161330000161 
Figure BDA0004260161330000171
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst for preparing ethylene and propylene through catalytic cracking, and the preparation and application of the catalyst. Background Art
[0002] Ethylene and propylene are important products in the field of petrochemicals. They are also the most important basic organic chemical raw materials in chemical production and occupy an important position in the national economy. At present, steam cracking of petroleum hydrocarbons is still the main process for producing dienes. About 90% of ethylene, 35% of propylene and 20% of butene in my country are produced from naphtha steam cracking. After years of development, the steam cracking process has become very mature, but it still has inherent disadvantages such as high construction cost, high energy consumption of the device, fixed product composition and high carbon emissions. At the same time, methods for preparing dienes such as catalytic cracking, propane dehydrogenation and methanol to olefins (MTO / MTP) have rapidly emerged. Among them, catalytic cracking has the advantages of flexible operation, wide source of raw materials, low energy consumption and low production cost, and can effectively control the ratio of propylene to ethylene, which has important practical significance.
[0003] With the rapid development of the oil refining industry, a large amount of C4 alkanes are produced as by-products during the extraction of oil and natural gas and oil refining, but their outlets are very narrow and they can usually only be treated as fuel. The demand gap for ethylene and propylene has turned people's attention to the preparation of ethylene and propylene through low-carbon alkanes. The temperature for catalytic cracking to produce propylene and ethylene is usually around 550°C. There are a large number of reports on existing olefin catalytic cracking technologies. The active components of the catalysts used are mainly hydrogen-type molecular sieves such as ZSM-5, ZSM-11, SAPO-34 and other molecular sieves. Due to the relatively low reaction activity of alkanes, the reaction usually requires a temperature above 600°C; due to the insufficient stability of the molecular sieve catalyst, the catalyst stability is poor. Some research on the application of metal oxide catalysts has made some progress, but there is still a certain gap from industrial application.
[0004] In the prior art, hydrocarbon cracking mostly uses easily cracked butene, isobutane or their mixture as raw materials, and uses molecular sieves or modified molecular sieves as catalysts to produce light olefins. However, n-butane, as a raw material with relatively stable chemical properties, has not been efficiently utilized, and the catalyst preparation process used in the prior art is complex and costly. The catalytic cracking of n-butane to produce ethylene and propylene has the problems of low diene selectivity and low single-pass yield of propylene. Summary of the invention
[0005] The present invention is made in order to further improve the efficiency of preparing ethylene and propylene by catalytic cracking and increase the selection space of related catalysts.
[0006] The catalyst referred to in this application refers to a catalyst product including a molecular sieve and a metal or its oxide, silicon dioxide, potassium and other components attached to the molecular sieve. The product is generally sold on a dry basis after calcination.
[0007] As one aspect of the present invention, it relates to a catalyst for preparing ethylene and propylene by catalytic cracking, the catalyst comprising silicon dioxide, potassium, molecular sieve and metal or its oxide attached to the molecular sieve, wherein the mass ratio of molecular sieve, silicon dioxide, metal oxide and K2O is 30-50:30-65:5-20:0.1-5, when the catalyst comprises metal, it is calculated as its metal oxide, and the potassium in the catalyst is calculated as potassium oxide. Preferably, the mass ratio of molecular sieve, silicon dioxide, metal oxide and K2O is 35-45:45-55:5-10:1-3. In a specific embodiment, the molecular sieve accounts for 30-50% of the total weight of the catalyst, the metal oxide accounts for 5-20% of the total weight of the catalyst, and the K2O accounts for 0.1-5% of the total weight of the catalyst. In a specific embodiment, the metal or its oxide comprises M1 and M2, wherein M1 is selected from Ga, In, Bi or its metal oxide, and M2 is selected from Fe, Zn or its metal oxide. The mass ratio of M1 to M2 is 1-7:1, preferably 1-2:1.
[0008] As another aspect of the present invention, it relates to a method for preparing the above catalyst, comprising:
[0009] (1) Dissolve soluble salts of M1 and M2 in water;
[0010] (2) adding and mixing with ZSM-5 molecular sieve and SiO2 powder;
[0011] (3) Add potassium tartrate, adjust the pH value to 7-9, and allow to stand for aging and roasting.
[0012] In the step (1), the soluble salts of M1 and M2 are nitrates, nitrites or sulfates of M1 and M2.
[0013] In the step (3), the static aging temperature is 60-80°C, and the static aging time is 2-24h.
[0014] In the step (3), the calcination is first carried out at 450-600°C for 2-3 hours, and then at 600-750°C for 1-2 hours.
[0015] As another aspect of the present invention, it relates to the use of the catalyst for preparing ethylene and propylene by catalytic cracking in the catalytic cracking of n-butane.
[0016] As another aspect of the present invention, it relates to a process for preparing ethylene and propylene by catalytic cracking of n-butane, using the above catalyst.
[0017] In a specific embodiment, the reaction conditions of the process for preparing ethylene and propylene by catalytic cracking of n-butane include, for example, a temperature of 500 to 650° C., normal pressure, and a gas volume space velocity of 1200 to 1600 h -1 The agent-oil ratio is 3 to 10, and the agent-oil ratio is a weight ratio.
[0018] When the catalyst provided by the invention is applied to catalytic cracking of butane to prepare ethylene and propylene, it has good conversion rate, propylene yield and ethylene and propylene selectivity.
[0019] The catalyst of the invention has high catalytic efficiency and is simple and easy to prepare.
[0020] By utilizing a large amount of n-butane produced as a by-product during the extraction of petroleum and natural gas and petroleum refining as a raw material and adopting the bimetallic modified ZSM-5 molecular sieve containing potassium salt provided by the present invention as a catalyst, the activity of the catalyst and the selectivity of ethylene and propylene are improved, the conversion rate of n-butane is greatly improved, and the yields of ethylene and propylene are increased.
[0021] The present invention uses common ZSM-5 molecular sieve mixed with metal and other materials, has simple process and low cost.
[0022] Since the catalytic cracking conditions of butane are often harsh, the present invention mainly focuses on the catalytic cracking reaction, and synthesizes a dual-carrier metal modified catalyst to have a higher catalytic reaction activity, reduce the reaction severity to a certain extent, and improve the selectivity and yield of ethylene and propylene. DETAILED DESCRIPTION
[0023] The inventors referred to CN103071522A and prepared the corresponding multi-level pore ZSM-5 molecular sieve as a catalyst using SiO2, Al2O3, TPAOH and a second template. This method requires a special method to prepare multi-level pore ZSM-5, which is complex and costly and cannot meet the inventors' expectations.
[0024] Ji Dong et al. (Ji Dong, Wang Yi, Liu Tao, Su Yi, Li Ping, Gao Xionghou. Research on the catalytic cracking of C4 alkanes to ethylene and propylene by high-silicon molecular sieve ZSM-23 [J]. Molecular Catalysis, 2007 (03): 193-199.) used silica sol as the silicon source and pyrrolidine as the template agent to synthesize ZSM-23 molecular sieves with different silicon-aluminum ratios by static hydrothermal crystallization method. Among them, the catalytic performance of ZSM-23 molecular sieve with a silicon-aluminum ratio of 30 was the best. Under the conditions of reaction temperature of 600℃ and GHSV: 3000ml / h / g, the yield of ethylene and propylene reached 56.0% and the conversion rate reached 88.9%. The raw material composition was 54.5% n-butene, 44.7% isobutylene and 0.8% other hydrocarbons. This C4 raw material with high olefin content is easier to react to obtain a high olefin yield. However, the inventor used it for alkane cracking, and the effect was not as good as the inventor expected.
[0025] CN104557396A discloses a method for producing propylene by catalytic cracking of n-butene, wherein phosphorus-modified SAPO-11 molecular sieve catalyst and ZSM-5 molecular sieve catalyst are used at a reaction temperature of 500-600°C and a weight space velocity of 1-10h -1 , etherified C4 as raw material, propylene yield can reach 39%. However, the inventor used it for alkane cracking, and the effect was not as good as the inventor expected.
[0026] The inventors referred to CN1026100C and prepared a cracking catalyst by loading metal palladium or platinum on activated alumina by impregnation. This method uses precious metals as active components, which is costly. At the same time, diluents are used during the reaction, which is not conducive to industrial scale-up. When n-butane is used as the raw material, the propylene yield is only 8%, which is lower than the inventors' expectations.
[0027] Ma Liqing et al. disclosed in the literature Ma Liqing, Weng Huixin. Research on catalytic cracking of n-butane to produce ethylene and propylene [J]. Natural Gas Chemical Industry (C1 Chemistry and Chemical Engineering), 2010, 35(02): 18-21+27.) that the rare earth-containing five-membered ring zeolite ZRP-1 catalyst has a good effect on the catalytic cracking of n-butane to produce ethylene and propylene, but the synthesis of the catalyst requires the use of rare earth and has high requirements on process conditions.
[0028] In his paper on the preparation of Co-based HZSM-5 catalyst and its catalytic cracking of n-butane, Ma Xiaobiao synthesized Co@ZSM-5 in situ. When the reaction temperature was 550°C and the flow ratio of n-butane to nitrogen was 1:19 (2mL / min:38mL / min), the butane conversion rate was 58.5%, the propylene yield was 15.2%, and the ethylene yield was 13.7%. However, the catalyst preparation cost of this study was high, diluents were used in the reaction process, and the propylene yield was low, which was not suitable for industrial application.
[0029] The inventors referred to CN101279287A to prepare a catalyst for catalytic cracking to produce olefins, by using metals loaded on ZSM-5 / mordenite symbiotic molecular sieves, ZSM-5 / β zeolite symbiotic molecular sieves or ZSM-5 / Y symbiotic molecular sieves for naphtha cracking to produce ethylene and propylene. It was found that due to the inappropriate content of silica in the symbiotic molecular sieve and the high content of 80-99.5% of the symbiotic molecular sieve, the catalyst was difficult to shape, and the wear resistance during use was poor, which was not suitable for industrial applications and could not meet the inventors' expectations. The symbiotic molecular sieve is a molecular sieve with a special structure. If it is to be used in large quantities as a catalyst, it needs to be specially customized, the cost is high, and it is not suitable for industrial applications.
[0030] In view of the fact that the prior art cannot meet the inventor's expectations, the inventor made the present invention after further research and development.
[0031] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0032] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.
[0033] The prepared catalyst was evaluated in a microreactor (manufacturer: Qingdao Jietian Technology) at a reaction temperature of 620°C and a gas volume space velocity of 1500 h -1 The preparation methods of different catalysts are shown in Examples 1 to 5, and the evaluation results are shown in Table 1. 99.5 wt% of n-butane is used as the raw material.
[0034] Example 1
[0035] The preparation of the catalyst is completed according to the following steps:
[0036] Step (1): dissolving 15 g of gallium nitrate and 8 g of ferric nitrate in 80 g of water at room temperature, heating the water bath to 60° C. to completely dissolve the gallium nitrate and 8 g of ferric nitrate, to obtain a mixed solution of metals;
[0037] Step (2): 35 g of ZSM-5 molecular sieve and 54.86 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 1 hour to obtain a mixed slurry;
[0038] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7, continue stirring for 2 h, and stand at 60° C. for aging for 3 h.
[0039] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.2 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 700°C for 1 hour. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-1 is obtained.
[0040] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 35: 54.86: 8.14: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is gallium oxide and M2 is iron oxide, and M1:M2 = 2.08:1.
[0041] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-1 catalyst prepared in Example 1.
[0042] Evaluation results of the catalyst: n-butane conversion was 70.48%, ethylene yield was 21.73 wt%, and propylene yield was 23.64 wt%.
[0043] Example 2
[0044] The preparation of the catalyst is completed according to the following steps:
[0045] Step (1): dissolving 15 g of indium nitrate and 8 g of ferric nitrate in 80 g of water at room temperature, heating the water bath to 60° C. to completely dissolve the indium nitrate and obtain a mixed solution of metals;
[0046] Step (2): 35 g ZSM-5 molecular sieve and 53.44 g SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 1 hour to obtain a mixed slurry;
[0047] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 9, continue stirring for 2 h, and stand at 60° C. for aging for 3 h.
[0048] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.3 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 650°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-2 is obtained.
[0049] The mass ratio of the catalyst components is as follows: molecular sieve: SiO2: metal oxide: K2O = 35: 53.44: 9.56: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is indium oxide and M2 is iron oxide, and M1:M2 = 2.62:1.
[0050] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-2 catalyst prepared in Example 2.
[0051] Evaluation results of the catalyst: n-butane conversion was 65.72%, ethylene yield was 17.80 wt%, and propylene yield was 22.43 wt%.
[0052] Example 3
[0053] The preparation of the catalyst is completed according to the following steps:
[0054] Step (1): dissolving 12 g of bismuth nitrate and 8 g of ferric nitrate in 60 g of water at room temperature, heating the mixture to 60° C. in a water bath to completely dissolve the bismuth nitrate and 8 g of ferric nitrate, to obtain a mixed solution of metals;
[0055] Step (2): 40 g of ZSM-5 molecular sieve and 50.09 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 1 hour to obtain a mixed slurry;
[0056] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7, continue stirring for 2 h, and stand at 60° C. for aging for 3 h.
[0057] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.2 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 700°C for 1 hour. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-3 is obtained.
[0058] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 40: 50.09: 7.91: 0.8. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is bismuth oxide, M2 is iron oxide, and M1:M2 = 2.00:1.
[0059] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h-1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-3 catalyst prepared in Example 3.
[0060] Evaluation results of the catalyst: n-butane conversion was 68.72%, ethylene yield was 19.05 wt%, and propylene yield was 24.76 wt%.
[0061] Example 4
[0062] The preparation of the catalyst is completed according to the following steps:
[0063] Step (1): at room temperature, dissolve 8 g of gallium nitrate and 8 g of zinc nitrate in 70 g of water, and heat the water bath to 60° C. to completely dissolve them, to obtain a mixed solution of metals;
[0064] Step (2): 30 g of ZSM-5 molecular sieve and 60.31 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 1 hour to obtain a mixed slurry;
[0065] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7-9, continue stirring for 2 h, and stand at 60° C. for aging for 3 h.
[0066] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed once with 0.2 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 650°C for 1.5 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-4 is obtained.
[0067] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 30: 60.31: 7.69: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is gallium oxide, M2 is zinc oxide, and M1:M2 = 6.03:1.
[0068] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-4 catalyst prepared in Example 4.
[0069] Evaluation results of the catalyst: n-butane conversion was 67.58%, ethylene yield was 17.51 wt%, and propylene yield was 23.56 wt%.
[0070] Example 5
[0071] The preparation of the catalyst is completed according to the following steps:
[0072] Step (1): dissolving 15 g of bismuth nitrate and 6 g of zinc nitrate in 50 g of water at room temperature, heating the mixture to 60° C. in a water bath to completely dissolve the bismuth nitrate and obtain a mixed solution of metals;
[0073] Step (2): 37 g ZSM-5 molecular sieve and 54.63 g SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0074] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7-9, continue stirring for 1.5 hours, and stand at 60°C for aging for 3 hours.
[0075] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 650°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-5 is obtained.
[0076] The components of the catalyst are calculated by mass ratio, molecular sieve: SiO2: metal oxide: K2O = 37: 54.63: 6.37: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is bismuth oxide, M2 is zinc oxide, and M1:M2 = 4.82:1.
[0077] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-5 catalyst prepared in Example 5.
[0078] Evaluation results of the catalyst: n-butane conversion was 67.9%, ethylene yield was 18.71 wt%, and propylene yield was 22.52 wt%.
[0079] Example 6
[0080] The preparation of the catalyst is completed according to the following steps:
[0081] Step (1): dissolving 15 g of bismuth nitrate and 6 g of zinc nitrate in 50 g of water at room temperature, heating the mixture to 60° C. in a water bath to completely dissolve the bismuth nitrate and obtain a mixed solution of metals;
[0082] Step (2): 37 g ZSM-5 molecular sieve and 54.63 g SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0083] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7-9, continue stirring for 1.5 hours, and stand at 70°C for aging for 10 hours.
[0084] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 550°C for 2 hours, and finally calcined at 700°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-6 is obtained.
[0085] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 37: 54.63: 6.37: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is bismuth oxide, M2 is zinc oxide, and M1:M2 = 4.82:1.
[0086] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 650°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-6 catalyst prepared in Example 6.
[0087] Evaluation results of the catalyst: n-butane conversion was 68.12%, ethylene yield was 19.71 wt%, and propylene yield was 22.83 wt%.
[0088] Example 7
[0089] The preparation of the catalyst is completed according to the following steps:
[0090] Step (1): dissolving 15 g of indium nitrate and 11 g of zinc nitrate in 50 g of water at room temperature, heating the water bath to 60° C. to completely dissolve the indium nitrate and obtain a mixed solution of metals;
[0091] Step (2): 35 g of ZSM-5 molecular sieve and 54.57 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0092] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 8, continue stirring for 1.5 hours, and stand at 70°C for aging for 8 hours.
[0093] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 550°C for 2 hours, and finally calcined at 700°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-6 is obtained.
[0094] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 35: 54.57: 8.43: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is indium oxide, M2 is zinc oxide, and M1:M2 = 4.6:1.
[0095] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 650°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-7 catalyst prepared in Example 7.
[0096] Evaluation results of the catalyst: n-butane conversion was 69.02%, ethylene yield was 20.71 wt%, and propylene yield was 21.73 wt%.
[0097] Example 8
[0098] The preparation of the catalyst is completed according to the following steps:
[0099] Step (1): dissolving 15 g of indium nitrate and 11 g of zinc nitrate in 50 g of water at room temperature, heating the water bath to 60° C. to completely dissolve the indium nitrate and obtain a mixed solution of metals;
[0100] Step (2): 35 g of ZSM-5 molecular sieve and 54.57 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0101] Step (3): Weigh 5 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 9, continue stirring for 1.5 hours, and stand at 63°C for aging for 24 hours.
[0102] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 1 hour, and finally calcined at 700°C for 3 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-8 is obtained.
[0103] The mass ratio of the catalyst components is as follows: molecular sieve: SiO2: metal oxide: K2O = 35: 54.57: 6.42: 4. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is indium oxide, M2 is zinc oxide, and M1:M2 = 3.27:1.
[0104] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 650°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-8 catalyst prepared in Example 8.
[0105] Evaluation results of the catalyst: n-butane conversion was 68.22%, ethylene yield was 19.67 wt%, and propylene yield was 22.03 wt%.
[0106] Example 9
[0107] The preparation of the catalyst is completed according to the following steps:
[0108] Step (1): at room temperature, dissolve 10.66 g of indium nitrate and 20 g of zinc nitrate in 80 g of water, and heat the water bath to 60° C. to completely dissolve them, to obtain a mixed solution of metals;
[0109] Step (2): 37 g ZSM-5 molecular sieve and 54.14 g SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0110] Step (3): Weigh 3 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 9, continue stirring for 1.5 hours, and stand at 66°C for aging for 14 hours.
[0111] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 1 hour, and finally calcined at 700°C for 3 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-9 is obtained.
[0112] The mass ratio of the catalyst components is as follows: molecular sieve: SiO2: metal oxide: K2O = 37: 54.14: 7.65: 1.2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is indium oxide, M2 is zinc oxide, and M1:M2 = 1.8:1.
[0113] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 650°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-9 catalyst prepared in Example 9.
[0114] Evaluation results of the catalyst: n-butane conversion was 69.32%, ethylene yield was 20.83 wt%, and propylene yield was 21.36 wt%.
[0115] Example 10
[0116] The preparation of the catalyst is completed according to the following steps:
[0117] Step (1): at room temperature, dissolve 10 g of indium nitrate and 18 g of zinc nitrate in 80 g of water, and heat the water bath to 60° C. to completely dissolve them, to obtain a mixed solution of metals;
[0118] Step (2): 36 g of ZSM-5 molecular sieve and 54 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0119] Step (3): Weigh 7.3 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 8, continue stirring for 1.5 hours, and stand at 72°C for aging for 14 hours.
[0120] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 1 hour, and finally calcined at 700°C for 3 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-10 is obtained.
[0121] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 36: 54: 7.08: 2.92. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is indium oxide, M2 is zinc oxide, and M1:M2 = 1.7:1.
[0122] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 650°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-10 catalyst prepared in Example 10.
[0123] Evaluation results of the catalyst: n-butane conversion was 68.84%, ethylene yield was 21.56 wt%, and propylene yield was 20.11 wt%.
[0124] Embodiment 11
[0125] The preparation of the catalyst is completed according to the following steps:
[0126] Step (1): dissolving 9 g of indium nitrate and 18 g of zinc nitrate in 80 g of water at room temperature, heating the water bath to 60° C. to completely dissolve the indium nitrate and obtain a mixed solution of metals;
[0127] Step (2): 40 g of ZSM-5 molecular sieve and 50 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0128] Step (3): Weigh 7.3 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7, continue stirring for 1.5 hours, and stand at 70°C for aging for 18 hours.
[0129] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 1 hour, and finally calcined at 700°C for 3 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-11 is obtained.
[0130] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 40: 50: 7.08: 2.92. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is indium oxide, M2 is zinc oxide, and M1:M2 = 1.7:1.
[0131] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1400 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-11 catalyst prepared in Example 11.
[0132] Evaluation results of the catalyst: n-butane conversion was 68.03%, ethylene yield was 20.86 wt%, and propylene yield was 20.35 wt%.
[0133] Example 12
[0134] The preparation of the catalyst is completed according to the following steps:
[0135] Step (1): at room temperature, dissolve 18 g of gallium nitrate and 7.8 g of ferric nitrate in 60 g of water, and heat the water bath to 60° C. to completely dissolve them, to obtain a mixed solution of metals;
[0136] Step (2): 50 g of ZSM-5 molecular sieve and 38 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0137] Step (3): Weigh 7.07 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7, continue stirring for 1.5 hours, and stand at 70°C for aging for 18 hours.
[0138] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 1 hour, and finally calcined at 700°C for 3 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-12 is obtained.
[0139] The mass ratio of the catalyst components is as follows: molecular sieve: SiO2: metal oxide: K2O = 50: 38: 9.17: 2.83. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is gallium oxide and M2 is iron oxide, and M1:M2 = 2.56:1.
[0140] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1400 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-12 catalyst prepared in Example 12.
[0141] Evaluation results of the catalyst: n-butane conversion was 70.12%, ethylene yield was 21.34 wt%, and propylene yield was 19.88 wt%.
[0142] Embodiment 13
[0143] The preparation of the catalyst is completed according to the following steps:
[0144] Step (1): at room temperature, dissolve 20 g of gallium nitrate and 13.85 g of bismuth nitrate in 60 g of water, and heat the water bath to 60° C. to completely dissolve them, to obtain a mixed solution of metals;
[0145] Step (2): 47 g ZSM-5 molecular sieve and 38 g SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0146] Step (3): Weigh 7 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 8, continue stirring for 1.5 h, and stand at 65° C. for aging for 20 h.
[0147] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 1 hour, and finally calcined at 700°C for 3 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-13 is obtained.
[0148] The mass ratio of the catalyst components is as follows: molecular sieve: SiO2: metal oxide: K2O = 47: 38: 12.2: 2.8. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is gallium oxide and M2 is bismuth oxide, and M1:M2 = 1.51:1.
[0149] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1400 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-13 catalyst prepared in Example 13.
[0150] Evaluation results of the catalyst: n-butane conversion was 68.88%, ethylene yield was 21.05 wt%, and propylene yield was 21.03 wt%.
[0151] Embodiment 14
[0152] The preparation of the catalyst is completed according to the following steps:
[0153] Step (1): at room temperature, dissolve 17.7 g of gallium nitrate and 8 g of indium nitrate in 65 g of water, and heat the water bath to 60° C. to completely dissolve them, to obtain a mixed solution of metals;
[0154] Step (2): 48 g of ZSM-5 molecular sieve and 39 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0155] Step (3): Weigh 7.05 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7, continue stirring for 1.5 h, and age at 68° C. for 22 h.
[0156] Step (4): The sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 490°C for 1 hour, and finally calcined at 700°C for 3 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst MC-14 is obtained.
[0157] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 48: 39: 10.18: 2.82. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is gallium oxide, M2 is indium oxide, and M1:M2 = 1.75:1.
[0158] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1400 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the MC-14 catalyst prepared in Example 14.
[0159] Evaluation results of the catalyst: n-butane conversion was 68.97%, ethylene yield was 21.45 wt%, and propylene yield was 19.34 wt%.
[0160] Comparative Example 1
[0161] The preparation of the catalyst is completed according to the following steps:
[0162] Step (1): dissolving 15 g of bismuth nitrate and 6 g of zinc nitrate in 50 g of water at room temperature, heating the mixture to 60° C. in a water bath to completely dissolve the bismuth nitrate and obtain a mixed solution of metals;
[0163] Step (2): 25 g of ZSM-5 molecular sieve and 66.63 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0164] Step (3): Weigh 10 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7-9, continue stirring for 1.5 hours, and stand at 60°C for aging for 3 hours.
[0165] In step (4), the sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 650°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst D-1 is obtained.
[0166] The components of the catalyst are calculated by mass ratio, molecular sieve: SiO2: metal oxide: K2O = 25: 66.63: 6.37: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is bismuth oxide, M2 is zinc oxide, and M1:M2 = 4.82:1.
[0167] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the D-1 catalyst prepared in Comparative Example 1.
[0168] Evaluation results of the catalyst: n-butane conversion was 63.5%, ethylene yield was 16.81 wt%, and propylene yield was 20.52 wt%.
[0169] Comparative Example 2
[0170] The preparation of the catalyst is completed according to the following steps:
[0171] Step (1): dissolving 15 g of bismuth nitrate and 6 g of zinc nitrate in 50 g of water at room temperature, heating the mixture to 60° C. in a water bath to completely dissolve the bismuth nitrate and obtain a mixed solution of metals;
[0172] Step (2): 55 g of ZSM-5 molecular sieve and 36.63 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0173] Step (3): Weigh 10 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7-9, continue stirring for 1.5 hours, and stand at 60°C for aging for 3 hours.
[0174] In step (4), the sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 650°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst D-2 is obtained.
[0175] The components of the catalyst are calculated by mass ratio, molecular sieve: SiO2: metal oxide: K2O = 55: 36.63: 6.37: 2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is bismuth oxide, M2 is zinc oxide, and M1:M2 = 4.82:1.
[0176] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h-1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the D-2 catalyst prepared in Comparative Example 2.
[0177] Evaluation results of the catalyst: n-butane conversion was 70.5%, ethylene yield was 10.81 wt%, and propylene yield was 20.52 wt%.
[0178] Comparative Example 3
[0179] The preparation of the catalyst is completed according to the following steps:
[0180] Step (1): dissolving 4 g of bismuth nitrate and 2 g of ferric nitrate in 50 g of water at room temperature, and heating the water bath to 60° C. to completely dissolve the bismuth nitrate and ferric nitrate to obtain a mixed solution of metals;
[0181] Step (2): 40 g of ZSM-5 molecular sieve and 57.53 g of SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0182] Step (3): Weigh 1 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 7-9, continue stirring for 1.5 hours, and stand at 60°C for aging for 3 hours.
[0183] In step (4), the sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 450°C for 3 hours, and finally calcined at 650°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst D-3 is obtained.
[0184] The components of the catalyst are calculated by mass ratio: molecular sieve: SiO2: metal oxide: K2O = 40: 57.53: 2.07: 0.4. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is bismuth oxide, M2 is zinc oxide, and M1:M2 = 2.13:1.
[0185] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 620°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the D-3 catalyst prepared in Comparative Example 3.
[0186] Evaluation results of the catalyst: n-butane conversion was 62.5%, ethylene yield was 17.1 wt%, and propylene yield was 22.02 wt%.
[0187] Comparative Example 4
[0188] The preparation of the catalyst is completed according to the following steps:
[0189] Step (1): at room temperature, dissolve 8.45 g of bismuth nitrate and 6 g of zinc nitrate in 50 g of water, and heat the water bath to 60° C. to completely dissolve them, to obtain a mixed solution of metals;
[0190] Step (2): 37 g ZSM-5 molecular sieve and 54.01 g SiO2 powder were added to the metal mixed solution obtained in step (1) under continuous stirring, and stirred for 0.5 h to obtain a mixed slurry;
[0191] Step (3): Weigh 13 g of potassium tartrate and add it to the slurry obtained in step (2) under continuous stirring, add ammonia water dropwise until the pH value of the solution reaches 10, continue stirring for 1.5 hours, and age at 90°C for 30 hours.
[0192] In step (4), the sample after static aging is first dried at 90°C for 4 hours, then rinsed twice with 0.1 mol / L dilute nitric acid, then calcined at 550°C for 2 hours, and finally calcined at 700°C for 2 hours. After cooling to room temperature, the bimetallic modified molecular sieve catalyst D-4 is obtained.
[0193] The mass ratio of the catalyst components is as follows: molecular sieve: SiO2: metal oxide: K2O = 37: 54.01: 3.79: 5.2. The metal oxide is a mixture of two metal oxides including M1 and M2, wherein M1 is bismuth oxide and M2 is zinc oxide, and M1: M2 = 3.62: 1.
[0194] Catalyst evaluation method: Performance evaluation was carried out on a microreactor (manufacturer: Qingdao Jietian Technology), with a reaction temperature of 650°C and a gas volume space velocity of 1500 h -1 The raw material for evaluation is 99.5 wt% of n-butane. The catalyst is the D-4 catalyst prepared in Comparative Example 4.
[0195] Evaluation results of the catalyst: n-butane conversion was 62.25%, ethylene yield was 16.71 wt%, and propylene yield was 17.38 wt%.
[0196] From the comparison of the reaction results: in Comparative Example 1, when the content of molecular sieve is too low, there are too few acidic centers, and the number of acidic active centers is insufficient, resulting in a low olefin yield; in Comparative Example 2, when the content of molecular sieve is too high, the number of high-density active centers is large, resulting in the survival of a large amount of methane and a low olefin yield; in Comparative Example 3, when the metal content in the catalyst is too low, the metal active centers are insufficient, resulting in a low olefin yield. In Comparative Example 4, the K content is too high, and the acidity of the molecular sieve is insufficient, resulting in a low olefin yield. The excellent olefin yield of the catalyst requires the co-catalysis of the acidic center and the metal active center. Compared with the prior art, the catalyst prepared by the present application is easy to shape, low in cost, has good anti-wear performance, and the finished catalyst has a high ethylene and propylene yield.
[0197] Table 1. Yield of pure n-butane cracking products (wt%)
[0198]
[0199]
Claims
1. A catalyst for preparing ethylene and propylene by catalytic cracking, characterized in that: The catalyst comprises silicon dioxide, potassium, molecular sieve and metal or its oxide attached to the molecular sieve, wherein the mass ratio of the molecular sieve, silicon dioxide, metal oxide and K2O is 30-50:30-65:5-20:0.1-5; the potassium in the catalyst is calculated as potassium oxide; when the catalyst comprises metal, it is calculated as its metal oxide.
2. The catalyst according to claim 1, characterized in that The mass ratio of molecular sieve, silicon dioxide, metal oxide and K2O is 35-45:45-55:5-10:1-3.
3. The catalyst according to claim 1, characterized in that The metal or its oxide includes M1 and M2, wherein M1 is selected from Ga, In, Bi or its metal oxide, and M2 is selected from Fe, Zn or its metal oxide.
4. The catalyst according to claim 3, characterized in that The mass ratio of M1 to M2 is 1-7:
1.
5. The catalyst according to claim 4, characterized in that The mass ratio of M1 to M2 is 1-2:
1.
6. A method for preparing the catalyst according to any one of claims 1 to 5, characterized in that: include: (1) Dissolve soluble salts of M1 and M2 in water; (2) mixed with ZSM-5 molecular sieve and SiO2 powder; (3) Add potassium tartrate, adjust the pH value to 7-9 with ammonia water, and allow to stand for aging and roasting.
7. The method of claim 6, characterized in that In the step (1), the soluble salts of M1 and M2 are nitrates, nitrites or sulfates of M1 and M2.
8. The method of claim 6, characterized in that In the step (3), the static aging temperature is 60-80°C, and the static aging time is 2-24h.
9. The method of claim 6, characterized in that In the step (3), the calcination is first carried out at 450-600°C for 2-3 hours, and then at 600-750°C for 1-2 hours.
10. Use of the catalyst for preparing ethylene and propylene by catalytic cracking according to any one of claims 1 to 5 in catalytic cracking of n-butane.
11. A process for preparing ethylene and propylene by catalytic cracking of n-butane, characterized in that: Use the catalyst according to any one of claims 1 to 5.
12. The process according to claim 11, characterized in that The reaction conditions of the process for preparing ethylene and propylene by catalytic cracking of n-butane include, for example, a temperature of 500-650° C., normal pressure, and a gas volume space velocity of 1200-1600 h -1 The agent-oil ratio is 3 to 10, and the agent-oil ratio is a weight ratio.
Citation Information
Patent Citations
Catalyst for producing olefin hydrocarbon by catalytic pyrolysis
CN101279287A
Production of mono-olefins by catalytic oxidative dehydrogenation of gaseous paraffinic hydrocarbons having 2 or more carbon atoms
CN1026100C
Catalyst for increasing yields of propylene and ethylene through catalytically cracking C4-C6 mixed hydrocarbon and method
CN103071522A
Method for producing propylene by catalytic cracking of n-butene
CN104557396A
Catalyst for preparation of light olefins and aromatic hydrocarbons and preparation method and application thereof
CN106694028A
Cited By
A process for the catalytic cracking of hydrocarbon feedstocks to produce olefins under low temperature plasma conditions
CN122789773A